A polymer synergistic biomass flame retardant material and preparation method thereof

By combining biomass raw materials with ammonium polyphosphate and pentaerythritol, polymer synergistic biomass flame retardant materials are prepared, which solves the environmental pollution and fire risk problems of existing polymer flame retardant materials and achieves the excellent flame retardant properties of epoxy resin And safety is improved, reaching V-0 flame retardant level.

CN118460000BActive Publication Date: 2024-10-15HUZHOU SHENGSHI HUAJUN NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410926240.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-15
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

Existing polymer flame retardant materials have problems with environmental pollution and fire risks, especially the environmental toxicity and flammability of melamine and halogen flame retardants.

Method used

Using biomass raw materials such as protein and phytic acid discarded from agriculture, forestry, animal husbandry and fishery, combined with ammonium polyphosphate and pentaerythritol through modification treatment, polymer synergistic biomass flame retardant materials are prepared to replace some polymer chemical flame retardant materials for epoxy Resin system to improve flame retardant performance and safety.

Benefits of technology

It achieves the significant flame retardant effect of epoxy resin, reduces its flammability and smoke density, improves toughness, and reaches V-0 flame retardant grade, while reducing the risk of environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118460000B_ABST
    Figure CN118460000B_ABST
Patent Text Reader

Abstract

The invention discloses a polymer-biomass synergistic flame retardant material and a preparation method thereof. Based on the traditional polymer flame retardant material, the flame retardant material replaces part of the polymer raw material with biomass raw material, and uses it for the flame retardancy of epoxy resin, which can effectively reduce the heat and smoke density generated by combustion and can achieve UL94 V-0 level flame retardancy. At the same time, the addition of the biomass raw material can also simultaneously improve the smoke density and oxygen index of the flame retardancy of the epoxy resin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a polymer-biomass synergistic flame retardant material and a preparation method thereof. The flame retardant material mainly uses part of biomass raw materials to replace existing polymer compounds, has excellent environmental effects and significant flame retardant effects. Background Art

[0002] Halogen flame retardants are cheap, stable, low in addition, and highly compatible with synthetic resin materials. They can also maintain the original physical and chemical properties of flame retardant products. They are the world's largest organic flame retardants in terms of production and usage. However, some chemical flame retardants have environmental pollution problems. In this context, it has become an urgent need for the industry to gradually replace flame retardant raw materials such as melamine that have environmental pollution risks with other raw materials. On this basis, the present invention intends to use biomass flame retardant materials to replace melamine and other components of conventional polymer flame retardants, in order to obtain environmentally friendly, energy-saving and efficient flame retardant materials.

[0003] The slaughtering industry generates a large amount of waste during the meat processing process, and these wastes mainly include animal blood, bones, viscera, etc. If not handled properly, it will not only cause environmental pollution, but also lead to waste of resources. At present, there are some applications that can transform these wastes into valuable products through reasonable treatment and resource utilization, and can be processed into organic fertilizers, protein feed or meat and bone meal, etc. The present invention intends to utilize the protein resources discarded by agriculture, forestry, animal husbandry and fishery, and utilize the nitrogen element therein to release non-combustible gas during the combustion process, dilute the combustible gas, reduce the oxygen concentration, and thus inhibit the combustion process; through the nitrogen combustion process, nitrogen and nitric oxide and other substances are generated to reduce the flame temperature and thermal radiation intensity, while blocking the pores of the explosive and slowing down the chemical reaction rate. Phytic acid is an important chemical form for plants to store phosphorus. It is a renewable resource and can be used as a source of phosphorus in nitrogen-phosphorus flame retardants; phosphorus helps to form a carbon layer and inorganic residues during the combustion process, isolates heat and oxygen, and reduces the release of combustible gases, thereby achieving the purpose of flame retardancy. The present invention intends to use the protein discarded from agriculture, forestry, animal husbandry and fishery to react with phytic acid after modification to prepare biomass flame retardant materials, and replace some polymer chemical flame retardant materials. Epoxy resin (EP) is widely used in adhesives, coatings, matrix composite materials and electrical materials due to its excellent bonding strength, good mechanical strength, excellent chemical corrosion resistance, good dimensional stability and processing performance. However, epoxy resin itself is flammable, and the oxygen index is only about 19, which is an extremely flammable material. In a fire accident, epoxy resin is the most flammable part of the composite material. After the fire, it will continue to burn and produce a lot of smoke. Therefore, in order to improve the safety of epoxy resin and reduce the risk of fire, it is necessary to modify the epoxy resin to be flame retardant. For the flame retardant of epoxy system, halogen flame retardant is still the most used flame retardant, especially tetrabromobisphenol A epoxy resin and TBBPA (tribromophenoxyphenol). This type of flame retardant has prominent environmental toxicity problems, and the addition of 9~23% is generally required to achieve V-0 flame retardant effect. Summary of the invention

[0004] The present invention replaces part of the polymer raw materials with biomass raw materials on the basis of traditional polymer flame retardant materials, and is applied to the epoxy resin system, has good flame retardant effect and can play a toughening effect on the epoxy resin.

[0005] The technical solution adopted by the present invention is as follows:

[0006] A polymer synergistic biomass flame retardant material, characterized in that the flame retardant material comprises: ammonium polyphosphate, pentaerythritol and keratin phytic acid biomass.

[0007] Furthermore, the flame retardant material comprises, by weight percentage: 1 part of ammonium polyphosphate, 1 part of pentaerythritol, and 1 part of keratin phytic acid biomass.

[0008] Preferably, the flame retardant material comprises, by weight percentage: 5 parts of ammonium polyphosphate, 5 parts of keratin phytic acid biomass, and 2 parts of pentaerythritol.

[0009] Wherein, the preparation method of the keratin phytic acid biomass is:

[0010] Step 1: Preparation of keratin liquid: Wash, dry and crush the biomass material. After steam explosion, add sodium hydroxide solution into the reactor, adjust the pH to 8.5-9.5, stir at 80-100℃ for 3-4 hours, filter the solid impurities, and prepare keratin liquid;

[0011] Step 2: Add an appropriate amount of phytic acid to the keratin solution prepared in step 1, and adjust the pH of the solution system to 7.5-8.5. At the same time, add an appropriate amount of sepiolite powder as a reaction nucleating agent, react at 55-60° C. for 3-4 hours, filter, dry, and crush to obtain powder.

[0012] Furthermore, in step one, the biomass material is pig hoof horn, sheep hoof horn or wool.

[0013] Furthermore, the cleaning and drying are carried out at 50-80° C., the particle size after pulverization is controlled to be less than 1 mm, and the mass fraction of the sodium hydroxide solution is 0.5%-2%.

[0014] Preferably, the steam explosion pressure is 0.8-2.0 MPa, and the explosion time is 0.5-5 minutes; in the step 2, the mass ratio of the sodium hydroxide solution to the keratin prepared in the step 1 is 10:1-15:1.

[0015] Furthermore, in the step 2, the particle size of the added sepiolite powder is 30um~150um; and the amount of the sepiolite powder added is 10wt%~15wt% of the mass of the protein powder prepared in step 1;

[0016] Furthermore, in the step 2, the drying condition is 70-90° C., the powder is crushed and sieved to obtain a powder of 10-50 um.

[0017] The present invention also relates to an epoxy resin material with excellent flame retardant effect. The preparation method is as follows: adding the polymer synergistic biomass flame retardant material into the epoxy resin system at a ratio of 10%.

[0018] The beneficial effects of the present invention are as follows:

[0019] In the prior art, epoxy systems usually use polymer compositions as flame retardant materials. The inventors used polymer flame retardants composed of ammonium polyphosphate, pentaerythritol, and melamine in the early stage. These three have synergistic effects. Pentaerythritol is a carbon-forming agent. It will carbonize when heated at high temperatures, so that the carbon layer can isolate air and heat conduction to achieve the purpose of flame retardancy. When ammonium polyphosphate and melamine produce gas, the carbon layer expands, which increases the insulation efficiency. However, polymer raw materials face environmental safety issues. The present invention uses biomass materials to replace part of the polymer materials, and utilizes the nitrogen in protein resources to form combustion inert gas to dilute the combustible gas; the phosphorus contained in phytic acid can promote the formation of the carbon layer; prevent the rapid diffusion and transmission of combustible gas to the epoxy resin, and finally achieve the functions of flame retardancy and smoke suppression.

[0020] The flame retardant material of the present invention is added to the epoxy resin system to reduce its flammability and smoke density, and can reach V-0 level flame retardancy at the highest, and can effectively improve the toughness of the epoxy resin, and at the same time has a better effect in reducing smoke density.

[0021] Compared with traditional polymer composite flame retardant materials, the present invention can effectively prevent the combustion of epoxy resin and reduce the smoke generated by combustion; and during the processing, it will not affect the molding process, there is no phenomenon of migration to the sample surface, and it will not affect the surface morphology and mechanical properties (especially it can enhance the toughness of the material).

[0022] In the embodiment of the present invention, epoxy resin is taken as an example, and the polymer synergistic biomass flame retardant manufactured according to the present invention is added into the system to prepare a sample. From the data, it can be seen that the sample has excellent flame retardant performance, the heat release peak value and the total heat release rate are significantly reduced, and the UL94 flame retardant V0 grade test is passed. The mechanical properties are good, the toughness of the epoxy resin is enhanced, and the smoke density is significantly reduced, which has a significant technical effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The sample of the present invention passed the UL94 V-0 test chart.

[0024] Figure 2 Examples 1-5 and epoxy resin UL94 test results.

[0025] Figure 3 Examples 1-5 and the peak heat release and total heat release rate results of epoxy resin.

[0026] Figure 4 Examples 1-5 and epoxy resin smoke density and oxygen index results.

[0027] Figure 5 Examples 1-5 and epoxy resin tensile strength and elongation at break results. DETAILED DESCRIPTION

[0028] The present invention is described in detail below with reference to specific embodiments, but the protection scope of the present invention is not limited to the described implementation cases.

[0029] Embodiments of the present invention are as follows:

[0030] Example 1

[0031] Biomass flame retardant materials are prepared by the following methods:

[0032] Step 1: Preparation of keratin negative liquid: Wash, dry and crush the pig's hoof horn at 60°C to a particle size of 500um to 1000um; add 0.5% mass fraction of sodium hydroxide solution into the reactor after blasting at a steam pressure of 0.8MPa for 0.5 minutes, adjust the pH value to 8.5, stir at 100°C for 3 hours, filter the solid impurities, and prepare keratin liquid;

[0033] Step 2: Add an appropriate amount of phytic acid to the keratin solution obtained in step 1, and adjust the pH of the solution system to 7.5. At the same time, add sepiolite powder with a particle size of 30um~50um as a reaction nucleating agent (the amount of sepiolite powder added: 10% of the mass of the keratin negative solution prepared in step 1), react at 55°C for 4 hours, filter, dry at 70°C, crush the powder, and sieve to obtain a powder of 30~50um, which is the keratin phytic acid biomass.

[0034] In order to verify the flame retardant effect of the product of the present invention, this embodiment takes epoxy resin as an example, and the prepared biomass flame retardant is added to the epoxy resin system at a ratio of 10%, and a sample is finally obtained by curing and molding. The parameters of its flame retardant properties and mechanical properties are listed in the following Table 1:

[0035] Table 1

[0036]

[0037] It can be seen from the table that after adding biomass flame retardant to epoxy resin, the total heat release during combustion is significantly reduced, indicating that the heat generated during combustion is reduced and the degree of burns is reduced; the peak heat release is also reduced, which means that the maximum degree of heat release during combustion is suppressed; after adding the product of the invention, the oxygen index of the epoxy resin is greater than 26, which means that the material has a flame retardant type after adding the biomass flame retardant. After adding the product of the present invention, the UL94 combustion test of the epoxy resin reaches V-1 level. In addition, after adding the flame retardant material of the present invention, the tensile strength and elongation at break of the epoxy are improved to a certain extent.

[0038] Example 2

[0039] Ammonium polyphosphate, pentaerythritol and melamine are prepared in a ratio of 2:1:1 to form a flame retardant polymer material.

[0040] In order to verify the flame retardant effect of the product of the present invention, this embodiment takes epoxy resin as an example, and the prepared flame retardant is added to the epoxy resin system at a ratio of 10%, and a sample is finally obtained by curing and molding. The parameters of the flame retardant properties and mechanical properties are listed in the following Table 2:

[0041] Table 2

[0042]

[0043] As can be seen from the table, the flame retardant prepared by the polymer composition of the prior art has a lower total heat release during the combustion process, the degree of burns will be reduced, and the peak heat release is also reduced, which means that the maximum degree of heat release during the combustion process is suppressed; after adding the polymer flame retardant, the oxygen index of the epoxy resin is greater than 26, proving that it is flame retardant, and the UL94 combustion test of the epoxy resin reaches V-0 level. The tensile strength and elongation at break of the epoxy are significantly improved.

[0044] Compared with pure biomass materials, the peak heat release and total heat release rate of polymer compositions are lower. It can be seen that the flame retardant effect of directly replacing polymer flame retardants with biomass materials is reduced, and the tensile and elongation at break have not reached the level of existing polymer flame retardant technology. However, in terms of smoke index and oxygen index, it is not inferior to polymer compositions, and even has certain advantages.

[0045] On this basis, the inventors hope to use biomass raw materials for certain substitutions according to the mechanism of action of polymer raw materials, in order to combine the advantages of the two.

[0046] Example 3

[0047] Biomass flame retardant materials are prepared by the following methods:

[0048] Step 1: Preparation of keratin negative liquid: Wash, dry and crush the pig's hoof horn at 60°C to a particle size of 500um to 1000um; add 0.5% mass fraction of sodium hydroxide solution into the reactor after blasting at a steam pressure of 0.8MPa for 0.5 minutes, adjust the pH value to 8.5, stir at 100°C for 3 hours, filter the solid impurities, and prepare keratin liquid;

[0049] Step 2: Add an appropriate amount of phytic acid to the keratin solution obtained in step 1, and adjust the pH of the solution system to 7.5. At the same time, add sepiolite powder with a particle size of 30um~50um as a reaction nucleating agent (the amount of sepiolite powder added: 10% of the mass of the keratin negative solution prepared in step 1), react at 55°C for 4 hours, filter, dry at 70°C, crush the powder, and sieve to obtain a powder of 30~50um, which is the keratin phytic acid biomass.

[0050] Step 3: prepare the ammonium polyphosphate and the keratin phytic acid biomass obtained above in a ratio of 1:1 into a high molecular weight synergistic biomass flame retardant material.

[0051] In order to verify the flame retardant effect of the product of the present invention, this embodiment takes epoxy resin as an example, and the prepared flame retardant is added to the epoxy resin system at a ratio of 10%, and a sample is finally obtained by curing and molding. The parameters of the flame retardant properties and mechanical properties are listed in the following Table 3:

[0052] Table 3

[0053]

[0054] It can be seen from the table that the suppression of heat release peak and total heat release rate has not yet reached the level of polymer flame retardants, but can basically meet the flame retardant requirements of epoxy resin; the oxygen index reaches 29, and the smoke index is significantly lower than that of polymer flame retardants. The tensile strength and elongation at break are improved compared with pure biomass flame retardants, but still have not reached the level of polymer flame retardants. It can be seen that although the replaced pentaerythritol and melamine are auxiliary materials, they still have certain irreplaceable effects. Finally, the UL94 combustion test of the epoxy resin in this example reached V-1 level.

[0055] Example 4

[0056] On the basis of the above experiments, the applicant tried to retain pentaerythritol, which has a different mechanism of action, while still not adding melamine, which has a greater environmental problem.

[0057] The keratin synergistic phytic acid biomass flame retardant material is still prepared by the method of the above embodiment. Ammonium polyphosphate, keratin phytic acid biomass and pentaerythritol are prepared in a ratio of 1:1:1 to form a high molecular synergistic biomass flame retardant material.

[0058] In order to verify the flame retardant effect of the product of the present invention, this embodiment takes epoxy resin as an example, and the prepared flame retardant is added to the epoxy resin system at a ratio of 10%, and a sample is finally obtained by curing and molding. The parameters of the flame retardant properties and mechanical properties are listed in the following Table 4:

[0059] Table 4

[0060]

[0061] It can be seen from the table that the suppression of the heat release peak and the total heat release rate is further improved compared with the case without adding pentaerythritol, and the effect is not significantly different from that of the pure polymer flame retardant, which can meet the flame retardant requirements of epoxy resin; the oxygen index reaches 30, the tensile strength is significantly improved compared with Example 3 without adding pentaerythritol, and the elongation at break does not change significantly. Finally, the UL94 combustion test of the epoxy resin in this example reaches the V-1 level, but fails to reach the V-0 level.

[0062] Example 5

[0063] On the basis of Examples 3-4, the inventors tried to use the ratio of the polymer composition in Example 2, maintaining the total proportion of ammonium polyphosphate and appropriately increasing the proportion of biomass materials. Finally, they tried to configure ammonium polyphosphate, keratin phytic acid biomass, and pentaerythritol in a ratio of 5:5:2 to form a polymer synergistic biomass flame retardant material.

[0064] In order to verify the flame retardant effect of the product of the present invention, this embodiment takes epoxy resin as an example, and the prepared flame retardant is added to the epoxy resin system at a ratio of 10%, and a sample is finally obtained by curing and molding. The parameters of the flame retardant properties and mechanical properties are listed in the following Table 5:

[0065] Table 5

[0066]

[0067] It can be seen from the table that the suppression of the heat release peak and the total heat release rate is further improved compared with the ratio of Example 4, and can reach a level equivalent to that of the pure polymer in Example 2. The inventors speculate that this is related to the proportion control of the polymer ammonium polyphosphate, pentaerythritol and biomass. The smoke density and oxygen index are advantageous over those in Example 2; the tensile strength and elongation at break are slightly different from those in Example 2, and are even within the conventional error range. Finally, the UL94 combustion test of the epoxy resin in this example reaches the V-0 level. The combustion test results are as follows: Figure 1 shown.

[0068] The lateral comparison results of UL94 test, heat release test, smoke density and oxygen index, tensile strength and elongation at break test of Examples 1-5 are as follows: Figure 2-5 As shown. Finally, the inventors carried out subsequent large-scale verification with the proportion of Example 5, mainly including biomass stability adjustment and compatibility optimization. As far as the present invention is concerned, the inventors believe that its advantage lies in replacing part of the polymer raw materials with green and environmentally friendly biomass raw materials, and the flame retardant obtained can reach the level and efficacy of existing polymer flame retardants, and the heat release, elongation at break, and tensile strength can all meet industry standards. The smoke density and oxygen index are further improved compared to polymer flame retardants. In addition, there is still room for improvement in the present invention, such as the refined treatment of raw keratin, optimization of compatibility, and exploration of higher proportions of substitution.

Claims

1. A use of a polymer-biomass flame retardant material in improving the toughness and flame retardancy of an epoxy resin system, characterized in that: The flame retardant material comprises, by weight percentage: 5 parts of ammonium polyphosphate, 5 parts of keratin phytic acid biomass, and 2 parts of pentaerythritol; The preparation method of the keratin phytic acid biomass is: Step 1: Preparation of keratin liquid: Using commercially available pig hoof horns as raw materials, washing, drying and crushing the keratin part of the pig hoof horns, adding sodium hydroxide solution into a reactor after steam explosion, adjusting the pH to 8.5-9.5, stirring at high speed at 80-100°C for 3-4 hours, filtering solid impurities, and preparing keratin liquid; Step 2: Add an appropriate amount of phytic acid to the keratin solution prepared in step 1, adjust the pH of the solution system to 7.5-8.5, and add an appropriate amount of sepiolite powder as a reaction nucleating agent. After reacting at 55-60° C. for 3-4 hours, filter, dry, and crush to obtain a powder, which is keratin phytic acid biomass; The cleaning and drying in step 1 are carried out at 50-80° C., the particle size after crushing is controlled to be less than 1 mm, and the mass fraction of the sodium hydroxide solution is 0.5%-2%; The steam explosion pressure is 0.8-2.0 MPa, and the explosion time is 0.5-5 minutes; in the step 2, the mass ratio of the sodium hydroxide solution to the keratin prepared in the step 1 is 10:1-15:1; In the step 2, the particle size of the added sepiolite powder is 30um~150um; and the amount of the sepiolite powder added is 10wt%~15wt% of the mass of the protein powder prepared in step 1; In the step 2, the drying condition is 70-90° C., the powder is crushed, and sieved to obtain a powder of 10-50 um.