A hydrogen storage composite film and a preparation method thereof
By adjusting the mass ratio of silicene nanosheets, graphene and PVA gel, and using 3D printing technology to prepare hydrogen storage composite films, the problem of insufficient hydrogen storage performance in the existing technology is solved, and efficient hydrogen storage and excellent mechanics are achieved. performance.
Patent Information
- Application Number
- CN202410938896.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-15
AI Technical Summary
Existing silicene nanosheets and graphene composite materials have insufficient hydrogen storage performance in hydrogen storage applications, and the conventional film-forming process limits the content of hydrogen storage components in the materials, causing hydrogen to escape easily and the hydrogen storage performance to deteriorate.
By mixing silene nanosheets, graphene and polyvinyl alcohol (PVA) gel, adjusting the mass ratio, and using 3D printing technology to prepare a hydrogen storage composite film, the pore structure is optimized to improve hydrogen loading efficiency.
The excellent mechanical properties and efficient hydrogen storage of the hydrogen storage composite film are achieved. The hydrogen diffusion coefficient is in the range of (1.59~7.52)×10-6cm2/s, which significantly improves the hydrogen storage performance.
Smart Images

Figure CN118459813B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hydrogen storage materials, and in particular relates to a hydrogen storage composite film and a preparation method thereof. Background Art
[0002] Energy is one of the most important resources for human survival. Hydrogen energy is clean, efficient, and easy to produce on a large scale, and has always been favored in the energy field. Hydrogen storage technology is one of the key technologies for the utilization of hydrogen energy, and the research and development of hydrogen storage materials has always been a hot topic in related fields.
[0003] Silicene nanosheets have certain advantages in storing hydrogen due to their unique spin-orbit effect and "pea pod" shaped hole structure. However, their single hole form leads to insufficient hydrogen storage capacity, and they must be combined with other structures to achieve a certain storage capacity. Graphene has a highly conductive sheet structure, and its combination with silicene nanosheets can improve the conduction and storage of hydrogen. However, in practical applications, hydrogen is easier to escape from the internal holes of the two materials, resulting in poor hydrogen storage performance. Therefore, how to coordinate the use of the two and improve the hydrogen storage performance of the material has become a technical problem that needs to be solved urgently.
[0004] Polyvinyl alcohol (PVA) is widely used in the energy field as a relatively safe and green polymer binder. Its hydrogel has moderate viscosity and is very easy to form a film. PVA hydrogel is combined with the above-mentioned graphene and silicene nanosheets, and the ratio of the three is adjusted to prepare a viscous material, and with the help of the entanglement effect of PVA, a film with hydrogen storage function can be manufactured. However, conventional film-forming processes, such as blade coating and casting, generally require materials with lower viscosity, resulting in the inability to increase the content of hydrogen storage components (such as graphene and silicene nanosheets) when preparing the material, and the hydrogen storage performance cannot be effectively improved. How to improve the hydrogen storage performance while ensuring the formation of the film is a key issue that needs to be solved. Summary of the invention
[0005] The purpose of the present invention is to provide a hydrogen storage composite film and a preparation method thereof. The hydrogen storage composite film prepared by the preparation method provided by the present invention has excellent hydrogen storage performance.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a hydrogen storage composite film, comprising the following steps:
[0008] Mixing silicene nanosheets, graphene and PVA gel to obtain ink;
[0009] 3D printing the ink to obtain a hydrogen storage composite film;
[0010] The mass ratio of the PVA gel, graphene and silicene nanosheets is (30-60): (1-2): (1-2).
[0011] Preferably, the preparation method of the PVA gel comprises the following steps:
[0012] The PVA powder and the inorganic solvent are mixed to form a gel to obtain the PVA gel.
[0013] Preferably, the ratio of the mass of the PVA powder to the volume of the inorganic solvent is (0.03-0.1) g:1 mL.
[0014] Preferably, the mixing is performed under stirring conditions.
[0015] Preferably, the stirring speed is 700-1000 r / min, and the stirring temperature is 40-70 °C.
[0016] Preferably, the gelling comprises stirring and standing in sequence.
[0017] Preferably, the stirring rate is 600-800 r / min, and the stirring time is 1.5-3 h.
[0018] Preferably, the parameters of the 3D printing include: a needle diameter of 200-600 μm, an extrusion pressure of 20-50 psi, and a moving speed of 8-10 mm / s.
[0019] The present invention also provides a hydrogen storage composite film prepared by the preparation method described in the above technical solution.
[0020] The present invention provides a method for preparing a hydrogen storage composite film, comprising the following steps: mixing silicene nanosheets, graphene and PVA gel to obtain ink; 3D printing the ink to obtain a hydrogen storage composite film; the mass ratio of the PVA gel, graphene and silicene nanosheets is (30~60): (1~2): (1~2). The present invention makes full use of the coordinated hydrogen storage performance of two two-dimensional nanomaterials, silicene nanosheets and graphene, and adds PVA gel to effectively adjust the pore structure in the film to improve the hydrogen loading efficiency; a hydrogen storage film with excellent mechanical properties is prepared by 3D printing; by controlling the mass ratio of PVA gel, graphene and silicene nanosheets, the hydrogen storage performance of the film can be further improved. Experimental results show that the hydrogen diffusion coefficient of the hydrogen storage composite film prepared by the present invention is (1.59~7.52)×10 -6 cm 2 / s. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 is a SEM image of the silicene nanosheet in Example 1;
[0022] Figure 2 is the XRD pattern of the silicene nanosheet in Example 1;
[0023] Figure 3 is the infrared spectrum of the silicene nanosheet in Example 1;
[0024] Figure 4 This is a SEM image of the hydrogen storage composite film prepared in Example 1;
[0025] Figure 5 This is a SEM image of the hydrogen storage composite film prepared in Example 2;
[0026] Figure 6 This is a SEM image of the hydrogen storage composite film prepared in Example 3;
[0027] Figure 7 This is a SEM image of the hydrogen storage composite film prepared in Example 4;
[0028] Figure 8 This is a SEM image of the composite film prepared in Comparative Example 1;
[0029] Fig. 9 The apparent viscosity curves of the inks in Examples 1 to 4 and Comparative Example 1;
[0030] Fig.10 The storage modulus (G′) and loss modulus (G″) of the ink in Examples 1 to 4 and Comparative Example 1 are curves showing the relationship between the storage modulus (G′) and the loss modulus (G″) and the oscillation strain;
[0031] Fig.11 : is the frequency modulus curve of the ink in Examples 1 to 4 and Comparative Example 1;
[0032] Fig.12 The thixotropy test curves of the inks in Examples 1 to 4 and Comparative Example 1;
[0033] Fig.13 The tensile strength test curves of the hydrogen storage composite films prepared in Examples 1 to 4 and the composite film prepared in Comparative Example 1 at room temperature;
[0034] Fig.14 is the constant potential polarization curve of the hydrogen storage composite film prepared in Example 1;
[0035] Fig.15 The constant potential polarization curve of the hydrogen storage composite film prepared in Example 2;
[0036] Fig.16 The constant potential polarization curve of the hydrogen storage composite film prepared in Example 3;
[0037] Fig.17 The constant potential polarization curve of the hydrogen storage composite film prepared in Example 4;
[0038] Fig.18 This is the constant potential polarization curve of the composite film prepared in Comparative Example 1. DETAILED DESCRIPTION
[0039] The present invention provides a method for preparing a hydrogen storage composite film, comprising the following steps:
[0040] Mixing silicene nanosheets, graphene and PVA gel to obtain ink;
[0041] 3D printing the ink to obtain a hydrogen storage composite film;
[0042] The mass ratio of the PVA gel, graphene and silicene nanosheets is (30-60): (1-2): (1-2).
[0043] The present invention has no particular limitation on the sources of the raw materials, and commercially available products known to those skilled in the art may be used.
[0044] The present invention mixes silicene nanosheets, graphene and PVA gel to obtain ink.
[0045] In the present invention, the silicene nanosheets are preferably prepared by a topochemical method. The present invention has no particular limitation on the specific operation of the topochemical method, and the operation well known to those skilled in the art can be used.
[0046] The present invention has no particular limitation on the size of the silicene nanosheets and graphene, and they can be prepared using commercially available products or well-known preparation methods known to those skilled in the art.
[0047] In the present invention, the preparation method of the PVA gel is preferably the following steps:
[0048] The PVA powder and the inorganic solvent are mixed to form a gel to obtain the PVA gel.
[0049] In the present invention, the inorganic solvent is preferably water.
[0050] In the present invention, the ratio of the mass of the PVA powder to the volume of the inorganic solvent is preferably (0.03-0.1) g:1 mL, and more preferably (0.05-0.1) g:1 mL.
[0051] In the present invention, the mixing is preferably carried out under stirring conditions; the stirring speed is preferably 700-1000 r / min; the stirring temperature is preferably 40-70°C, more preferably 50°C. The present invention has no particular limitation on the stirring time, as long as the stirring is uniform. The present invention can ensure that the powder added to the water does not agglomerate and is evenly dispersed by controlling the mixing process parameters.
[0052] In the present invention, the gelling process preferably includes stirring and standing in sequence; the stirring rate is preferably 600-800 r / min; the stirring time is preferably 1.5-3 h, more preferably 2 h; the standing time is preferably 22-30 h, more preferably 24-26 h.
[0053] In the present invention, the mass ratio of the PVA gel, graphene and silicene nanosheets is (30-60): (1-2): (1-2), preferably (35-55): (1-2): (1-2), and more preferably 50: 1: 1. The present invention can further improve the hydrogen storage performance of the film by controlling the mass ratio of the three.
[0054] In the present invention, the mixing of the silicene nanosheets, graphene and PVA gel is preferably carried out under stirring conditions; the stirring speed is preferably 800-1000 r / min. The present invention has no particular limitation on the stirring time, as long as the mixing is uniform. The present invention can further improve the uniformity of mixing by controlling the stirring process parameters.
[0055] In the present invention, the mixing is preferably performed under vacuum conditions. The present invention has no special limitation on the vacuum operation, and the operation well known to those skilled in the art can be used. The present invention uses vacuum to remove bubbles inside the ink.
[0056] After obtaining the ink, the present invention performs 3D printing on the ink to obtain a hydrogen storage composite film.
[0057] In the present invention, the parameters of the 3D printing preferably include: a needle diameter of 200-600 μm, an extrusion pressure of 20-50 psi, and a moving speed of 8-10 mm / s, and more preferably: a needle diameter of 400 μm, an extrusion pressure of 40 psi, and a moving speed of 8 mm / s.
[0058] The key technology of the present invention is to ensure the high content of hydrogen storage components by adjusting the mass ratio of PVA gel, graphene and silicene nanosheets, and prepare high-viscosity ink suitable for 3D printing, and then use 3D printing technology to achieve precise manufacturing of hydrogen storage film. The present invention can be promoted in many fields, such as the economical and customized manufacturing of various functional films; the direct and precise coverage of functional films required for the surface of special-shaped structures, and the low-cost assembly of various thin film devices.
[0059] The introduction of PVA gel in the present invention can effectively close a part of the ineffective macropores in the film and improve the hydrogen loading efficiency; the present invention prepares a high mechanical strength hydrogen storage composite film through 3D printing, improves the overall hydrogen storage capacity of the composite material, and opens up a new research idea for the development of hydrogen storage materials and devices.
[0060] The film of the present invention uses silicene nanosheets as the main material and is appropriately doped with graphene. Both graphene and silicene nanosheets belong to a sheet structure. The combination of the two can fully utilize their hydrogen storage advantages and improve the hydrogen storage performance of the material.
[0061] The present invention also provides a hydrogen storage composite film prepared by the preparation method described in the above technical solution.
[0062] The hydrogen storage composite film provided by the invention has large hydrogen storage capacity and hydrogen adsorption rate.
[0063] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0064] The experimental drugs used in the embodiments and comparative examples are shown in Table 1.
[0065] Table 1 Experimental drugs
[0066]
[0067] The experimental instruments used in the embodiments and comparative examples are shown in Table 2.
[0068] Table 2 Experimental instruments
[0069]
[0070] Example 1
[0071] The preparation method of the hydrogen storage composite film comprises the following steps:
[0072] (1) Preparation of silicene nanosheets using chemical topological method:
[0073] 1) Purification of CaSi2: Add CaSi2 to 2 mol / L NaOH aqueous solution, soak in a 60 ℃ constant temperature water bath for 24 h, then filter and wash, and dry for 1 h to obtain purified CaSi2;
[0074] 2) Preparation of silicene nanosheets by chemical topological method: 60 mL of anhydrous methanol, 1.161 g of anhydrous stannous chloride and 0.2 g of calcium disilicide were stirred and dissolved to obtain solution A; 0.03 g of sodium dodecyl sulfate was weighed and added to solution A, and stirred with a glass rod for 5 min to obtain solution B; solution B was placed in a 60 ℃ water bath for reaction for 24 h; the supernatant was first poured out, and the precipitate was washed into a centrifuge tube with anhydrous methanol, and centrifuged at 8000 r / min for 6 min, and the supernatant was poured out after the end; a hydrochloric acid methanol solution with a hydrochloric acid concentration of 5wt% was added and centrifuged at 8000 r / min for 6 min to obtain a precipitate, which was then filtered and placed in a vacuum drying oven and vacuumed at 80 ℃ for 24 h to obtain silicene nanosheets;
[0075] (2) Preparation of PVA gel: Weigh 4 g of PVA powder, add 40 mL of deionized water into a beaker, and perform magnetic stirring. Set the speed to 800 r / min and the temperature to 50 °C. Slowly add PVA powder while stirring. After adding, control the speed to 650 r / min, stir for 2 h, and finally let it stand for 24 h to obtain a relatively viscous PVA gel.
[0076] (3) 60 mg of the silicene nanosheets obtained in step (1), 60 mg of graphene and 3 g of the PVA gel obtained in step (2) were placed in a degassing tank, and the degassing tank was placed in a planetary stirring degassing device. The stirring parameter was set to 1000 r / min, the cover was closed and vacuum was drawn, and the stirring time was controlled to be 3 min. After the stirring was completed, the gel on the inner wall of the tank was mixed with a medicine spoon, and then the above operation was repeated 6 times to obtain ink, which was recorded as PSG-1;
[0077] (4) The ink obtained in step (3) is subjected to direct writing 3D printing to obtain a hydrogen storage composite film; wherein the needle diameter is 400 μm, the extrusion pressure is 40 psi, and the moving speed is 8 mm / s.
[0078] Example 2
[0079] On the basis of Example 1, the amount of silicene nanosheets was set to 80 mg, and other conditions remained unchanged, wherein the ink was recorded as PSG-2.
[0080] Example 3
[0081] On the basis of Example 1, the amount of graphene was set to 80 mg, and other conditions remained unchanged, wherein the ink was recorded as PSG-3.
[0082] Example 4
[0083] On the basis of Example 1, the amount of graphene was set to 80 mg, the amount of silicene nanosheets was set to 80 mg, and other conditions remained unchanged, wherein the ink was recorded as PSG-4.
[0084] Comparative Example 1
[0085] On the basis of Example 4, the silicene nanosheets were omitted and other conditions remained unchanged to prepare a composite film, wherein the ink was denoted as PSG-5.
[0086] The morphology of the silicene nanosheets in Example 1 was analyzed using a scanning electron microscope. Figure 1 As shown, Figure 1 This is the SEM image of the silicene nanosheet in Example 1.
[0087] from Figure 1 It can be seen that the silicene nanosheets prepared by the chemical topological method described in Example 1 have a unique "pea pod"-shaped sheet hole structure, which has certain storage advantages for hydrogen. In addition, the prepared silicene nanosheets have smooth inner and outer surfaces without impurity adsorption.
[0088] The silicene nanosheets in Example 1 were analyzed using an X-ray diffractometer, and the results are as follows: Figure 2 As shown, Figure 2 This is the XRD spectrum of the silicene nanosheets in Example 1.
[0089] from Figure 2 It can be seen that a typical broad peak region appears between 20° and 30°, indicating that the silicene nanosheets are in an amorphous state, the crystal regularity is not high, and the interlamellar spacing is large, which is consistent with Figure 1 Corresponding as shown.
[0090] The silicene nanosheets in Example 1 were subjected to infrared characterization analysis, and the results were as follows: Figure 3 As shown, Figure 3 This is the infrared spectrum of the silicene nanosheet in Example 1.
[0091] from Figure 3 It can be seen that at 873 cm -1 A small peak that appears is the infrared characteristic peak of Si-H / H-Si-H functional groups, indicating that silicene nanosheets have a certain hydrogen storage capacity and can be used in the preparation of PVA / silicene nanosheets / graphene composite film materials.
[0092] The hydrogen storage composite films prepared in Examples 1 to 4 and the composite film prepared in Comparative Example 1 were characterized and analyzed by SEM. The results are as follows: Figures 4 to 8 As shown, Figure 4 This is a SEM image of the hydrogen storage composite film prepared in Example 1; Figure 5 This is a SEM image of the hydrogen storage composite film prepared in Example 2; Figure 6 This is a SEM image of the hydrogen storage composite film prepared in Example 3; Figure 7 This is a SEM image of the hydrogen storage composite film prepared in Example 4; Figure 8 This is the SEM image of the composite film prepared in Comparative Example 1.
[0093] from Figure 4 It can be seen that the composite film prepared in Example 1 contains blocky silicene nanosheets with a large degree of agglomeration.
[0094] from Figure 5 It can be seen that in the composite film prepared in Example 2, the content of silicene nanosheets accounts for a relatively high proportion, and there are evenly dispersed silicene nanosheets in the composite film, which means that after ink preparation and 3D printing, graphene and silicene nanosheets are always evenly distributed during the composite film formation, and the two nanomaterials are intertwined to construct a porous structure. In addition, open holes with micron-sized pore sizes and smaller intertwined shielding holes can be found in the film, and these pore structures are beneficial for gas storage.
[0095] from Figure 6 It can be seen that in the composite film prepared in Example 3, the graphene content accounts for a relatively high proportion, and there are a large number of pore structures with a pore diameter of about 2 to 5 μm, which means that graphene can increase the pore structure, but the pore diameter is relatively large, which will lead to a decrease in the hydrogen storage capacity.
[0096] from Figure 7 It can be seen that in the composite film prepared in Example 4, due to the further increase in the total content of graphene and silicene nanosheets, the barrier effect of the two nanomaterials on the continuous casting of PVA gel during ink preparation and 3D printing film formation is increased, resulting in the presence of a large number of open macropores, which will cause a significant decrease in the hydrogen storage capacity and the mechanical properties of the film will also decrease.
[0097] from Figure 8 It can be seen that in the composite film prepared in comparative example 1, the film surface presents a continuous surface with ups and downs, and no obvious holes exist. Since comparative example 1 contains only 80 mg of graphene, this indirectly shows that the effect of using graphene printing to form a film alone on the hole adjustment is not obvious; after adding silicene nanosheets, the two can further adjust the hole structure through mutual cooperation to achieve the purpose of hydrogen storage.
[0098] The rheological properties of the inks in Examples 1 to 4 and Comparative Example 1 were tested: The rheological properties of PSG inks were tested using the ARES-G2 rheometer of TA Company of the United States. Since the operation process of direct writing 3D printing is carried out at room temperature, the test temperature of the rheometer is set to 25 °C. The rheological properties test uses a parallel plate fixture with a diameter of 40 mm, and the fixture spacing is set to 0.5 mm. The rheological properties test mainly includes the apparent viscosity curve, stress modulus curve, frequency modulus curve and thixotropy curve. The specific test parameters are set as follows:
[0099] Apparent viscosity test: shear rate range is 0.01~100 s -1 ;
[0100] Stress modulus test: frequency is 1 Hz, shear stress scanning range is 0.01~1000%;
[0101] Frequency modulus test: set the strain value to 1% and the frequency sweep range to 0.01~100Hz;
[0102] Thixotropy Test: This test consists of two parts, oscillation time and step stress increase.
[0103] In the oscillation time section, set the duration to 120 s, the sampling rate to 1 pts / s, the pressure to 0.1%, and the single-point frequency to 1 Hz. In the step stress growth section, set the duration to 15 s and the shear rate to 100 s. -1 , linear sampling, sampling rate 1pts / s. Finally, the data is plotted, the result is as follows Figures 9 to 12 .
[0104] Fig. 9 The apparent viscosity curves of the inks in Examples 1 to 4 and Comparative Example 1; Fig.10 The storage modulus (G′) and loss modulus (G″) of the ink in Examples 1 to 4 and Comparative Example 1 are curves showing the relationship between the storage modulus (G′) and the loss modulus (G″) and the oscillation strain; Fig.11 : is the frequency modulus curve of the ink in Examples 1 to 4 and Comparative Example 1; Fig.12 The thixotropy test curves of the inks in Examples 1 to 4 and Comparative Example 1 are shown.
[0105] from Fig. 9It can be seen that with the continuous increase of shear rate, the apparent viscosity of all inks shows a trend of increasing first and then decreasing; this shows that the apparent viscosity of the ink will increase appropriately within the range of action from static to small agitation; and after the rate increases to the critical value, the apparent viscosity of the ink decreases with the increase of shear rate, showing a shear thinning phenomenon. This rheological property can meet the needs of 3D printing process. Comparing the apparent viscosity curves of the five PSG inks, it can be found that the apparent viscosity of PSG-2 is lower than that of other components, and the content of silicene nanosheets corresponding to this ratio is greater than that of graphene. It shows that with the increase of the proportion of silicene nanosheets, the apparent viscosity of PSG ink will decrease, but within an appropriate range, this is beneficial for 3D printing film. The viscosity is relatively low, and the ink still has a certain degree of casting after printing and extrusion, which has a certain positive effect on the adjustment of film pores. PSG-5 contains only 80 mg of graphene, and the overall solid content of the film is the lowest, but its apparent viscosity is relatively the highest; comparison shows that graphene has a positive effect on the increase in the apparent viscosity of the ink, while silicene nanosheets will appropriately reduce the viscosity of the ink.
[0106] from Fig.10 It can be seen that when the oscillation strain is 10 -2 % to 10%, the storage modulus and loss modulus of PSG ink change slowly, indicating that when PSG ink is affected by small oscillations, its internal structure can withstand the influence of external disturbances and has good stability; when the oscillation strain increases further, the storage modulus and loss modulus of PSG ink drop sharply, especially when the oscillation strain is greater than 100%, the PSG ink begins to yield and then shows fluidity; PSG-2 has the lowest storage modulus and loss modulus, which corresponds to the aforementioned apparent viscosity, further illustrating that this ink is conducive to casting. The modulus value of PSG-4 ink is relatively high, indicating that the large amount of graphene and silicene nanosheets added will improve the ink's anti-disturbance ability, but its casting degree will decrease. The ink will take shape immediately after 3D printing and extrusion, and the holes or cracks at the interface between the PVA gel and the nanopowder will increase after drying, which is consistent with the aforementioned Figure 7 This will lead to a decrease in the hydrogen storage capacity and mechanical properties of the film.
[0107] from Fig.11 It can be seen that within the set frequency scanning range, the storage modulus (G′) and loss modulus (G″) of the five groups of PSG inks basically do not change greatly with the change of frequency, and generally tend to be stable and slightly rising. Moreover, within the entire frequency scanning range, the storage modulus of the five groups is higher than the loss modulus, indicating that the PSG ink is more evenly dispersed, has a higher degree of stability, and can be stored for a long time.
[0108] from Fig.12It can be seen that when the ink is subjected to the multiple continuous effects of "oscillation-shear-oscillation", the modulus values of the five groups of PSG inks will decrease, but the storage modulus is higher than the loss modulus, indicating that the ink remains stable; and after the ink is oscillated, the change in its apparent viscosity still maintains a trend of continuously decreasing with the increase in shear rate, which shows that the overall rheological properties of the five groups of PSG inks can meet the needs of 3D printing.
[0109] Use a tensile testing machine to test the room temperature tensile properties of the hydrogen storage composite films prepared in Examples 1 to 4 and the composite film prepared in Comparative Example 1: First, print a film structure of 3cm×1cm in size. After the film is dried, use a vernier caliper to measure the width and thickness of the film. Enter the data into the "test width" and "test thickness" in the tensile test program, and set the gauge length to 15 mm. Clamp one end of the film to the upper end of the test bench and fix it. Use a scale to determine the position of the lower end and rotate the nut to fix it. Make sure that the film samples are clamped at both ends to avoid falling off and causing test data errors. The film samples of the five components were measured separately and analyzed graphically. The results are as follows: Fig.13 As shown, Fig.13 These are the tensile strength test curves of the hydrogen storage composite films prepared in Examples 1 to 4 and the composite film prepared in Comparative Example 1 at room temperature.
[0110] from Fig.13 It can be seen that PSG-5 has the best tensile properties, while PSG-4 has poor tensile properties. This is related to the structure of the aforementioned films. There are almost no holes in the PSG-5 film, while PSG-4 has a large number of continuous holes, which will inevitably cause its mechanical properties to decline. For the other three groups of film samples, as the internal solid content increases, the overall mechanical properties improve; but when the proportion of graphene is relatively large, the mechanical properties of the film are better. It was observed that the mechanical properties of the PSG-2 film are relatively high and can withstand a tensile load of 2.2Kgf.
[0111] The hydrogen storage performance of the composite film prepared in Examples 1 to 4 and the composite film prepared in Comparative Example 1 was tested using an electrochemical workstation. By using a dual electrolytic cell device, each electrolytic cell is connected to an independent electrochemical system, and the film to be tested is sandwiched between the two electrolytic cells as a common working electrode. One end of the electrolytic cell is used as the cathode chamber, and the electrochemical workstation connected thereto uses a constant current charge and discharge method to charge hydrogen; the other end is used as the anode chamber, and the electrochemical workstation connected thereto uses a constant potential polarization method to measure hydrogen.
[0112] Preparation of PVA / silicene nanosheets / graphene composite film-based working electrode: cut out two nickel foam discs with a diameter of 26 mm and a copper bar with a length of 40 mm and a width of about 5 mm, clamp the PVA / silicene nanosheets / graphene composite film and one end of the copper bar in the middle of the two nickel foam discs, and press with a force of 6 MPa for 30 s to ensure that the copper bar does not loosen or fall off.
[0113] Assemble the electrochemical hydrogen diffusion test system: clamp the PVA / silicene nanosheet / graphene composite film-based working electrode between the double electrolytic cells, clamp it and ensure that the solution in the electrolytic cell does not leak out. The cathode chamber of the double electrolysis is connected to the constant current charge and discharge workstation, the electrolyte solution is 0.1 mol / L hydrochloric acid solution, the counter electrode is a Pt sheet electrode, the reference electrode is a saturated calomel electrode, the PVA / silicene nanosheet / graphene composite film is the working electrode, and the other end of the copper strip is clamped with a green chuck; the anode chamber is connected to the constant potential polarization workstation, the electrolyte solution is 0.1 mol / L hydrochloric acid solution, the counter electrode is a Pt sheet electrode, the reference electrode is a saturated calomel electrode, the PVA / silicene nanosheet / graphene composite film is the working electrode, and the other end of the copper strip is clamped with a green chuck, which is the same as the clamping position of the corresponding copper strip in the cathode chamber.
[0114] After assembling the test system, first add 0.1 mol / L hydrochloric acid solution into the anode chamber to perform hydrogen extraction operation; when the current reaches the anode residual current, add 0.1 mol / L hydrochloric acid solution into the cathode chamber to start the hydrogen diffusion test. The reaction principle is that the H generated in the cathode chamber + Arrived at the anode chamber.
[0115] The later calculation of hydrogen diffusion coefficient mainly uses Fick's first law (Formula I):
[0116] Formula I;
[0117] Where F is the Faraday constant and D is the hydrogen diffusion coefficient.
[0118] Right now
[0119] Formula II;
[0120] Formula III;
[0121] In the formula, It is the current corresponding to the lag time.
[0122] Formula IV;
[0123] In the formula, L is the thickness of the specimen, t Lis the corresponding lag time.
[0124] Fig.14 is the constant potential polarization curve of the hydrogen storage composite film prepared in Example 1; Fig.15 The constant potential polarization curve of the hydrogen storage composite film prepared in Example 2; Fig.16 The constant potential polarization curve of the hydrogen storage composite film prepared in Example 3; Fig.17 The constant potential polarization curve of the hydrogen storage composite film prepared in Example 4; Fig.18 This is the constant potential polarization curve of the composite film prepared in Comparative Example 1.
[0125] Read Figures 14 to 18 Substituting the data into formula I, the hydrogen diffusion coefficient D can be obtained. The sorted data are shown in Table 3.
[0126] Table 3 Hydrogen diffusion coefficients of the hydrogen storage composite films prepared in Examples 1 to 4 and the composite film prepared in Comparative Example 1
[0127]
[0128] It can be seen from Table 3 that the hydrogen diffusion coefficient of the hydrogen storage composite film prepared in Example 2 (the contents of graphene and silicene nanosheets are 60 mg and 80 mg, respectively) is the largest, which is 7.52×10 -6 cm 2 / s, with the best hydrogen storage performance.
[0129] In summary, when the content of silicene nanosheets in the composite film is the largest, the hydrogen storage performance is the best, which shows that appropriately increasing the content of silicene nanosheets can effectively enhance the hydrogen storage capacity of the composite film material; when the content of graphene is large, the mechanical properties of the composite film can be effectively enhanced.
[0130] It can be seen from the above examples and comparative examples that the hydrogen storage composite film prepared by the preparation method provided by the present invention has excellent hydrogen storage performance and mechanical properties.
[0131] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a hydrogen storage composite film, characterized in that: For the following steps: Mixing silicene nanosheets, graphene and PVA gel to obtain ink; 3D printing the ink to obtain a hydrogen storage composite film; The mass ratio of the PVA gel, graphene and silicene nanosheets is (30-60): (1-2): (1-2); The preparation method of the PVA gel comprises the following steps: The PVA powder and the inorganic solvent are mixed to form a gel to obtain the PVA gel.
2. The preparation method according to claim 1, characterized in that: The ratio of the mass of the PVA powder to the volume of the inorganic solvent is (0.03-0.1) g:1 mL.
3. The preparation method according to claim 1, characterized in that: The mixing is performed under stirring conditions.
4. The preparation method according to claim 3, characterized in that: The stirring speed is 700-1000 r / min, and the stirring temperature is 40-70°C.
5. The preparation method according to claim 1, characterized in that: The gelling process includes stirring and standing in sequence.
6. The preparation method according to claim 5, characterized in that: The stirring rate is 600-800 r / min, and the stirring time is 1.5-3 h.
7. The preparation method according to claim 1, characterized in that: The parameters of the 3D printing include: a needle diameter of 200-600 μm, an extrusion pressure of 20-50 psi, and a moving speed of 8-10 mm / s.
8. The hydrogen storage composite film prepared by the preparation method according to any one of claims 1 to 7.
Citation Information
Patent Citations
Material for an electrochemical device
CN101965657A
Method for synthesizing graphene film material
CN102020263A
Method for improving hydrogen storage performance of nano material
CN112209335A
Hydrogen storage fiber paper loaded with silylene-doped polyaniline
CN114045707A
Hydrogen storage material, and its manufacturing method
JP2005075707A
Cited By
Solid hydrogen storage membrane, amplification preparation method, system and application
CN121183333A