A modified composite fiber and a warm and moisture-absorbing fabric made therefrom
By using modified composite fibers and wear-resistant layers in warm fabrics, the problem of poor wear resistance of fiber wool fabrics is solved, the wear resistance and breathability of the fabrics are improved, and the overall improvement of warm and moisture absorption performance is ensured.
Patent Information
- Application Number
- CN202410633186.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-21
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-05-21
AI Technical Summary
The fiber velvet fabrics of existing warm fabrics have poor wear resistance and are not easy to care for.
Using modified composite fibers, the terminal amino hyperbranched polysiloxane formed by hyperbranching reaction of aminosilane coupling agent under acid catalytic conditions and graphene oxide is grafted to form modified graphene and mixed with polyurethane. The wear resistance and breathability of the fibers are improved, and the modified composite fibers are subsequently made by wet spinning, and an wear-resistant layer is introduced into the fabric to improve overall performance.
It improves the wear resistance and breathability of the fabric, enhances the comfort of wearing, and improves the overall performance of the fabric while ensuring warm and moisture absorption.
Smart Images

Figure BDA0004850876510000061 
Figure BDA0004850876510000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fabric manufacturing, and in particular relates to a modified composite fiber and a thermal and moisture-absorbing fabric manufactured therefrom. Background Art
[0002] With the continuous development of fiber modification and fabric preparation technology, multifunctional fabrics have been developed and are welcomed by the market. For example, warm and hygroscopic fabrics are widely welcomed by the market because of their warmth and sweat absorption. For example, the warm and hygroscopic sweat-wicking plush fabric with a bionic structure disclosed in CN103103680A Chinese patent is a multi-layer plush fabric woven with double warp beams. The warp yarn forms a bionic structure that forks layer by layer from the bottom layer of the fabric to the top layer of the fabric in the direction of the fabric thickness, and the wool warp yarn forms plush on the fabric surface. The fabric has good warmth retention and moisture permeability. The double warp beam weaving is that the warp yarn is composed of yarns of two systems, wool warp yarn and ground warp yarn. The multi-layer plush fabric consists of three layers, the first layer is a plain weave, the second layer is a square weave, and the third layer is a surface-to-surface layer-changing structure composed of warp floating long lines. However, the wear resistance of the fabric is poor and it is not easy to take care of. Summary of the invention
[0003] The purpose of the present invention is to provide a modified composite fiber and a warm and moisture-absorbing fabric made thereof.
[0004] The technical problem to be solved by the present invention is that the fiber fleece fabrics in the existing thermal insulation fabrics have poor wear resistance and are difficult to care for.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] The first object of the present invention is to provide a modified composite fiber, wherein the modified composite fiber is prepared by wet spinning a raw material spinning solution, wherein the raw material spinning solution is prepared by mixing a mixed solvent, polyurethane and modified graphene;
[0007] The mixed solvent is prepared by mixing N,N-dimethylformamide and tetrahydrofuran;
[0008] The modified graphene is formed by grafting an amino-terminated hyperbranched polysiloxane formed by a hyperbranching reaction of an aminosilane coupling agent under acid catalysis conditions with graphene oxide.
[0009] The addition of modified graphene not only improves the wear resistance of the obtained modified composite fiber, but also the modified graphene fiber is evenly dispersed in the raw spinning solution through the hyperbranched polysiloxane molecular chain grafted on its surface. The unique branching characteristics and low surface properties of the hyperbranched polysiloxane molecular chain make it easier for it to mix with the polyurethane molecular chain, and then generate entanglement, hydrogen bonding and other forces. That is, the hyperbranched polysiloxane grafted on the graphene surface enhances the interaction between the graphene and the polyurethane molecules, facilitates the graphene and polyurethane molecular chains to embrace and form fibers in the subsequent textile process, increases the fiber diameter, and improves the air permeability of the textile layer composed of the modified composite fiber; finally, the introduced hyperbranched polysiloxane molecules can improve the flexibility of the modified composite fiber and improve the wearing comfort of the corresponding textile layer.
[0010] Furthermore, in the hyperbranching reaction, the acid catalysis condition is to maintain the pH of the reaction system at 5.5-6 by hydrochloric acid, the reaction temperature is 50-60° C., the reaction time is 3-4 h, and the reaction solvent is a mixed solvent formed by mixing deionized water and ethanol;
[0011] In the hyperbranching reaction, the self-hyperbranching hydrolysis reaction of siloxane under acidic conditions is utilized to form hyperbranched polysiloxane. In this process, deionized water is used as a raw material for hydrolysis and as a reaction solvent. In addition, ethanol is introduced as a dissolution aid, which helps the uniformity of the entire reaction system and makes the average molecular weight distribution of the amino-terminated hyperbranched polysiloxane obtained by the hyperbranching reaction of siloxane (aminosilane coupling agent in the present invention) relatively narrow.
[0012] Preferably, in the hyperbranching reaction, the reaction solvent is a mixture of deionized water and ethanol in a volume ratio of 5-10:1.
[0013] Furthermore, in the grafting reaction, the reaction pH is 9-9.5, the reaction temperature is 85-90° C., the reaction time is 4-6 hours, and the reaction solvent is a mixed solvent formed by mixing deionized water and ethanol;
[0014] In the grafting reaction, the end group of the amino-terminated hyperbranched polysiloxane reacts with the epoxy group on the surface of the graphene oxide to form a graft, so that the graphene oxide surface is grafted with a hyperbranched polysiloxane molecular chain;
[0015] Preferably, in the grafting reaction, the reaction solvent is a mixture of deionized water and ethanol in a volume ratio of 3-4:2.
[0016] Furthermore, the mass ratio of the aminosilane coupling agent to the graphene oxide is 8-10:1.
[0017] Furthermore, the mixed solvent is prepared by mixing N,N-dimethylformamide and tetrahydrofuran in a volume ratio of 2-2.5:3.
[0018] Furthermore, the solid content of the raw spinning solution is 8-12%.
[0019] Furthermore, the mass ratio of the polyurethane to the modified graphene is 1:0.08-0.17.
[0020] Furthermore, during the wet spinning, the extrusion speed is 10-15 mL / h.
[0021] The second object of the present invention is to provide a thermal insulation and moisture-absorbing fabric, comprising a thermal insulation layer and wear-resistant layers adhered to the upper and lower surfaces of the thermal insulation layer;
[0022] According to the percentage by mass, the thermal insulation layer is woven from 25-35% cashmere, 15-30% spandex and the remainder cotton fiber;
[0023] The wear-resistant layer is a unilaterally-adhesively modified textile layer, and the textile layer is formed by weaving the modified composite fiber as described above;
[0024] The one-sided adhesion modification is achieved by soaking the modified side in an oxidation solution for oxidation modification.
[0025] Furthermore, the oxidation solution is prepared by mixing potassium permanganate powder and nitric acid solution with a mass fraction of 65-68% at a mass ratio of 0.5-0.8:1.
[0026] Furthermore, during the one-sided adhesion modification, the modification temperature is 50-70° C. and the modification time is 1.5-2.5 h.
[0027] Furthermore, the diameter of the cashmere is 12.0-15 μm.
[0028] Beneficial effects of the present invention:
[0029] The modified composite fiber provided by the present invention is made of polyurethane and modified graphene through electrostatic spinning. The introduction of modified graphene not only improves the wear resistance of the obtained modified composite fiber, but also in the raw spinning solution, there are entanglement, hydrogen bonding and other forces between the modified graphene and the polyurethane molecules, which facilitates the graphene and polyurethane molecular chains to be entangled and formed into fibers in the subsequent electrostatic spinning process, increases the diameter of the fiber, improves the air permeability of the obtained modified composite fiber, and avoids the subsequent modification of the composite fiber causing a significant reduction in the air permeability and hygroscopicity of the thermal insulation layer;
[0030] The thermal insulation fabric provided by the present invention comprises a thermal insulation layer woven from cashmere, spandex and bamboo charcoal fibers, and modified composite fibers adhered to both surfaces of the thermal insulation layer. On the one hand, through the reasonable combination of cashmere, spandex and bamboo charcoal fibers, the thermal insulation properties of cashmere and the moisture absorption and breathability of cotton fibers are fully utilized, and the elasticity of spandex is fully utilized, thereby ensuring the integrity of the thermal insulation and moisture absorption properties of the fabric and improving the elasticity of the fabric; on the other hand, through the introduction of the modified composite fibers, the wear resistance of the fabric is improved. DETAILED DESCRIPTION
[0031] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Example 1
[0033] Preparation of modified graphene:
[0034] 100g KH550, 150mL deionized water and 15mL ethanol were mixed evenly, then stirred and heated to 50°C, hydrochloric acid was used to maintain the pH of the reaction system at 5.5-6, and the reaction was stirred for 4h, the reaction was stopped, and rotary evaporation was performed to obtain terminal amino hyperbranched polysiloxane; the obtained terminal amino hyperbranched polysiloxane, 10g graphene oxide, 150mL deionized water and 70mL ethanol were mixed evenly, then stirred and heated to 85°C, and the pH of the reaction system was adjusted to 9-9.5 by strong sodium oxide, and the reaction time was stirred for 6h, the reaction was stopped, aged, precipitated water, ethanol washed alternately, and dried to obtain modified graphene.
[0035] Example 2
[0036] Preparation of modified graphene:
[0037] 80g KH550, 150mL deionized water and 70mL ethanol were mixed evenly, then stirred and heated to 60°C, hydrochloric acid was used to maintain the pH of the reaction system at 5.5-6, and the reaction was stirred for 3h, the reaction was stopped, and rotary evaporation was performed to obtain terminal amino hyperbranched polysiloxane; the obtained terminal amino hyperbranched polysiloxane, 10g graphene oxide, 150mL deionized water and 100mL ethanol were mixed evenly, then stirred and heated to 90°C, and the pH of the reaction system was adjusted to 9-9.5 by strong sodium oxide, and the reaction time was stirred for 4h, the reaction was stopped, aged, precipitated water, ethanol washed alternately, and dried to obtain modified graphene.
[0038] Example 3
[0039] Preparation of modified composite fibers:
[0040] 1. 100 mL of N,N-dimethylformamide and 150 mL of tetrahydrofuran were mixed as solvents, and then 20 g of polyurethane and 3.2 g of the modified graphene prepared in Example 1 were added, and the mixture was stirred and dissolved uniformly to prepare a raw spinning solution;
[0041] 2. The raw spinning solution is wet-spun according to the following process: the extrusion speed is 15 mL / h. During the wet spinning, after extrusion, it is immersed in a water bath (the water temperature is room temperature) for about 2 minutes, and then pulled 1.5 times to obtain a modified composite fiber (wire diameter 0.5±0.03 mm).
[0042] Example 4
[0043] Preparation of modified composite fibers:
[0044] 1. 100 mL of N,N-dimethylformamide and 120 mL of tetrahydrofuran were mixed to prepare a mixed solvent, and then 23 g of polyurethane and 1.83 g of the modified graphene prepared in Example 2 were added, and after stirring and dissolving evenly, a raw material spinning solution was prepared;
[0045] 2. The raw spinning solution was wet-spun according to the following process: the extrusion speed was 10 mL / h, and after extrusion, it was immersed in a water bath (the water temperature was room temperature) for about 2 minutes, and then pulled 1.5 times to obtain a modified composite fiber (wire diameter 0.5±0.03 mm).
[0046] Comparative Example 1
[0047] Preparation of modified composite fibers:
[0048] 1. Mix 100 mL of N,N-dimethylformamide and 150 mL of tetrahydrofuran as a solvent, then add 20 g of polyurethane and 3.2 g of graphene oxide, stir and dissolve evenly to prepare a raw spinning solution;
[0049] 2. The raw spinning solution is wet-spun according to the following process: the extrusion speed is 15 mL / h. During the wet spinning, after extrusion, it is immersed in a water bath (the water temperature is room temperature) for about 2 minutes, and then pulled 1.5 times to obtain a modified composite fiber (wire diameter 0.4±0.03 mm).
[0050] Comparative Example 2
[0051] Fiber preparation:
[0052] 1. Mix 100 mL of N,N-dimethylformamide and 150 mL of tetrahydrofuran as a solvent, then add 20 g of polyurethane, stir and dissolve evenly to prepare a raw spinning solution;
[0053] 2. The raw spinning solution was wet-spun according to the following process: the extrusion speed was 15 mL / h, and after extrusion, it was immersed in a water bath (the water temperature was room temperature) for about 2 minutes, and then pulled 1.5 times to obtain a modified composite fiber (wire diameter 0.1±0.03 mm).
[0054] The modified composite fibers obtained in Examples 3-4 and Comparative Example 1 and the fibers obtained in the comparative example were woven into textile layers, and the wear resistance and air permeability tests were performed. The test results are shown in Table 1.
[0055] Table 1
[0056]
[0057] It can be seen from the data in Table 1 that the wear resistance and air permeability of the textile layer composed of the modified fibers obtained in Examples 3-4 of the present invention are better than the corresponding properties of the textile layer obtained in Comparative Examples 1-2.
[0058] The wear resistance is tested according to GB / T 21196.2 and is measured by the number of frictions. The air permeability is tested by setting the test pressure to 0.1 MPa and measuring the volume of nitrogen passing through the sample per minute. The sample area is 35 cm 2 .
[0059] Example 5
[0060] Preparation of warm and moisture-wicking fabric:
[0061] i. Take the following raw materials according to mass percentage: 25% cashmere, 20% spandex and the remainder of cotton fiber, and then weave into a cloth, wherein the diameter of the cashmere is 12.0 to 15 μm;
[0062] ii. The modified composite fiber obtained in Example 3 was woven into a textile layer, and then unilaterally protected, and the other unprotected side was placed in an oxidant solution, oxidized and modified at 50 ° C for 2.5 hours, taken out and cooled, to obtain a unilaterally adhered modified modified textile layer, wherein the oxidizing solution was prepared by mixing potassium permanganate powder and a nitric acid solution with a mass fraction of 65-68% according to a mass ratio of 0.5:1;
[0063] iii. The woven fabric is used as the thermal insulation layer and as the base layer, and the modified textile layer with single-side adhesion is adhered to both surfaces of the base layer by hot pressing to form a wear-resistant layer on both surfaces of the base layer, and finally a thermal insulation and moisture-absorbing fabric is obtained.
[0064] Example 6
[0065] Preparation of warm and moisture-wicking fabric:
[0066] i. Take the following raw materials according to mass percentage: 30% cashmere, 30% spandex and the remainder of cotton fiber, and then weave them into cloth, wherein the diameter of the cashmere is 12.0 to 15 μm;
[0067] ii. The modified composite fiber obtained in Example 4 was woven into a textile layer, and then unilaterally protected, and the other unprotected side was placed in an oxidant solution, oxidized and modified at 60 ° C for 2 h, taken out and cooled, to obtain a unilaterally adhered modified textile layer, wherein the oxidizing solution was prepared by mixing potassium permanganate powder and a nitric acid solution with a mass fraction of 65-68% according to a mass ratio of 0.8:1;
[0068] iii. The woven fabric is used as the thermal insulation layer and as the base layer, and the modified textile layer with single-side adhesion is adhered to both surfaces of the base layer by hot pressing to form a wear-resistant layer on both surfaces of the base layer, and finally a thermal insulation and moisture-absorbing fabric is obtained.
[0069] Example 7
[0070] Preparation of warm and moisture-wicking fabric:
[0071] i. Take the following raw materials according to mass percentage: 35% cashmere, 15% spandex and the remainder of cotton fiber, and then weave into a cloth, wherein the diameter of the cashmere is 12.0 to 15 μm;
[0072] ii. The modified composite fiber obtained in Example 3 was woven into a textile layer, and then unilaterally protected, and the other unprotected side was placed in an oxidant solution, oxidized and modified at 70 ° C for 1.5 h, taken out and cooled, to obtain a unilaterally adhered modified modified textile layer, wherein the oxidizing solution was prepared by mixing potassium permanganate powder and a nitric acid solution with a mass fraction of 65-68% according to a mass ratio of 0.5:1;
[0073] iii. The woven fabric is used as the thermal insulation layer and as the base layer, and the modified textile layer with single-side adhesion is adhered to both surfaces of the base layer by hot pressing to form a wear-resistant layer on both surfaces of the base layer, and finally a thermal insulation and moisture-absorbing fabric is obtained.
[0074] Comparative Example 3
[0075] Preparation of fabric: Compared with Example 5, the wear-resistant layer is replaced by the fiber membrane prepared in Comparative Example 1, and the rest is the same.
[0076] Comparative Example 4
[0077] Preparation of fabric: Compared with Example 5, the wear-resistant layer is replaced by the fiber membrane prepared in Comparative Example 2, and the rest is the same.
[0078] The fabrics obtained in Examples 5-7 and Comparative Examples 3-4 and the thermal insulation layer obtained in Examples 5-7 were tested for moisture absorption performance (moisture regain) and washability. The test results are shown in Table 2.
[0079] Table 2
[0080]
[0081] From the data in Table 2, it can be seen that the thermal insulation layer has good air permeability and moisture absorption performance. After being combined with the textile layer formed by the modified composite fiber, the wear resistance of the fabric is significantly improved. Although its air permeability and moisture regain are reduced, it can still maintain good air permeability and moisture absorption performance. In addition, the thermal insulation layer and the wear-resistant layer (the textile layer formed by the modified composite fiber) in the fabric obtained in the embodiment of the present invention have good adhesion and good washability.
[0082] Among them, the washability is based on the wear resistance of the fabric after a fixed number of washes according to GB / T 21196.2; the test conditions for moisture regain are: 20℃, 65%RH; air permeability: set the test pressure to 0.1MPa, measure the volume of nitrogen permeating the sample per minute, and the sample area is 35cm 2 .
[0083] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0084] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A modified composite fiber, characterized in that: The modified composite fiber is prepared by wet spinning a raw material spinning solution, wherein the raw material spinning solution is prepared by mixing a mixed solvent, polyurethane and modified graphene; The mixed solvent is prepared by mixing N,N-dimethylformamide and tetrahydrofuran; The modified graphene is formed by grafting an amino-terminated hyperbranched polysiloxane formed by a hyperbranching reaction of an aminosilane coupling agent under acid catalysis with graphene oxide; The mass ratio of the aminosilane coupling agent to the graphene oxide is 8-10:1; The mixed solvent is prepared by mixing N,N-dimethylformamide and tetrahydrofuran in a volume ratio of 2-2.5:3; The solid content of the raw spinning solution is 8-12%; The mass ratio of the polyurethane to the modified graphene is 1:0.08-0.
17.
2. The modified composite fiber according to claim 1, characterized in that In the hyperbranched reaction, the acid catalysis condition is to maintain the pH of the reaction system at 5.5-6 by hydrochloric acid, the reaction temperature is 50-60° C., the reaction time is 3-4 hours, and the reaction solvent is a mixed solvent formed by mixing deionized water and ethanol.
3. The modified composite fiber according to claim 1, characterized in that In the grafting reaction, the reaction pH is 9-9.5, the reaction temperature is 85-90° C., the reaction time is 4-6 hours, and the reaction solvent is a mixed solvent formed by mixing deionized water and ethanol.
4. The modified composite fiber according to claim 1, characterized in that During the wet spinning, the extrusion speed is 10-15 mL / h.
5. A warm and moisture-absorbing fabric, characterized in that: It comprises a thermal insulation layer and a wear-resistant layer adhered to the upper and lower surfaces of the thermal insulation layer; According to the percentage by mass, the thermal insulation layer is woven from 25-35% cashmere, 15-30% spandex and the remainder cotton fiber; The wear-resistant layer is a unilaterally-adhesively modified textile layer, and the textile layer is formed by weaving the modified composite fiber according to any one of claims 1 to 4; The one-sided adhesion modification is achieved by soaking the modified side in an oxidation solution for oxidation modification.
6. The thermal insulation and moisture absorption fabric according to claim 5, characterized in that: During the one-sided adhesion modification, the modification temperature is 50-70° C., and the modification time is 1.5-2.5 hours; the diameter of the cashmere is 12.0-15 μm.