A method for preparing synthesis gas by dry reforming of carbon dioxide / methane

Through a synergistic catalytic system of high-energy electron beams and nickel and other metal combination catalysts, the dry reforming reaction between methane and carbon dioxide is carried out at a lower temperature, which solves the problem of reduced catalyst activity and carbon deposits, improves reaction efficiency and reduces costs.

CN118495472BActive Publication Date: 2024-11-29OPTIMUM PROCESS TECH SHANGHAI CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202410971601.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-29
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

The existing methane dry reforming technology has the problem of reduced catalyst activity and carbon deposit formation at high temperatures, resulting in low reaction efficiency and high cost, making it difficult to achieve industrial application.

Method used

A collaborative catalytic system with a high-energy electron beam combined with nickel and other metal catalysts is adopted to carry out dry reforming of carbon dioxide and methane at 300°C to 500°C through high-energy electron beam irradiation, reducing the reaction temperature and extending the catalyst life.

Benefits of technology

It realizes efficient catalyzing of methane and carbon dioxide conversion at lower temperatures, reducing the carbon deposits of the catalyst, extending the service life of the catalyst, improving the reaction efficiency and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118495472B_ABST
    Figure CN118495472B_ABST
Patent Text Reader

Abstract

The present application relates to a method for preparing synthesis gas by dry reforming of carbon dioxide / methane. The method includes using a catalytic system, and the catalytic system includes a high-energy electron beam and a catalyst. Through the catalytic system of the high-energy electron beam and the catalyst, the dry reforming of carbon dioxide and methane at a relatively low temperature is achieved, which solves the carbon deposition problem of the dry reforming reaction to a certain extent, prolongs the service life of the catalyst, and provides a guarantee for stable production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of methane dry reforming reaction, and relates to a method for preparing synthesis gas by dry reforming of carbon dioxide / methane. Background Art

[0002] To address global warming, reducing dependence on fossil energy is a key step. Fossil energy, such as coal, oil and natural gas, is the main source of greenhouse gas emissions. On the one hand, reducing dependence on fossil energy and increasing the use of new energy can help reduce greenhouse gas emissions and slow down the process of global warming. On the other hand, recycling and reusing greenhouse gases that have already been emitted can achieve more results with less effort, especially when these captured greenhouse gases can be further produced into high-value-added products, such as synthetic fuels or raw materials and intermediates for petrochemicals. Methane dry reforming (DRM) is one of the most promising ways to mitigate global warming because it can simultaneously convert two major greenhouse gases into synthesis gas, thereby providing versatility as a gas fuel or a raw material for high-value chemical and liquid fuel products. Currently, a variety of methods have been used to convert carbon dioxide through homogeneous and heterogeneous catalytic reactions, including photocatalytic reactions, electrochemical conversion, carbon dioxide hydrogenation, carboxylation reactions, polymer synthesis and dry reforming.

[0003] In recent years, dry reforming has received increasing attention. In this process, carbon dioxide is used for the catalytic reforming of hydrocarbons to produce synthesis gas (hydrogen and carbon monoxide). A large number of studies have focused on the dry reforming of carbon dioxide with alkanes (methane, ethane and butane) and alcohols (ethanol, methanol and glycerol). Among them, the dry reforming of carbon dioxide with methane has received special attention. In addition to the above-mentioned advantages of carbon dioxide reuse, this technology can obtain a higher CO / H2 ratio than traditional methane steam reforming, which is crucial for the production of some downstream chemicals (such as methanol, olefins, acetic acid, acetic anhydride, ethers and ammonia) (patent number: CN107921427B).

[0004] Methane dry reforming is usually carried out at temperatures exceeding 600°C using catalysts containing Ni, Rh, Pt, Ru, and Co supported on inert supports. The industrialization of methane dry reforming still faces many difficulties: both CH4 and CO2 reactants are highly stable, and in order to achieve considerable conversion in highly endothermic reactions, very high energy input from external heating and long conversion times are required. On an industrial scale, the main problem of dry reforming is the reduction in catalyst activity and carbon deposition during high-temperature reactions: Patent US11724937B2 uses 8-16wt.% Ni and 2-14wt.% Cu supported on Al2O3 and MgO catalysts for methane dry reforming. The performance of DRM depends on the catalyst used, among which Ni-based catalysts have the advantages of low cost and availability, and have a better balance between cost-effectiveness and active performance. However, this type of catalyst will be deactivated by carbon deposition because carbon covers the active sites on the catalyst surface and metal particles will sinter due to the migration of atoms or molecules on the catalyst surface.

[0005] The use of noble metal catalysts Ru and Rh has relatively higher activity and is resistant to carbon deposition. For example, in Well-dispersed Rh nanoparticles with high activity for the dry reforming of methane (DOI: 10.1016 / j.ijhydene.2017.04.070), the conversion rate of methane reached 77% using a catalyst loaded with not less than 0.36% Rh on CaO / SiO2. However, due to the high cost and limited supply of noble metal catalysts, it is not feasible to apply them on an industrial scale.

[0006] In summary, it can be found that the existing regulation of the interaction between metal and support can be a strategy to enhance catalytic activity and alleviate carbon deposition, but it cannot fundamentally solve the problem of short life of non-precious metal catalysts. The reason is that it is difficult to reduce the reaction temperature of dry reforming over 600°C to a lower level.

[0007] Using clean energy to generate electrons, such as existing semiconductor photogenerated electrons and electrode electrolysis, is also an effective low-temperature DRM strategy. However, the kinetics of the initial activation of CO2 driven by photoelectricity is relatively slow, which greatly limits its energy conversion efficiency and product synthesis rate. The reason is that the carbon atoms in the CO2 molecule use sp hybrid orbitals to bond with oxygen atoms, which has a very negative redox potential.

[0008] In recent years, arc plasma technology has gradually shown its special utility in various gas-phase chemical reactions. Plasma reforming, which can operate in a wide temperature range (from room temperature to over 1000°C), is one of its applications in DRM. Both non-thermal plasma and thermal plasma have been proven to effectively convert CO2 and CH4 into syngas. However, it also has the problems of low energy utilization efficiency, low syngas selectivity, and low syngas production efficiency.

[0009] Plasma catalysis has been shown to have a synergistic effect to improve the efficiency of syngas production, as catalysis and plasma can enhance each other's performance. A review of different catalytic systems for dry reforming ofmethane: Conventional catalysis-alone and plasma-catalytic system (DOI: 10.1016 / j.jcou.2021.101462) studied the mechanism of plasma-catalyst interaction, compared the advantages and disadvantages of conventional single-catalytic systems and plasma-catalytic systems, described the mechanism of catalytic promotion, elucidated the synergistic effect between catalyst and plasma, and proposed possible methods to optimize DRM.

[0010] Characteristics of the plasma produced by the energetic electron beam in sub-atmospheric pressure (DOI: 10.1063 / 5.0038571) studied the characteristics of plasma produced by high-energy electron beams. The attenuation amplitude of the penetration distance of the electron beam from the electron beam outlet, the plasma distribution envelope, and the influence of gas pressure on the penetration distance of the electron beam and the generated plasma were revealed. The industrialization of atmospheric pressure plasma technology has been studied to a high degree in the prior art: US4647818A discloses a plasma electron beam generator for manufacturing multi-purpose electron beams. The prior art CN101355005A proposes an electron beam generator for generating planar plasma.

[0011] There have been some studies and reports on the use of high-energy particles in certain treatments of organic materials. For example, CN101194684A uses high-energy electron beam irradiation to crack and reduce the polymerization degree of short cotton linter cellulose to prepare dietary fiber with different cellulose components. CN2616279Y designs a device for desulfurization and denitrification of flue gas using high-energy electron beams. CN1544129A proposes a method for purifying flue gas using electron beams; CN101348731A uses high-energy electron beams generated by high-energy electron accelerators to molecularly crack petroleum products to generate low-level olefins; CN113233539A uses electron beam irradiation to assist in the catalytic degradation of organic pollutants; CN103482718A uses electron irradiation to degrade dienestilbestrol in water. However, there has been no report on the use of high-energy electron irradiation in DRM dry reforming production. Summary of the invention

[0012] The present application is made to solve the above-mentioned problems, and aims to provide a method for preparing synthesis gas by dry reforming of carbon dioxide / methane, using a high-energy electron beam as the ionization source of the reaction system, and realizing the dry reforming of carbon dioxide and methane at a relatively low temperature through a catalytic system of a high-energy electron beam and a catalyst, which solves the carbon deposition problem of the dry reforming reaction to a certain extent, prolongs the service life of the catalyst, and provides a guarantee for stable production.

[0013] The present application provides a method for preparing synthesis gas by dry reforming of carbon dioxide / methane. The method comprises using a catalytic system, wherein the catalytic system comprises a high-energy electron beam and a catalyst.

[0014] In some embodiments of the present application, methane and carbon dioxide are introduced into the catalyst and reacted under high-energy electron beam irradiation at a reaction temperature of 300°C to 500°C.

[0015] In some embodiments of the present application, the high-energy electron beam is emitted by one or more electron beam emitters, the catalyst is disposed on a catalyst bed, and each of the electron beam emitters irradiates the high-energy electron beam to the catalyst bed in a scanning manner through titanium glass.

[0016] In some embodiments of the present application, the number of the electron beam emitters is 2, and the electron beam emitters irradiate the catalyst bed in a scanning manner with a high-energy electron beam from two opposite directions through titanium glass.

[0017] In some embodiments of the present application, the acceleration voltage of the electron beam emitter is 80-180KV.

[0018] In some embodiments of the present application, the electron amount of the electron beam emitter is 20-30 mA.

[0019] In some embodiments of the present application, the scanning rate of the electron beam in the electron beam emitter is 100-200 mm / s, with one cycle every 20-40 seconds.

[0020] In some embodiments of the present application, the catalyst includes an active component and a catalyst carrier, and the active component is selected from nickel or a combination of nickel and other metals.

[0021] In some embodiments of the present application, the other metal is selected from one or more of palladium, platinum, ruthenium, rhodium, gold, copper, and molybdenum.

[0022] In some embodiments of the present application, in the catalyst, the mass percentage of nickel is 12% to 15%, the mass percentage of other metals is 0.2% to 1.5%; and the remainder is the catalyst carrier.

[0023] In some embodiments of the present application, the catalyst carrier is selected from one or more of magnesium oxide, aluminum oxide, and silicon oxide.

[0024] In some embodiments of the present application, the method for preparing the catalyst comprises the following steps:

[0025] a) dissolving a precursor solution of an active component in a dilute acid to obtain a dilute solution;

[0026] b) Add the dilute solution into the catalyst carrier, stir and disperse it, spin dry the solvent, take out the catalyst, dry it and then calcine it to obtain the catalyst.

[0027] In some embodiments of the present application, the catalyst is diluted with a diluent. The diluent is selected from one or more of magnesium oxide, aluminum oxide, and silicon oxide. The mesh size of the diluent is 40-60 mesh.

[0028] In some embodiments of the present application, hydrogen is used for activation before the introduction of methane and carbon dioxide. The hydrogen activation temperature is not higher than the reaction temperature.

[0029] In some embodiments of the present application, the volume ratio of methane to carbon dioxide is 1:1.

[0030] In some embodiments of the present application, the intake rate of methane and carbon dioxide is 8~12mL / min.

[0031] This application has the following beneficial effects:

[0032] The catalyst system used in the present application includes a high-energy electron beam and a catalyst, wherein the catalyst includes, for example, nickel and a combination catalyst thereof with other metals (such as palladium, platinum, ruthenium, rhodium, gold, copper, molybdenum, etc.). The present application compares the effects of the presence or absence of electron irradiation on various catalytic systems. At the same time, the effects of irradiation of different intensities and intake of different components on the final yield are compared to obtain the optimal reaction conditions. The catalytic system in which the catalyst and the high-energy electron beam are coordinated realizes the dry reforming reaction of CH4 and CO2 at a relatively low temperature, and has a high catalytic efficiency. In particular, the catalytic system in which the nickel / Al2O3 catalyst and the high-energy electron beam are coordinated has the advantages of both catalytic efficiency and cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 Shown is a schematic diagram of an experimental device used in the method for preparing synthesis gas by dry reforming of carbon dioxide / methane in the present application. DETAILED DESCRIPTION

[0034] Hereinafter, an embodiment of a method for preparing synthesis gas by dry reforming of carbon dioxide / methane is described in detail.

[0035] The present application provides a method for methane dry reforming reaction, which reduces the reaction temperature by using high-energy electron beam irradiation, improves the efficiency of dry reforming, and reduces the generation of catalyst carbon deposition.

[0036] High-energy electron beams break chemical bonds, causing CH4 and CO2 to be in an excited state at a higher energy level, which can significantly reduce the heating temperature required to reach the reaction energy barrier.

[0037] The main reaction of dry reforming reaction:

[0038] CO2+CH4=2CO+2H2, △H (298K)=247kJ / mol;

[0039] Side reaction 1 is the CO disproportionation reaction, which occurs at a temperature of 550-700°C:

[0040] 2CO=C+CO2, △H (298K) =-171kJ / mol;

[0041] The temperature of the side reaction 2, the CH4 cracking reaction, is 900°C:

[0042] CH4=C+2H2, △H (298K)=75kJ / mol.

[0043] The two side reactions are the main causes of carbon deposition and catalyst deactivation. Therefore, finding a suitable catalytic system to reduce the reaction temperature has become the main means to solve the carbon deposition problem. CO2 reduction is essentially an energy-consuming electron capture process. For this reason, many studies have proposed strategies such as semiconductor photogenerated electrons and electrode electrolysis. However, the carbon atoms in the CO2 molecule use sp hybrid orbitals to bond with oxygen atoms to form free radical intermediates (CO2•). The key step of electron transfer has a very negative redox potential (-1.9V relative to the standard hydrogen electrode), which leads to extremely slow kinetics of photoelectrically driven CO2 initial activation, greatly limiting its energy conversion efficiency and product synthesis rate.

[0044] In recent years, arc plasma technology has gradually shown its special utility in various gas-phase chemical reactions. Plasma reforming, which can operate in a wide temperature range (from room temperature to over 1000°C), is one of its applications in DRM. Both non-thermal plasma and thermal plasma have been proven to effectively convert CO2 and CH4 into syngas. However, its energy utilization efficiency is still low, and the syngas selectivity is low, resulting in low syngas production efficiency.

[0045] Therefore, the combination of catalysis and plasma can be an alternative to integrate the advantages of catalysis and plasma: plasma catalysis has been shown to have a synergistic effect to improve the efficiency of syngas production, and catalysis and plasma can enhance the performance of each other. Plasma can improve catalytic activity and durability, while the presence of catalysts increases the electron density in plasma and improves energy utilization efficiency. Catalyst characterization shows that plasma introduces charge defects on the catalyst surface, making it more electronegative. At the same time, the crystal structure of the catalyst is not affected by contact with plasma, and the synergistic effect between plasma and Ni catalyst can significantly reduce the apparent activation energy by about 50%, which is why the synergistic catalytic system can maintain high catalytic performance at low temperatures.

[0046] When a high-energy electron beam is injected into a background neutral gas, about 30% to 50% of the energy is used to ionize and produce plasma, which is a very effective ionization source. During the electron impact ionization process, the electron beam energy gradually loses its energy through the impact ionization and excitation process. When the energy is reduced to a certain threshold, it will lose its ionization and excitation functions and become a hot electron that is not significantly different from the plasma electron. The range of an electron beam with an energy of 140KeV in air at an atmospheric pressure is about 46cm, at which time the electron beam flux is reduced to 1% of the initial flux. Within this range, the energy of the electron beam gradually decreases, and the rate of energy reduction increases with the increase in distance. Finally, the electron beam is converted into hot electrons. Relative to the transmission path, the thermalization area of ​​the electron beam is narrow, about 5cm. In the thermalization area of ​​the electron beam, the ionization rate of the electron beam reaches a peak, which is consistent with the distribution peak of the electron impact ionization and excitation cross section in the low energy region (about 100eV).

[0047] Studies on the electron irradiation decomposition of methane have shown that the gas pressure has a significant effect on the penetration distance of the electron beam and the generated plasma. An increase in gas pressure will reduce the penetration distance of the electron beam and plasma because higher pressure will increase the probability of collisions between electrons and gas molecules, and the energy transfer becomes stronger.

[0048] The catalyst system used in this application includes nickel and its combination catalyst with other metals (such as palladium, platinum, ruthenium, rhodium, gold, copper, molybdenum, etc.), and the influence of the presence or absence of electron irradiation on each catalytic system is compared. At the same time, the influence of irradiation of different intensities and intake of different components on the final yield is also compared to obtain the optimal reaction conditions. Among them, the catalytic system of nickel / Al2O3 catalyst and high-energy electron beam synergistically realizes the dry reforming reaction of CH4 and CO2 at a lower temperature, and has the advantages of catalytic efficiency and cost. On this basis, this application is completed.

[0049] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0050] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0051] [Method for preparing synthesis gas by dry reforming of carbon dioxide / methane]

[0052] The present application provides a method for preparing synthesis gas by dry reforming of carbon dioxide / methane. The method comprises using a catalytic system, wherein the catalytic system comprises a high-energy electron beam and a catalyst.

[0053] In the method for preparing synthesis gas by dry reforming of carbon dioxide / methane provided in the present application, methane and carbon dioxide are introduced into the catalyst and reacted under high-energy electron beam irradiation at a relatively low reaction temperature. For example, the reaction temperature in the present application can be 300°C to 500°C. Further optionally, the reaction temperature can be, for example, 300°C to 400°C, 400°C to 500°C, 300°C to 330°C, 330°C to 500°C, 300°C to 350°C, 350°C to 500°C, 300°C to 360°C, 360°C to 500°C, 300°C to 370°C, 370°C to 500°C, 300°C to 380°C, 380°C to 500°C, 300°C to 420°C, 420°C to 500°C, 300°C to 430°C, 430°C to 500°C, 300°C to 460°C or 460°C to 500°C, etc.

[0054] In the method for preparing synthesis gas by dry reforming of carbon dioxide / methane provided in the present application, the high-energy electron beam is emitted by one or more electron beam emitters, the catalyst is arranged on a catalyst bed, and each of the electron beam emitters respectively irradiates the high-energy electron beam to the catalyst bed by scanning through titanium glass. The catalyst can be placed on the catalyst bed. Scanning irradiation prevents local overheating.

[0055] In some preferred embodiments of the present application, the number of the electron beam emitters is 2, and the electron beam emitters irradiate the catalyst bed with a high-energy electron beam in a scanning manner from two opposite directions through titanium glass. By irradiating from two opposite directions, not only a uniform system can be obtained, but also because the penetration depth of the high-energy electron beam is limited, irradiating from different directions can increase the penetration depth. Specifically, the following method can be used: Figure 1 The experimental equipment is shown.

[0056] The experimental equipment includes a reaction device and an electron emission device, wherein a catalyst bed is provided in the reaction device, and the electron emission device includes two electron emitters. The top and bottom of the reaction device are respectively provided with openings, and the openings are respectively provided with reaction device windows, and the reaction device windows are titanium glass. The electron reflector is suitable for irradiating a high-energy electron beam to the catalyst bed from two opposite directions through the titanium glass. The electron beam is provided by an emitter, and the emitter is composed of an electron source, a confinement device and an accelerator.

[0057] In the method for preparing synthesis gas by dry reforming of carbon dioxide / methane provided in the present application, the effective dose of the high-energy electron beam relative to carbon dioxide / methane gas is 20-500kGy. Optionally, the effective dose of the high-energy electron beam relative to carbon dioxide / methane gas is 20-50kGy, 50-500kGy, 50-250 kGy or 250-500kGy. The effective dose can be calculated by the following formula: effective dose = (1-loss rate) * electron beam power w / (methane flow rate g / s + carbon dioxide flow rate g / s) * 100%; wherein the loss rate is the ratio of the energy lost during the electron beam from emission to action on carbon dioxide / methane gas to the total energy of the electron beam. The loss rate is 80%~98%, which can be selected as 80%~95%, 80%~90%, 90%~95% or 95%~98%. The gas inlet rates of methane and carbon dioxide are 8~12mL / min, respectively, and can be selected as 8~10mL / min or 10~12mL / min. The electron beam power is equal to the acceleration voltage*electron quantity.

[0058] In the method for preparing synthesis gas by dry reforming of carbon dioxide / methane provided in the present application, the accelerating voltage of the electron beam emitter is 80-180KV. Optionally, the accelerating voltage of the electron beam emitter is 80-150KV, 150-180KV, 80-100KV, 100-120KV, 120-150KV, 150-160KV, 160-200KV, 150-180KV, 180-200KV or 150-180KV, etc.

[0059] In the method for preparing synthesis gas by dry reforming of carbon dioxide / methane provided in the present application, the electron amount of the electron beam emitter is 20-30 mA. Optionally, the electron amount of the electron beam emitter can be, for example, 20-25 mA or 25-30 mA.

[0060] In the method for preparing synthesis gas by dry reforming of carbon dioxide / methane provided in the present application, the scanning rate of the electron beam in the electron beam emitter is 100-200 mm / s, and one cycle is performed every 20-40 seconds. Alternatively, the scanning rate can be, for example, 100-150 mm / s, 150-200 mm / s, and one cycle is performed every 20-30 seconds or 30-40 seconds.

[0061] In the method for preparing synthesis gas by dry reforming of carbon dioxide / methane provided in the present application, the catalyst includes an active component and a catalyst carrier.

[0062] The active component is selected from nickel, or a combination of nickel and other metals. Among them, other metals can be selected from one or more of palladium, platinum, ruthenium, rhodium, gold, copper, and molybdenum. Alternatively, other metals can be selected from one of palladium, platinum, ruthenium, rhodium, gold, copper, and molybdenum.

[0063] The catalyst carrier is selected from one or more of magnesium oxide, aluminum oxide, and silicon oxide. Optionally, the catalyst carrier is selected from aluminum oxide, or a combination of magnesium oxide and aluminum oxide.

[0064] In the catalyst, the mass percentage of nickel is 12% to 15%, the mass percentage of other metals is 0.2% to 1.5%; the remainder is the catalyst carrier.

[0065] In the method for preparing synthesis gas by dry reforming of carbon dioxide / methane provided in the present application, the catalyst is diluted with a diluent. Specifically: after the catalyst is diluted with a diluent, methane and carbon dioxide are introduced into the catalyst to react under high-energy electron beam irradiation.

[0066] Optionally, the diluent is selected from one or more of magnesium oxide, aluminum oxide, and silicon oxide. The mesh size of the diluent may be, for example, 40-60 meshes.

[0067] In some embodiments of the present application, the catalyst can be prepared by the following method, which comprises the following steps:

[0068] a) dissolving a precursor solution of an active component in a dilute acid to obtain a dilute solution;

[0069] b) Add the dilute solution into the catalyst carrier, stir and disperse it, spin dry the solvent, take out the catalyst, dry it and then calcine it to obtain the catalyst.

[0070] In step a) of the present application, the dilute acid may be selected from dilute nitric acid, for example.

[0071] In step a) of the present application, the precursor solution of the active component may be, for example, a nitrate solution or an acetate solution of the active component. For example, when the active component is nickel, the precursor solution of the active component is nickel nitrate hexahydrate, or a combination of nickel nitrate hexahydrate and other solutions. Other solutions may be, for example, copper nitrate trihydrate, palladium nitrate dihydrate, potassium chloroaurate, ruthenium trichloride monohydrate, ammonium molybdate tetrahydrate, rhodium sulfate, and the like.

[0072] In step a) of the present application, the dilute acid is obtained by adding water to the acid to adjust the pH, wherein the pH is 2-3.

[0073] In step b) of the present application, the dispersion is ultrasonic-assisted dispersion.

[0074] In step b) of the present application, the drying temperature is 100-140°C; it can be optionally 100-120°C or 120-140°C, etc.

[0075] In step b) of the present application, the drying time is 6-10 hours, which may be 6-8 hours or 8-10 hours, etc.

[0076] In step b) of the present application, the calcination temperature is 550-650°C; it can be optionally 550-600°C or 600-650°C, etc.

[0077] In step b) of the present application, the calcination time is 2-4 hours, which can be 2-3 hours or 3-4 hours.

[0078] The catalyst obtained in step b) of the present application is stored in a desiccator for future use.

[0079] In the method for preparing synthesis gas by dry reforming of carbon dioxide / methane provided in the present application, hydrogen is used for activation before introducing methane and carbon dioxide. Specifically: after the catalyst is diluted with a diluent, it is loaded into a catalyst bed, activated with hydrogen, and then the intake air is switched to methane and carbon dioxide. Optionally, the hydrogen activation temperature is not higher than the reaction temperature. For example, when the reaction temperature is 300°C-500°C, the hydrogen activation temperature can be 300°C. The volume ratio of methane and carbon dioxide is 1:1. The intake rate of methane and carbon dioxide is 8~12mL / min, for example, it can also be 8~10mL / min or 10~12mL / min, etc.

[0080] The beneficial effects of the present application are further illustrated below in conjunction with embodiments.

[0081] In order to make the invention purpose, technical scheme and beneficial technical effect of the present application clearer, the present application is further described in detail below in conjunction with the examples. However, it should be understood that the examples of the present application are only for explaining the present application, not for limiting the present application, and the examples of the present application are not limited to the examples given in the specification. The specific experimental conditions or operating conditions not specified in the examples are made under conventional conditions, or are made under the conditions recommended by the material supplier.

[0082] In addition, it should be understood that one or more method steps mentioned in this application do not exclude the existence of other method steps before or after the combination step or the insertion of other method steps between these explicitly mentioned steps, unless otherwise specified; it should also be understood that the combination connection relationship between one or more devices / apparatuses mentioned in this application does not exclude the existence of other devices / apparatuses before or after the combination device / apparatus or the insertion of other devices / apparatuses between these two explicitly mentioned devices / apparatuses, unless otherwise specified. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or the scope of implementation of this application. Changes or adjustments in their relative relationships shall also be regarded as the scope of implementation of this application without substantial changes in the technical content.

[0083] In the following examples, the reagents, materials and instruments used are all commercially available unless otherwise specified.

[0084] Unless otherwise specified, the purity of each product in each embodiment of the present application exceeds 98%.

[0085] The catalysts used in the following examples and comparative examples are numbered as follows:

[0086] Catalyst a: Ni / Al2O3, containing 15% Ni;

[0087] Catalyst b: Ni / MgO-Al2O3, containing 15% Ni, MgO:Al2O3 is 1:1;

[0088] Catalyst c: Co-Ni / Al2O3, containing Ni 12%, Co 1.5%;

[0089] Catalyst d: Cu-Ni / Al2O3, containing 12% Ni and 3% Cu;

[0090] Catalyst e: Pt-Ni / Al2O3, containing Ni 12%, Pt 0.2%;

[0091] Catalyst f: Au-Ni / Al2O3, containing 12% Ni and 0.5% Au;

[0092] Catalyst g: Ru-Ni / Al2O3, containing 12% Ni and 0.2% Ru;

[0093] Catalyst h: Mo-Ni Al2O3, containing Ni 12%, Mo 0.5%;

[0094] Catalyst i: Rh-Ni / Al2O3, containing Ni 12%, Rh 0.2%.

[0095] Embodiments 1a-1k are to explore the temperature 1 at which the catalytic system is significantly deactivated when the electron beam emitter is turned on, and determine the appropriate reaction temperature of the catalytic system to meet a raw gas conversion rate of more than 90%.

[0096] Example 1a:

[0097] Catalyst treatment: Weigh 6g of deionized water and add 0.1mL of nitric acid to adjust the pH to 2-3, then weigh the precursor solution of the catalyst active component, nickel nitrate hexahydrate, and dissolve it in dilute nitric acid; weigh 10g of catalyst carrier Al2O3, add the dilute solution to the carrier Al2O3, stir evenly, and then disperse it with ultrasonic assistance for 15 minutes, then transfer it to a rotary evaporator, spin dry the solvent, take out the catalyst and put it in a 120℃ oven to dry for 8h, then heat it to 600℃ and calcine for 3h, and the obtained catalyst a is stored in a desiccator for later use.

[0098] Weigh 0.5g of the treated catalyst a and dilute it to 2mL with 40-60 mesh Al2O3, load it into a fixed bed reactor, activate it with hydrogen at 300°C for 30min, then switch the inlet gas to CH4 and CO2 with an inlet gas composition of 1:1. The flow rates of CH4 and CO2 are both 10mL / min. After maintaining the temperature of the reaction device stable at 300°C, turn on the electron beam emitter for scanning irradiation to prevent local overheating. Set the acceleration voltage to 150KV, the current to 20mA, the scanning rate to 150mm / s, and one cycle every 30s (specifically, the device window is titanium glass, the energy loss of the electron beam through the titanium glass is 95%, and the electron beam bombardment point is scanned on the titanium glass window at a rate of 150mm / s, with one cycle every 30s). The reactor was heated at a constant rate from 300°C to 900°C, and the gas phase composition at the outlet was monitored online by gas chromatography. Analysis showed that the temperature 1 at which the catalytic system was significantly deactivated was 820°C. When the carbon dioxide conversion rate of the raw gas was 91.1% and the methane conversion rate was 95.2%, the suitable reaction temperature of the catalytic system was 350°C.

[0099] Examples 1b to 1i use catalysts b to catalysts i to replace catalyst a in Example 1a. Other conditions are the same as those in Example 1a. The specific amount of the precursor solution of each active component in the catalyst treatment is shown in Table 1:

[0100] Table 1

[0101]

[0102] Comparative Examples 1a-1i are obtained when the electron beam emitter is turned off, and the temperature at which the catalyst system undergoes obvious deactivation in the absence of an electron beam is 2.

[0103] Comparative Example 1a:

[0104] The electron beam emitter was turned off, and other conditions were the same as those in Example 1a. The activation and reaction heating process were repeated, and the gas phase composition at the outlet was recorded. Analysis showed that the temperature 2 at which the catalytic system was significantly deactivated in the absence of an electron beam was 720°C. When the carbon dioxide conversion rate of the raw gas was 91.3% and the methane conversion rate was 93.6%, the suitable reaction temperature of the catalytic system was 740°C.

[0105] Comparative Examples 1b to 1i respectively use catalysts b to catalysts i to replace catalyst a in Comparative Example 1a. Other conditions are the same as those in Comparative Example 1a.

[0106] The deactivation temperatures of Examples 1a-1i and Comparative Examples 1a-1i are shown in Table 2.

[0107] Table 2

[0108]

[0109] Embodiment 2a~2i:

[0110] With the electron beam emitter turned on, the reaction was continued for 100 hours at the optimal reaction temperature of catalyst a-catalyst i, and the conversion rate of the catalytic system after long-term operation was recorded.

[0111] Comparative Example 2:

[0112] Using catalyst a, with the electron beam emitter turned off, the reaction temperature was maintained at 740°C for 100 hours, and the changes in activity of different catalytic systems after long-term operation were compared.

[0113] Comparative Example 3

[0114] Using catalyst a, with the electron beam emitter turned off, the reaction temperature was maintained at 670°C for 100 hours, and the changes in activity of different catalytic systems after long-term operation were compared.

[0115] The conversion rates of Examples 2a to 2i and Comparative Examples 2 and 3 are shown in Table 3.

[0116] Table 3

[0117]

[0118] Combined with Table 2 and Table 3, the above experiments show that the catalytic system of high-energy electron beam and catalyst can avoid catalyst deactivation to a certain extent compared with the use of a single catalyst. More importantly, it can effectively reduce the reaction temperature of dry reforming, so that the reaction avoids the carbon deposition problem caused by side reactions. The reaction is carried out at a temperature lower than the deactivation temperature of the catalyst. Therefore, the coordinated catalytic system can maintain the stability of catalytic efficiency during continuous operation.

[0119] Example 3

[0120] Using Ni / Al2O3 catalyst a, based on the experimental scheme in Example 2a, the current of the electron beam emitter was adjusted to the range of 2-30 mA, and the efficiency changes of the catalytic system under different currents were compared.

[0121] Example 4

[0122] Using Ni / Al2O3 catalyst, based on the experimental scheme in Example 2, the acceleration voltage of the electron beam emitter was adjusted to the range of 80-180 KV, and the effects of different electron beam energies on the efficiency of the catalytic system were compared.

[0123] The test results of Examples 3 and 4 are shown in Table 4.

[0124] Table 4

[0125]

[0126] The above experiments show that changes in electron beam data will directly affect the efficiency of the synergistic catalytic system. The most relevant factors for catalytic efficiency are electron beam energy and temperature. When the electron beam cannot provide enough energy, the efficiency of synergistic catalysis will be greatly reduced (to achieve the same catalytic efficiency, the reaction temperature needs to be increased accordingly).

[0127] The above implementations are preferred cases of the present application and are not intended to limit the protection scope of the present application. However, the present application is not limited to the specific details of the above implementations. Within the technical concept of the present application, the technical solution of the present application can be subjected to a variety of simple modifications, and these simple modifications all belong to the protection scope of the present application.

[0128] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, this application will not further describe various possible combinations.

Claims

1. A method for preparing synthesis gas by dry reforming of carbon dioxide / methane, It is characterized in that The method comprises using a catalytic system comprising a high energy electron beam and a catalyst, The high-energy electron beam is emitted by one or more electron beam emitters, the catalyst is arranged on the catalyst bed, each electron beam emitter respectively irradiates the high-energy electron beam to the catalyst bed through titanium glass in a scanning manner, the acceleration voltage of the electron beam emitter is 80-180KV, and the electron quantity of the electron beam emitter is 20-30mA; The catalyst comprises an active component and a catalyst carrier, wherein the active component is selected from nickel or a combination of nickel and other metals; Methane and carbon dioxide are introduced into the catalyst and reacted under high-energy electron beam irradiation at a reaction temperature of 300° C. to 500° C.

2. The method for preparing synthesis gas by dry reforming of carbon dioxide / methane according to claim 1, It is characterized in that The number of the electron beam emitters is 2, and the electron beam emitters irradiate the catalyst bed in a scanning manner with high-energy electron beams from two opposite directions through titanium glass.

3. The method for preparing synthesis gas by dry reforming of carbon dioxide / methane according to claim 1, It is characterized in that The scanning rate of the electron beam in the electron beam emitter is 100-200 mm / s, with one cycle every 20-40 seconds.

4. The method for preparing synthesis gas by dry reforming of carbon dioxide / methane according to claim 1, It is characterized in that Also includes any one or more of the following features: B1) the other metal is selected from one or more of palladium, platinum, ruthenium, rhodium, gold, copper and molybdenum; B2) In the catalyst, the mass percentage of nickel is 12% to 15%, the mass percentage of other metals is 0.2% to 1.5%; the remainder is the catalyst carrier; B3) The catalyst carrier is selected from one or more of magnesium oxide, aluminum oxide and silicon oxide.

5. The method for preparing synthesis gas by dry reforming of carbon dioxide / methane according to claim 1, It is characterized in that The preparation method of the catalyst comprises the following steps: a) dissolving a precursor solution of an active component in a dilute acid to obtain a dilute solution; b) Add the dilute solution into the catalyst carrier, stir and disperse it, spin dry the solvent, take out the catalyst, dry it and then calcine it to obtain the catalyst.

6. The method for preparing synthesis gas by dry reforming of carbon dioxide / methane according to claim 1, It is characterized in that Also includes any one or more of the following features: C1) the catalyst is diluted with a diluent; C2) Use hydrogen to activate before introducing methane and carbon dioxide; C3) the volume ratio of methane to carbon dioxide is 1:1; C4) The intake rate of methane and carbon dioxide is 8-12 mL / min.

7. The method for preparing synthesis gas by dry reforming of carbon dioxide / methane according to claim 6, It is characterized in that Also includes any one or more of the following features: C11) the diluent is selected from one or more of magnesium oxide, aluminum oxide and silicon oxide; C12) The mesh number of the diluent is 40-60 mesh; C21) The hydrogen activation temperature is not higher than the reaction temperature.

Citation Information

Patent Citations

  • Process for preparing soluble edible fibres

    CN101194684A

  • Method for producing light alkene by irradiating and cracking oil with high-energy electron beam

    CN101348731A

  • Electron beam generating apparatus for generating flat-plate shape plasma

    CN101355005A

  • Method for degrading dienestrol in water body through electron beam irradiation

    CN103482718A

  • Dry reforming of methane, core-shell catalysts containing nickel and cerium for dry reforming of methane and their preparation

    CN107921427B