A method for producing ultra-fine wire
By replenishing the spinneret in real-time in ultra-fine filament production, the heat loss problem of spinneret is solved, the uniformity of spinning quality and production efficiency are improved, and the thermal stress difference and breaking of the product are reduced.
Patent Information
- Application Number
- CN202410911311.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-09
AI Technical Summary
In the production of ultrafine filament, the heat loss of the spinning plate causes the temperature of the spinning assembly to drop, affecting the spinningability and quality of the wire. The existing technology is difficult to effectively solve, resulting in the difference in thermal stress and quality of the product's bottom yarn and surface yarn. Uniformity.
Control the temperature of the heating plate in the spinning box by 7~10℃ higher than the normal spinning temperature. The spinning plate is heated in real time during the cleaning process, and heated the spinning plate is used to provide heat to ensure the spinning plate temperature. stability.
The quality uniformity of the yarn on the bottom of the POY surface after the ultra-fine filament is improved, the head breaking rate and the success rate of over-tail are reduced, the product is improved, and the quality abnormalities caused by thermal stress differences are avoided.
Smart Images

Figure CN118480871B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of superfine filament production and relates to a method for producing superfine filaments. Background Art
[0002] Due to production needs, the spinneret of the spinning assembly needs to be cleaned and repaired regularly, usually every 1 to 2 days, to keep the plate surface clean. However, in the production of ultra-fine filaments, due to the large number of holes and small hole diameters in the spinneret, the plate cleaning cycle is significantly shortened. Often, the spinneret surface becomes dirty about ten hours after cleaning, which can easily cause problems such as spinning breakage and floating filaments, increasing production costs.
[0003] The ring-blowing cooling device is mainly used to produce porous fine denier and ultrafine denier fibers. For the ring-blowing spinning position, the conventional spinning board cleaning operation requires a series of steps such as stopping spinning, lowering the bellows 50~70cm, spraying silicone oil while cleaning the board, and re-hanging the silk. However, there is a lot of heat loss in this process; the temperature of the POY spinning box is generally around 292℃, while the temperature of the spinning workshop is usually around 30℃, and there is a large temperature difference between the two. After lowering the spinning bellows, the lower surface of the spinning box and the surrounding cold air produce convection, which will cause a large amount of heat loss on the spinneret surface of the spinning assembly over a period of time; in addition, during the board cleaning process, silicone oil needs to be sprayed repeatedly on the spinneret surface, and the silicone oil at room temperature evaporates due to heat and takes away part of the heat; at the same time, part of the cooling air in the ring-blowing bellows blows vertically to the spinneret surface, causing the temperature of the spinneret surface of the assembly to lose rapidly.
[0004] Patent CN101440532, a method for maintaining a stable temperature of a spinneret, points out that the drop in spinneret temperature during spinneret cleaning affects the spinnability of the melt and the quality of the spun yarn bundle, especially the bottom layer of yarn in the first drop winding molding after the spinneret cleaning is completed. The effect is the greatest, which is manifested in obvious tension fluctuations when this part of the yarn is used for post-spinning processing, affecting its post-processing performance and quality.
[0005] In order to solve the above problems, patent CN 201339076Y provides a set of automatic control devices for the air valve of the spinning cooling system of the ring-blowing production of chemical fiber filaments, that is, the air supply of the ring-blowing system is stopped during the plate cleaning operation, and the cooling air in the ring-blowing bellows is inhibited from blowing vertically to the spinneret surface; patent CN116427040A provides a spinning device, which is used to cover the top of the ring-blowing bellows during the plate cleaning operation to reduce the cooling air in the ring-blowing bellows blowing vertically to the spinneret surface; patent CN116555925A discloses a preparation device for fine denier and special-shaped polyester pre-stretched yarns, in which a slow cooler is arranged around the spinneret, and the slow cooler is used to compensate for the extra heat loss of the spinneret during the spinning process, which can effectively reduce the thermal stress of the polyester pre-oriented yarn and improve the quality and stability of the fiber.
[0006] The above patents can reduce the heat loss of the component spinneret during the plate cleaning operation to a certain extent, but the heat on the spinneret will still be lost, and the problem cannot be fundamentally solved. After the plate cleaning operation, the spinneret surface temperature is usually 4~7℃ lower than the normal spinning temperature. This temperature difference takes time (25~35 minutes) to balance and recover during normal spinning. The smaller the pipeline melt flow, the longer it takes for the spinneret temperature to recover. This is particularly obvious in the production process of fine denier porous yarns, and ultra-fine denier fibers have higher requirements for the spinneret surface temperature. If there is no artificial intervention in the heat loss of the component spinneret surface caused by the plate cleaning process, there will be a large difference in the physical properties of the bottom yarn and the surface yarn of the product, especially in the thermal stress data.
[0007] In order to ensure the quality uniformity of the bottom yarn and the surface yarn of the ultra-fine denier silk cake, the existing technology mostly chooses the method of cutting small rolls, that is, after spinning for a period of time after the spinning assembly spinneret surface temperature balance is restored, the spun small rolls are cut off and thrown away. However, this method not only reduces the product quality rate, but also increases the workload.
[0008] Therefore, it is of great significance to develop a method for producing ultrafine filaments that can solve the above problems. Summary of the invention
[0009] The purpose of the present invention is to solve the problems existing in the prior art and provide a method for producing ultra-fine filaments.
[0010] To achieve the above object, the technical solution adopted by the present invention is as follows:
[0011] A method for producing ultrafine filaments includes a plate clearing operation. During the plate clearing process, a controller is used to control the temperature of a heating plate in a spinning box to be 7-10°C higher than the temperature of the heating plate during normal spinning. During the plate clearing process, the temperature of the heating plate in the spinning box is increased to compensate for the heat loss of the spinneret during the plate clearing process, thereby achieving real-time heating of the spinneret.
[0012] As the preferred technical solution:
[0013] A method for producing ultrafine filaments as described above, wherein the heating plate is a rectangular plate, and n circular through holes are vertically opened on the heating plate, where n is equal to the number of spinnerets, and n ≥ 1, and the n circular through holes are arranged at intervals along the length direction of the heating plate and correspond one to one to the n spinnerets;
[0014] The spinneret is located inside the corresponding circular through hole, and the spinneret and the corresponding circular through hole are coaxial;
[0015] The lower surface of the spinneret is flush with the lower surface of the heating plate, which reduces the extrusion expansion effect caused by the melt passing through the spinneret holes, ensures that the primary filaments can quickly enter the cooling area, and quickly cools the filaments just extruded from the spinneret;
[0016] Heating alloy coils are evenly laid inside the heating plate. When these heating alloy coils are energized by an external power source, the alloy coils generate heat, which is transferred to the spinneret of the spinning assembly by radiation, continuously replenishing heat to the spinneret.
[0017] A method for producing ultra-fine filaments as described above, wherein the controller comprises a PC terminal, a PLC and a conversion switch;
[0018] The PLC is electrically connected to the PC and the switch, and the switch is electrically connected to the heating plate;
[0019] The PC end is used to set the first working temperature and the second working temperature, and send the set first working temperature and the second working temperature to the PLC; the first working temperature is 7-10°C higher than the second working temperature, and the second working temperature is the spinning temperature;
[0020] The PLC is used to store the first working temperature and the second working temperature set by the PC, and send the first working instruction and the second working instruction to the conversion switch;
[0021] The conversion switch is used to: when the plate cleaning starts, send the first working instruction to the heating plate, so that the temperature of the heating plate is the first working temperature; when the plate cleaning ends, send the second working instruction to the heating plate, so that the temperature of the heating plate is the second working temperature.
[0022] As described above, the spinning parameters in the production process of ultrafine filaments are as follows: cooling air supply pressure is 13~15Pa, cooling air temperature is 19~20℃, cooling air relative humidity is 85~87%, oiling rate is 0.52~0.57wt%, spinning speed is 2100~2150m / min, spinning box temperature is 292~294℃, heating plate temperature is 305~320℃, and bunching height is 625~635cm.
[0023] The method for producing ultrafine filaments as described above has a specification of 45-60 dtex / 144f, a POY full winding rate ≥ 97.5%, and a tail passing success rate ≥ 92.55%.
[0024] According to the method for producing ultrafine filaments as described above, in a fully rolled ultrafine filament cake, the strength of the bottom yarn is 98.88-99.23% of that of the surface yarn, the strength unevenness is 102.33-105.91% of that of the surface yarn, the elongation is 99.05-99.25% of that of the surface yarn, the elongation unevenness is 105.53-106.04% of that of the surface yarn, the thermal stress is 102.65-102.81% of that of the surface yarn, and the thermal stress unevenness is 115.7-122.5% of that of the surface yarn.
[0025] Principle of the invention:
[0026] Affected by the low temperature of the spinneret surface, the intrinsic quality of the spun fiber is unstable, and the suction gun pressure is difficult to control during spinning, which can easily lead to spinning failure. At the same time, the low spinneret surface temperature increases the outlet expansion and melt fracture of the spun fiber, and abnormal fibers such as floating fibers, hard head fibers, and injected head fibers are prone to occur. These abnormal fibers are prone to breakage during the winding process, so repeated spinning is required, which seriously affects the product quality.
[0027] In the prior art, the temperature of the heating plate is achieved through parameter control. This control method relies on manual settings by engineering technicians on the PC side. Once the setting is completed, it will not change during the fiber spinning process. If the temperature needs to be adjusted to adapt to different fiber batches, engineering technicians need to travel back and forth between the spinning site and the central control room to reset new parameters. This lacks flexibility and real-time performance, and is difficult to meet the complex and changeable spinning production needs.
[0028] The present invention adds a second working instruction to the existing heating plate control system and sets a command conversion switch for the bottom heater on the spinning box. The engineering and technical personnel can set the heating temperature of the first working instruction and the second working instruction in advance on the PC end. During normal spinning, the PLC gives the first working instruction of the heating plate to ensure the uniform molding of the primary fiber. When the plate is cleared and the head is produced, the conversion switch is pressed, and the PLC gives the second working instruction of the heating plate to switch the heating temperature. After the plate is cleared, the conversion switch is pressed again, and the heating temperature is switched again. One-key switching is convenient, time-saving and labor-saving. There is no need for engineering and technical personnel to travel back and forth between the spinning site and the central control room, thereby improving production efficiency and product quality.
[0029] Beneficial effects:
[0030] (1) The method for producing ultra-fine filaments of the present invention improves the uniformity of the quality of the POY top and bottom yarns after the ultra-fine filaments are cleaned, the POY top and bottom yarns have small thermal stress differences, few broken ends, and a high success rate of tail passing;
[0031] (2) The present invention provides a method for producing ultra-fine filaments. After the ultra-fine filaments are periodically cleaned and produced, there is no need to switch to small coils for isolation and downgrading for 25 to 35 minutes, thereby improving the quality rate of POY products and avoiding the production of cheap small coils.
[0032] (3) In the method for producing ultrafine filaments of the present invention, the post-spinning and texturing workshop does not need to worry about the abnormal color of dyeing caused by the difference in thermal stress between the surface and bottom layers of the yarn due to periodic board cleaning, thereby ensuring the uniformity of product quality and reducing the difference in product post-spinning use. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 is a control logic diagram of the controller in the present invention;
[0034] Figure 2 It is a schematic diagram of the positions of the surface yarn and the bottom yarn in a full-rolled silk cake;
[0035] Among them, 1-PC end, 2-PLC, 3-conversion switch, 4-heating plate, 5-bottom yarn, 6-surface yarn. DETAILED DESCRIPTION
[0036] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0037] The test / calculation methods involved in the performance indicators of the present invention are as follows:
[0038] (1) POY full roll rate: Full roll rate = full roll weight / off-machine output, where full roll weight is the total weight of all POY rolls that have reached the preset weight within a time period t, and off-machine output is the total weight of POY rolls that have been unloaded from the spinning machine within the same time period t;
[0039] (2) Tail passing success rate: Tail passing success rate = number of spindles that have successfully passed the tail on a single machine / total number of spindles on a single machine;
[0040] (3) Strength, strength unevenness, elongation and elongation unevenness: tested in accordance with GB / T 14344-2022;
[0041] (4) Thermal stress and thermal stress unevenness: The test was carried out in accordance with FZ / T 50051-2020, where the pre-tension was (0.05±0.005) cN / dtex, the test temperature was 170°C, the test speed was 100 m / min, the test length was 50 m, the pre-tension length was 10 m, and the draft ratio was 1.60 times.
[0042] The device for producing ultrafine filaments in the embodiment includes a heating plate, a controller and n spinnerets, n≥1;
[0043] The heating plate is a rectangular plate, and n circular through holes are vertically opened on the heating plate. The n circular through holes are arranged at intervals along the length direction of the heating plate and correspond to the n spinnerets one by one.
[0044] The spinneret is located inside the corresponding circular through hole, and the spinneret and the corresponding circular through hole are coaxial;
[0045] The lower surface of the spinneret is flush with the lower surface of the heating plate;
[0046] The heating alloy coils are evenly laid inside the heating plate;
[0047] like Figure 1 As shown, the controller includes a PC terminal 1, a PLC 2 and a conversion switch 3;
[0048] The PLC 2 is electrically connected to the PC terminal 1 and the conversion switch 3 at the same time, and the conversion switch 3 is electrically connected to the heating plate 4;
[0049] PC terminal 1 is used to set the first working temperature and the second working temperature, and send the set first working temperature and the second working temperature to PLC 2; the first working temperature is 7-10°C higher than the second working temperature, and the second working temperature is the spinning temperature;
[0050] The PLC 2 is used to store the first working temperature and the second working temperature set by the PC terminal 1, and send the first working instruction and the second working instruction to the conversion switch 3;
[0051] The conversion switch 3 is used to: when the plate cleaning starts, send the first working instruction to the heating plate 4 so that the temperature of the heating plate 4 is the first working temperature; when the plate cleaning ends, send the second working instruction to the heating plate 4 so that the temperature of the heating plate 4 is the second working temperature.
[0052] Example 1
[0053] A method for producing ultra-fine wires, including a plate clearing operation;
[0054] The spinning parameters in the production process include: cooling air supply pressure of 15Pa, cooling air temperature of 19.3℃, cooling air relative humidity of 85%, oiling rate of 0.52wt%, spinning speed of 2120m / min, spinning box temperature of 293℃, heating plate temperature of 320℃, and clustering height of 625cm;
[0055] During the plate cleaning process, the temperature of the heating plate in the spinning box is controlled by the controller to be 10°C higher than the temperature of the heating plate during normal spinning. The amount of silicone oil used during plate cleaning is 60ml / spinning position, and the plate cleaning time is 4min / spinning position.
[0056] The final ultra-fine yarn has a specification of 45dtex / 144f, a POY full winding rate of 97.50%, and a tail passing success rate of 92.55%; Figure 2 The figure shows the positions of the surface yarn 6 and the bottom yarn 5 in the full-wind silk cake of superfine silk. In the full-wind silk cake of superfine silk, the strength of the bottom yarn is 98.88% of that of the surface yarn, the strength unevenness is 105.91% of that of the surface yarn, the elongation is 99.05% of that of the surface yarn, the elongation unevenness is 106.04% of that of the surface yarn, the thermal stress is 102.81% of that of the surface yarn, and the thermal stress unevenness is 122.50% of that of the surface yarn.
[0057] Comparative Example 1
[0058] A method for producing ultrafine filaments is basically the same as Example 1, except that: in this comparative example, the plate cleaning operation is performed according to the method of the prior art, that is, the temperature of the heating plate is not increased during the plate cleaning process.
[0059] The final specifications of the ultrafine filaments are 45dtex / 144f, the POY full roll rate is 94.10%, and the tail-passing success rate is 90.23%; in the ultrafine filament full roll silk cake, the strength of the bottom yarn is 95.42% of that of the surface yarn, the strength unevenness is 114.78% of that of the surface yarn, the elongation is 98.19% of the surface yarn, the elongation unevenness is 109.43% of the surface yarn, the thermal stress is 125.26% of that of the surface yarn, and the thermal stress unevenness is 255.71% of the surface yarn.
[0060] By comparing Example 1 with Comparative Example 1, it can be found that the POY full roll rate and tail-passing success rate of the ultrafine filaments prepared in Comparative Example 1 are reduced, the strength and elongation of the bottom yarn are reduced, and the strength unevenness, elongation unevenness, thermal stress and thermal stress unevenness of the bottom yarn are increased. This is because in the spinning process, after the comparative example 1 uses the method of the prior art to clean the plate, since there is no artificial intervention in the heat loss of the spinneret during the cleaning process, the spinneret surface temperature will be 4~7°C lower than the normal spinning temperature; after the cleaning is completed, it takes a certain amount of time for the spinneret surface temperature to return to normal; however, the spinning process does not wait for the spinneret surface temperature to fully recover before it starts; this low temperature state has a significant impact on the fiber quality. On the one hand, since the temperature has not reached the normal spinning temperature, the spinning temperature will not reach the normal spinning temperature. level, the intrinsic quality of the spun fiber is unstable, and the strength unevenness and elongation unevenness of the bottom yarn increase accordingly; at the same time, low temperature reduces the free space between molecules, which is not conducive to the thermal motion of the molecules inside the fiber, slows down the relaxation process, and makes it impossible to release the stress inside the filament in time, and the thermal stress index increases accordingly; on the other hand, the low temperature of the spinneret surface also increases the outlet swelling and melt fracture of the spun fiber, and it is easy to have abnormal filaments such as floating filaments, hard head filaments, and injected head filaments. These abnormal filaments are easy to cause breakage during the winding stroke and need to be repeatedly re-spun, so the POY full roll rate is reduced. When these poor quality POY raw yarns are used in the post-spinning and texturing workshop, high tension or even shredding will occur, resulting in a decrease in the success rate of the bottom yarn using texturing.
[0061] Example 2
[0062] A method for producing ultra-fine wires, including a plate clearing operation;
[0063] The spinning parameters in the production process include: cooling air supply pressure of 13Pa, cooling air temperature of 19.5℃, cooling air relative humidity of 87%, oil loading rate of 0.57wt%, spinning speed of 2150m / min, spinning box temperature of 292℃, heating plate temperature of 310℃, and cluster height of 635cm;
[0064] During the plate cleaning process, the temperature of the heating plate in the spinning box is controlled by the controller to be 8°C higher than the temperature of the heating plate during normal spinning. The amount of silicone oil used during plate cleaning is 55ml / spinning position, and the plate cleaning time is 4min / spinning position.
[0065] The final specifications of the ultrafine filaments are 58dtex / 144f, the POY full roll rate is 97.50%, and the tail passing success rate is 93.02%; in the ultrafine filament full roll silk cake, the strength of the bottom yarn is 99.02% of the surface yarn, the strength unevenness is 103.11% of the surface yarn, the elongation is 99.23% of the surface yarn, the elongation unevenness is 105.78% of the surface yarn, the thermal stress is 102.72% of the surface yarn, and the thermal stress unevenness is 118.3% of the surface yarn.
[0066] Example 3
[0067] A method for producing ultra-fine wires, including a plate clearing operation;
[0068] The spinning parameters in the production process include: cooling air supply pressure of 14Pa, cooling air temperature of 20℃, cooling air relative humidity of 85%, oiling rate of 0.51wt%, spinning speed of 2150m / min, spinning box temperature of 294℃, heating plate temperature of 307℃, and clustering height of 635cm;
[0069] During the plate cleaning process, the temperature of the heating plate in the spinning box is controlled by the controller to be 8°C higher than the temperature of the heating plate during normal spinning. The amount of silicone oil used during plate cleaning is 50ml / spinning position, and the plate cleaning time is 3min / spinning position.
[0070] The final specifications of the ultrafine filaments are 59dtex / 144f, the POY full roll rate is 97.60%, and the tail passing success rate is 93.65%; in the ultrafine filament full roll silk cake, the strength of the bottom yarn is 99.22% of that of the surface yarn, the strength unevenness is 102.45% of that of the surface yarn, the elongation is 99.25% of that of the surface yarn, the elongation unevenness is 105.53% of that of the surface yarn, the thermal stress is 102.66% of the surface yarn, and the thermal stress unevenness is 116.9% of the surface yarn.
[0071] Example 4
[0072] A method for producing ultra-fine wires, including a plate clearing operation;
[0073] The spinning parameters in the production process include: cooling air supply pressure of 15Pa, cooling air temperature of 19.5℃, cooling air relative humidity of 86%, oil loading rate of 0.57wt%, spinning speed of 2100m / min, spinning box temperature of 293℃, heating plate temperature of 305℃, and clustering height of 635cm;
[0074] During the plate cleaning process, the temperature of the heating plate in the spinning box is controlled by the controller to be 7°C higher than the temperature of the heating plate during normal spinning. The amount of silicone oil used during plate cleaning is 50ml / spinning position, and the plate cleaning time is 3min / spinning position.
[0075] The final specification of the ultrafine filament is 60dtex / 144f, the POY full roll rate is 97.80%, and the tail passing success rate is 93.67%; in the ultrafine filament full roll silk cake, the strength of the bottom yarn is 99.23% of that of the surface yarn, the strength unevenness is 102.33% of that of the surface yarn, the elongation is 99.25% of that of the surface yarn, the elongation unevenness is 105.53% of that of the surface yarn, the thermal stress is 102.65% of that of the surface yarn, and the thermal stress unevenness is 115.70% of that of the surface yarn.
[0076] Comparative Example 2
[0077] A method for producing ultrafine filaments is basically the same as Example 4, except that: this comparative example uses the prior art method to perform the plate cleaning operation, that is, the temperature of the heating plate is not increased during the plate cleaning process.
[0078] The final specifications of the ultrafine filaments are 60dtex / 144f, the POY full roll rate is 94.8%, and the tail passing success rate is 91.73%; in the ultrafine filament full roll silk cake, the strength of the bottom yarn is 95.88% of that of the surface yarn, the strength unevenness is 104.67% of that of the surface yarn, the elongation is 98.08% of the surface yarn, the elongation unevenness is 113.83% of the surface yarn, the thermal stress is 119.87% of the surface yarn, and the thermal stress unevenness is 206.25% of the surface yarn.
[0079] By comparing Comparative Example 2 with Example 4, it can be found that the POY full roll rate and tail-passing success rate of the ultrafine filaments prepared in Comparative Example 2 are reduced, the strength and elongation of the bottom yarn are reduced, and the strength unevenness, elongation unevenness, thermal stress and thermal stress unevenness of the bottom yarn are increased. This is because in the spinning process, after the comparative example 2 uses the existing technology to clean the plate, since there is no artificial intervention in the heat lost by the spinneret during the cleaning process, the spinneret surface temperature will be 4~7°C lower than the normal spinning temperature; after the cleaning is completed, it takes a certain amount of time for the spinneret surface temperature to return to the normal state; however, the spinning process does not wait for the spinneret surface temperature to fully recover before it starts; this low temperature state has a significant impact on the fiber quality. On the one hand, since the temperature has not reached the normal spinning level , the intrinsic quality of the spun fiber is unstable, and the strength unevenness and elongation unevenness of the bottom yarn increase accordingly; at the same time, low temperature reduces the free space between molecules, which is not conducive to the thermal motion of the molecules inside the fiber, slows down the relaxation process, and makes it impossible to release the stress inside the filament in time, and the thermal stress index increases accordingly; on the other hand, the low temperature of the spinneret surface also increases the outlet swelling and melt fracture of the spun fiber, and it is easy to have abnormal filaments such as floating filaments, hard head filaments, and injected head filaments. These abnormal filaments are easy to cause breakage during the winding stroke and need to be repeatedly re-spun. Therefore, the POY full roll rate is reduced. When these poor quality POY raw yarns are used in the post-spinning and texturing workshop, high tension or even silk cutting will occur, resulting in a decrease in the success rate of the bottom yarn using texturing.
Claims
1. A method for producing ultrafine wires, comprising a plate cleaning operation, characterized in that: During the plate cleaning process, the temperature of the heating plate in the spinning box is controlled by a controller to be 7-10°C higher than the temperature of the heating plate during normal spinning; the controller includes a PC terminal, a PLC and a conversion switch; The PLC is electrically connected to the PC and the switch, and the switch is electrically connected to the heating plate; The PC end is used to set the first working temperature and the second working temperature, and send the set first working temperature and the second working temperature to the PLC; the first working temperature is 7-10°C higher than the second working temperature, and the second working temperature is the spinning temperature; The PLC is used to store the first working temperature and the second working temperature set by the PC, and send the first working instruction and the second working instruction to the conversion switch; The conversion switch is used to: when the plate cleaning starts, send the first working instruction to the heating plate, so that the temperature of the heating plate is the first working temperature; when the plate cleaning ends, send the second working instruction to the heating plate, so that the temperature of the heating plate is the second working temperature.
2. The method for producing ultra-fine filaments according to claim 1, characterized in that: The heating plate is a rectangular plate, and n circular through holes are vertically opened on the heating plate, where n is equal to the number of spinnerets, n≥1, and the n circular through holes are arranged at intervals along the length direction of the heating plate and correspond one to one to the n spinnerets; The spinneret is located inside the corresponding circular through hole, and the spinneret and the corresponding circular through hole are coaxial; The lower surface of the spinneret is flush with the lower surface of the heating plate; The heating alloy coils are evenly laid inside the heating plate.
3. A method for producing ultra-fine filaments according to claim 1 or 2, characterized in that: The spinning parameters in the ultrafine filament production process are: cooling air supply pressure is 13~15Pa, cooling air temperature is 19~20℃, cooling air relative humidity is 85~87%, oiling rate is 0.52~0.57wt%, spinning speed is 2100~2150m / min, spinning box temperature is 292~294℃, heating plate temperature is 305~320℃, and bunching height is 625~635cm.
4. The method for producing ultra-fine filaments according to claim 3, characterized in that: The specifications of the ultra-fine filaments are 45~60dtex / 144f, the POY full winding rate is ≥97.5%, and the tail passing success rate is ≥92.55%.
5. The method for producing ultra-fine filaments according to claim 4, characterized in that: In the fully rolled cake of ultra-fine yarn, the strength of the bottom yarn is 98.88~99.23% of that of the surface yarn, the strength unevenness is 102.33~105.91% of that of the surface yarn, the elongation is 99.05~99.25% of that of the surface yarn, the elongation unevenness is 105.53~106.04% of that of the surface yarn, the thermal stress is 102.65~102.81% of that of the surface yarn, and the thermal stress unevenness is 115.7~122.5% of that of the surface yarn.