A carbon nanotube / silicon carbide composite fiber and preparation method thereof
By depositing a silicon carbide shell layer on the surface of carbon nanotube fibers and performing specific treatments, the problem of insufficient performance of existing carbon nanotube/silicon carbide composite fibers is solved, achieving high thermal conductivity, high electrical conductivity and excellent mechanical properties, which is suitable for micro-electronics. environment.
Patent Information
- Application Number
- CN202410968731.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-19
AI Technical Summary
Existing carbon nanotube/silicon carbide composite fibers have deficiencies in mechanical, electrical and thermal properties, cannot provide excellent performance at the same time, and have poor durability in micro-electronic environments.
By depositing a silicon carbide shell layer on the surface of carbon nanotube fibers, twisting, homogenizing and stretching treatments are used, combined with chemical vapor deposition technology, to prepare carbon nanotube/silicon carbide composite fibers to ensure uniform deposition and integration of silicon carbide. Tight binding of carbon nanotubes.
The carbon nanotube/silicon carbide composite fiber has high thermal conductivity, high electrical conductivity and excellent mechanical properties, is suitable for complex micro-electronic environments, and improves the corrosion resistance of the material.
Smart Images

Figure CN118498073B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of silicon carbide / carbon nanofiber materials, and in particular to a carbon nanotube / silicon carbide composite fiber and a preparation method thereof. Background Art
[0002] Carbon nanotubes have high thermal conductivity, high electrical conductivity and excellent mechanical properties under microscopic conditions, but there are still many problems in fully releasing their microscopic properties in macroscopic materials. Silicon carbide has excellent properties such as high strength and good corrosion resistance, but its electrical and thermal conductivity is poor.
[0003] Currently, there are plans to coat carbon nanotube fibers with materials containing carbon and silicon by sintering, which are mainly used in the field of thermal insulation of certain special equipment such as aluminum electrolytic cells and microwave sintering furnaces, or to coat carbon nanotube fibers with silicon carbide by coating. The resulting coated nanotubes can be used in fields such as bio-equipment and thermal management. However, the mechanical properties of the silicon carbide / carbon nanotube fibers obtained by the sintering method are poor and their high-temperature performance is limited. The silicon carbide / carbon nanotube fibers obtained by the coating method have poor bonding strength and poor electrical conductivity. In addition, the thickness of the carbon nanotube fibers is much smaller than that of the silicon carbide. The silicon carbide / carbon nanotube fibers prepared in this way have poor thermal conductivity and mechanical properties. In addition, the uniformity of the silicon carbide deposited on the carbon nanotubes is not good enough, and the middle section of the composite fiber is prone to expansion. As a result, the resulting composite fiber material cannot simultaneously possess good mechanical, electrical and thermal properties, making it unsuitable for various complex microelectronic environments. Even if it can be used in microelectronic environments, its durability is still poor.
[0004] Therefore, there is an urgent need to provide a composite material that can simultaneously possess the excellent properties of carbon nanotubes and silicon carbide. Summary of the Invention
[0005] The present invention aims to overcome the aforementioned problems of the prior art and provides a carbon nanotube / silicon carbide composite fiber and a method for preparing the same. The present invention deposits a silicon carbide shell on the surface of the carbon nanotube fiber to produce the carbon nanotube / silicon carbide composite fiber, thereby imparting excellent mechanical, electrical, and thermal properties to the carbon nanotube / silicon carbide composite fiber.
[0006] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a method for preparing carbon nanotube / silicon carbide composite fibers, which includes depositing a silicon carbide shell layer on the surface of a carbon nanotube fiber to obtain a carbon nanotube / silicon carbide composite fiber; the preparation method of the carbon nanotube fiber includes: (1) twisting a carbon nanotube fiber preform to obtain a twisted carbon nanotube fiber; (2) homogenizing the twisted carbon nanotube fiber to obtain a homogenized carbon nanotube fiber; the homogenizing method is to perform a through-hole treatment on the carbon nanotube fiber; (3) stretching the homogenized carbon nanotube fiber in the length direction The carbon nanotube fibers are obtained by twisting for 60s-240s and twisting at a speed of 120r / min-350r / min. The stretching treatment conditions include a stretching force of 5N-10N. The ratio of the radius of the carbon nanotube fiber to the thickness of the silicon carbide shell is 2-30:1, the thickness of the silicon carbide shell is 1µm-18µm, the radius of the carbon nanotube fiber is 15µm-80µm, and the carbon nanotube / silicon carbide composite fiber contains 50wt%-80wt% of the carbon nanotube fiber and 20wt%-50wt% of the silicon carbide.
[0007] Preferably, the direction of the gas flow during the chemical vapor deposition process is perpendicular to the placement direction of the carbon nanotube fibers.
[0008] Preferably, the method further comprises heat treating the material after depositing the silicon carbide shell layer; the heat treatment conditions include a temperature of 1350° C.-1800° C. and a time of 0.5 h-5 h.
[0009] Preferably, the ratio of the radius of the carbon nanotube fiber to the thickness of the silicon carbide shell is 3-20:1.
[0010] Preferably, the thickness of the silicon carbide shell layer is 3 μm-12 μm.
[0011] Preferably, the radius of the carbon nanotube fiber is 30 μm-60 μm.
[0012] Preferably, the length of the carbon nanotube fiber is 50 cm-80 cm.
[0013] A second aspect of the present invention provides a carbon nanotube / silicon carbide composite fiber prepared by the method described in the first aspect.
[0014] Preferably, the tensile strength of the carbon nanotube / silicon carbide composite fiber is 1500MPa-3000MPa, the electrical conductivity of the carbon nanotube / silicon carbide composite fiber is 3500S / cm-6500S / cm, and the thermal conductivity of the carbon nanotube / silicon carbide composite fiber is 450w / mK-1000w / mK.
[0015] During the experiment, it was found that coating the carbon nanotube fibers with a shell layer is beneficial to increasing the mechanical properties of the carbon nanotube fibers, and can also prevent the carbon nanotube fibers from direct contact with the external environment, preventing oxidation from destroying their excellent electrical and thermal conductivity.
[0016] During the experiment, it was found that uniformly coating the carbon nanotube fibers with a thin silicon carbide shell layer can combine the excellent corrosion resistance and mechanical properties of silicon carbide with the high electrical and thermal conductivity of carbon nanotube fibers, resulting in a new type of high thermal conductivity and high electrical conductivity carbon nanotube fiber material.
[0017] The present invention adopts the above technical solution to achieve the following beneficial effects:
[0018] (1) The carbon nanotube / silicon carbide composite fiber provided by the present invention has excellent mechanical, electrical and thermal properties, strong corrosion resistance, high thermal conductivity and high electrical conductivity.
[0019] (2) The carbon nanotube / silicon carbide composite fiber provided by the present invention can be used for the preparation of microelectronic devices and can be used in various complex electronic environments.
[0020] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Herein, unless otherwise specified, data ranges include endpoints. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 Shown is the SEM image of the carbon nanotube / silicon carbide composite fiber of Example 1.
[0022] Figure 2 Shown is a SEM image of the cross section of the carbon nanotube / silicon carbide composite fiber of Example 1. DETAILED DESCRIPTION
[0023] The following is a detailed description of the specific embodiments of the present invention. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention and are not intended to limit the present invention.
[0024] Unless otherwise defined, all scientific and technical terms used in the present invention have the same meanings as commonly understood by one of ordinary skill in the art to which the present invention relates.
[0025] The first aspect of the present invention provides a method for preparing carbon nanotube / silicon carbide composite fibers, which comprises depositing a silicon carbide shell layer on the surface of a carbon nanotube fiber to obtain a carbon nanotube / silicon carbide composite fiber; the method for preparing the carbon nanotube fiber comprises: (1) twisting a carbon nanotube fiber preform to obtain a twisted carbon nanotube fiber; (2) homogenizing the twisted carbon nanotube fiber to obtain a homogenized carbon nanotube fiber; the homogenizing treatment is performed by performing a through-hole treatment on the carbon nanotube fiber; (3) stretching the homogenized carbon nanotube fiber in the length direction to obtain Carbon nanotube fiber; the twisting conditions include: a time of 60s-240s, a twisting speed of 120r / min-350r / min; the stretching treatment conditions include: a stretching force of 5N-10N; the ratio of the radius of the carbon nanotube fiber to the thickness of the silicon carbide shell is 2-30:1, the thickness of the silicon carbide shell is 1µm-18µm, the radius of the carbon nanotube fiber is 15µm-80µm, and in the carbon nanotube / silicon carbide composite fiber, the content of the carbon nanotube fiber is 50wt%-80wt%, and the content of the silicon carbide is 20wt%-50wt%.
[0026] The method for preparing carbon nanotube fibers includes twisting a carbon nanotube fiber preform to obtain twisted carbon nanotube fibers. Twisting helps make the surface of the carbon nanotube fibers more uniform, making the diameters at different locations more consistent, and allowing silicon carbide to be more evenly deposited on the surface of the carbon nanotube fibers. Without twisting, the carbon nanotube fibers expand when heated in a deposition chamber, preventing silicon carbide from being evenly deposited on the surface of the carbon nanotube fibers. This results in different deposition patterns at different locations of the final deposited carbon nanotube / silicon carbide composite fibers, thereby affecting thermal and electrical conductivity.
[0027] In some embodiments, the radius of the carbon nanotube fiber preform is 30 μm to 60 μm; for example, it can be 30 μm, 40 μm, 50 μm, or 60 μm. The carbon nanotube fiber preform described herein is a bundle of multiple carbon nanotubes, and the radius of the carbon nanotube fiber preform is the radius of the bundle of multiple carbon nanotubes.
[0028] In some embodiments, the diameter of the carbon nanotube is 2 nm to 10 nm, for example, 2 nm, 4 nm, 6 nm, 8 nm, and 10 nm. The diameter of the carbon nanotube refers to the diameter of a single carbon nanotube.
[0029] In some embodiments, the length of the carbon nanotubes is 0.5 μm-10 μm, for example, 0.5 μm, 1 μm, 2 μm, 4 μm, 6 μm, 8 μm, and 10 μm.
[0030] In some embodiments, the carbon nanotubes are at least one of single-walled carbon nanotubes, double-walled carbon nanotubes, and multi-walled carbon nanotubes. More preferably, the carbon nanotubes are single-walled carbon nanotubes.
[0031] The twisting conditions include: a time of 60s-240s, for example, 60s, 80s, 100s, 140s, 180s, 200s and 240s, and a twisting speed of 120r / min-350r / min, for example, 120r / min, 150r / min, 200r / min, 250r / min, 300r / min and 350r / min.
[0032] In some embodiments, the radius of the twisted carbon nanotube fibers is 25 μm-115 μm; for example, it can be 25 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, and 115 μm.
[0033] The method also includes homogenizing the twisted carbon nanotube fibers to produce homogenized carbon nanotube fibers. Homogenized carbon nanotube fibers are fibers with approximately equal diameters at different locations, without uneven diameters such as one end being particularly large and the other being particularly small. This homogenization treatment allows for more uniform deposition of silicon carbide on the surface of the carbon nanotube fibers, resulting in the final carbon nanotube / silicon carbide composite fibers having superior mechanical, electrical, and thermal properties.
[0034] The homogenization process involves subjecting the carbon nanotube fibers to a through-hole treatment. This helps to make the diameters of the carbon nanotube fibers approximately equal at different locations, preventing uneven diameters such as one end being particularly large and the other being particularly small. This also prevents the silicon carbide deposited at different locations from varying in content and thickness, which could lead to poor thermal and electrical conductivity of the carbon nanotube / silicon carbide composite fibers as a whole.
[0035] In some embodiments, the pore size of the template used for the via hole treatment is 25 μm to 150 μm. The pore size of the template used for the via hole treatment refers to the radius of the template, and can be, for example, 25 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, and 150 μm. The template used for the via hole treatment is not particularly limited, as long as it can achieve uniform carbon nanotube fibers.
[0036] The method also includes stretching the homogenized carbon nanotube fibers in the longitudinal direction to obtain carbon nanotube fibers. The carbon nanotube fibers are in a stretched state for depositing silicon carbide. The carbon nanotube fibers are subject to stress after the holes are formed. Without stretching, the carbon nanotube fibers expand upon exposure to heat in the deposition chamber, preventing uniform deposition of silicon carbide on the carbon nanotube fiber surface. Therefore, stretching can, to a certain extent, overcome the stress after the holes are formed, facilitating more uniform deposition of silicon carbide on the carbon nanotube fiber surface.
[0037] The stretching treatment conditions include: a stretching force of 5N-10N, for example, 5N, 6N, 7N, 8N, 9N and 10N. The stretching force is tested by attaching a weight.
[0038] In some embodiments, the deposition method includes at least one of chemical vapor deposition, electrochemical deposition, and physical vapor deposition, preferably chemical vapor deposition.
[0039] In some embodiments, the process parameters of chemical vapor deposition include a deposition temperature of 900°C-1450°C, for example, 900°C, 1000°C, 1100°C, 1200°C, 1300°C, 1400°C and 1450°C, a deposition pressure of 10kPa-40kPa, for example, 10kPa, 15kPa, 20kPa, 25kPa, 30kPa, 35kPa and 40kPa, and a deposition time of 10min-60min; for example, 10min, 20min, 30min, 40min, 50min and 60min.
[0040] In some embodiments, the direction of the gas flow during the chemical vapor deposition process is perpendicular to the orientation of the carbon nanotube fibers. This perpendicular orientation of the gas flow facilitates more uniform deposition of silicon carbide on the surface of the carbon nanotube fibers. If the gas flow during the chemical vapor deposition process is not perpendicular to the orientation of the carbon nanotube fibers, the thickness of the silicon carbide deposited at different locations may vary, thereby affecting the final thermal and electrical conductivity.
[0041] In some embodiments, the gas used in the chemical vapor deposition process includes a carbon silicon source gas and a reducing gas.
[0042] In some embodiments, the flow ratio of the carbon silicon source gas to the reducing gas is 1:5-30; for example, it can be 1:5, 1:10, 1:15, 1:20, 1:25 and 1:30.
[0043] In some embodiments, the flow rate of the carbon silicon gas source is 5-18 L / min.
[0044] In some embodiments, the H2 gas flow rate is 10-35 L / min.
[0045] In some embodiments, the carbon silicon gas source includes a carbon silicon gas source with carbon atoms of C1-C4 and / or a chlorocarbon silicon gas source; preferably, the carbon silicon gas source includes at least one of monosilane, disilane and trisilane; preferably, the chlorosilane includes at least one of methylchlorosilane, dimethylchlorosilane and trichloromethylsilane.
[0046] In some embodiments, the reducing gas comprises hydrogen.
[0047] In some embodiments, the method further comprises heat treating the material after depositing the silicon carbide shell layer.
[0048] In some embodiments, the heat treatment conditions include a temperature of 1350° C. to 1800° C., for example, 1350° C., 1400° C., 1500° C., 1600° C., 1700° C., and 1800° C., and a time of 0.5 h to 5 h, for example, 0.5 h, 1 h, 2 h, 3 h, 4 h, and 5 h. Heat treatment helps to make the carbon nanotube fibers and the silicon carbide shell layer more tightly bonded, thereby improving the mechanical properties of the carbon nanotube / silicon carbide composite fibers.
[0049] The ratio of the radius of the carbon nanotube fiber to the thickness of the silicon carbide shell is 2-30:1, for example, 2:1, 5:1, 10:1, 15:1, 20:1 and 30:1.
[0050] The thickness of the silicon carbide shell layer is 1 μm-18 μm; for example, it can be 1 μm, 2 μm, 4 μm, 6 μm, 8 μm, 10 μm, 12 μm, 14 μm, 16 μm and 18 μm.
[0051] The radius of the carbon nanotube fiber is 15 μm-80 μm; for example, it can be 15 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm and 80 μm. In the carbon nanotube / silicon carbide composite fiber, the content of the carbon nanotube fiber is 50 wt%-80 wt%, for example, it can be 50 wt%, 60 wt%, 70 wt% and 80 wt%, and the content of silicon carbide is 20 wt%-50 wt%, for example, it can be 20 wt%, 30 wt%, 40 wt% and 50 wt%. The content of silicon carbide in the present invention is the percentage of the mass of silicon carbide to the mass of the carbon nanotube / silicon carbide composite fiber, and the mass of silicon carbide is the difference between the mass of the carbon nanotube / silicon carbide composite fiber and the mass of the carbon nanotube fiber.
[0052] In some embodiments, the ratio of the radius of the carbon nanotube fiber to the thickness of the silicon carbide shell is 3-20:1, for example, 3:1, 5:1, 10:1, 15:1, or 20:1.
[0053] In some embodiments, the thickness of the silicon carbide shell is 3 μm to 12 μm; for example, it can be 3 μm, 4 μm, 6 μm, 8 μm, 10 μm, and 12 μm. The thickness of the silicon carbide shell is the difference between the radius of the carbon nanotube / silicon carbide composite fiber and the radius of the carbon nanotube fiber, where the radius of the carbon nanotube fiber is the radius of the carbon nanotube fiber during chemical deposition. The present invention helps improve the mechanical properties of the carbon nanotube / silicon carbide composite fiber by depositing the silicon carbide shell on the carbon nanotube fiber. It also prevents the carbon nanotube fiber from direct contact with the external environment, preventing oxidation from damaging the electrical and thermal conductivity of the carbon nanotube fiber.
[0054] In some embodiments, the radius of the carbon nanotube fiber is 30 μm-60 μm; for example, it can be 30 μm, 40 μm, 50 μm, or 60 μm. The radius of the carbon nanotube fiber described here is the radius of the carbon nanotube fiber when the silicon carbide shell is deposited.
[0055] In some embodiments, the length of the carbon nanotube fibers is 50 cm to 80 cm, for example, 50 cm, 60 cm, 70 cm, and 80 cm. The length of the carbon nanotube fibers described herein refers to the length of the carbon nanotube fibers when the silicon carbide shell is deposited.
[0056] A second aspect of the present invention provides a carbon nanotube / silicon carbide composite fiber obtained using the preparation method described in the first aspect.
[0057] In some embodiments, the carbon nanotube / silicon carbide composite fiber includes a carbon nanotube fiber and a silicon carbide shell layer wrapping the carbon nanotube fiber; the ratio of the radius of the carbon nanotube fiber to the thickness of the silicon carbide shell layer is 2-30:1, and the thickness of the silicon carbide shell layer is 1 μm-18 μm; the radius of the carbon nanotube fiber is 15 μm-80 μm.
[0058] In some embodiments, the carbon nanotube fiber has a tensile strength of 1000 MPa-1500 MPa, for example, 1000 MPa, 1100 MPa, 1200 MPa, 1300 MPa, 1400 MPa, and 1500 MPa.
[0059] In some embodiments, the tensile strength of the carbon nanotube / silicon carbide composite fiber is between 1500 MPa and 3000 MPa; for example, 1500 MPa, 1800 MPa, 2000 MPa, 2300 MPa, 2500 MPa, 2800 MPa, and 3000 MPa. The tensile strength test method described herein is to use an Instron 3365 to test the mechanical properties of the carbon nanotube / silicon carbide composite fiber.
[0060] In some embodiments, the carbon nanotube / silicon carbide composite fiber has an electrical conductivity of 3500 S / cm-6500 S / cm; for example, 3500 S / cm, 4000 S / cm, 4500 S / cm, 5000 S / cm, 5500 S / cm, 6000 S / cm, and 6500 S / cm. The electrical conductivity test method described herein is to measure resistance at room temperature using a quadrupole method, and then calculate the electrical conductivity based on the resistance value.
[0061] In some embodiments, the thermal conductivity of the carbon nanotube / silicon carbide composite fiber is between 450 W / mK and 1000 W / mK; for example, 450 W / mK, 600 W / mK, 700 W / mK, 800 W / mK, 900 W / mK, and 1000 W / mK. The thermal conductivity is measured using a laser flash method using a laser thermal conductivity analyzer (LFA467).
[0062] In some embodiments, the silicon carbide of the silicon carbide shell is α-silicon carbide and / or β-silicon carbide. More preferably, the silicon carbide shell is β-silicon carbide.
[0063] The description of the carbon nanotube fibers and silicon carbide in the carbon nanotube / silicon carbide composite fibers refers to that described in the first aspect and will not be repeated here.
[0064] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.
[0065] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0066] The present invention will be described in detail below with reference to specific embodiments. These embodiments are intended to help you understand the present invention but are not intended to limit it.
[0067] Example 1
[0068] This example is used to illustrate the preparation method of the carbon nanotube / silicon carbide composite fiber of the present invention.
[0069] (1) Commercially available carbon nanotube fiber raw materials with a radius of 40 μm and a length of 60 cm were twisted for 100 s at a twisting speed of 250 r / min. The twisted carbon nanotube fibers were then passed through a drawing die with a pore size of 40 μm.
[0070] (2) Place the twisted and perforated carbon nanotube fiber in a chemical vapor deposition furnace (CVD deposition furnace), and fix the two ends between the motor and the spring respectively, so that the carbon nanotube fiber is perpendicular to the flow direction of the subsequent reaction gas, and the spring tension is 8N.
[0071] (3) CH3SiCl3 gas and H2 were introduced into the CVD deposition furnace with the dilution gas Ar, wherein the gas flow rate of CH3SiCl3 was 3 L / min, the gas flow rate of H2 was 24 L / min, the flow ratio of CH3SiCl3 gas and H2 was 1:8, and the flow rate of the dilution gas Ar was 30% of the mixed gas. The deposition process parameters were set as follows: the deposition temperature was 1215 °C, the deposition pressure was 13 kPa, and the deposition time was 30 min. After the chemical vapor deposition was completed, the reaction gas was stopped and the protective gas argon was continuously introduced for cooling treatment to obtain a preformed carbon nanotube / silicon carbide composite fiber.
[0072] (4) The preformed carbon nanotube / silicon carbide composite fiber deposited above was heat treated at a temperature of 1650°C for 1 hour to obtain a carbon nanotube / silicon carbide composite fiber. The final carbon nanotube / silicon carbide composite fiber had a carbon nanotube fiber radius of 40 μm, a silicon carbide shell thickness of 5 μm, a carbon nanotube fiber content of 67 wt%, and a silicon carbide content of 33 wt%. Figure 1 The above is a SEM image of the side surface of the carbon nanotube / silicon carbide composite fiber of Example 1. Figure 2 Shown is the SEM image of the cross section of carbon nanotube / silicon carbide composite fiber.
[0073] Example 2
[0074] This embodiment is used to illustrate carbon nanotube / silicon carbide composite fibers made from carbon nanotube fibers with different radii.
[0075] Example 2-1
[0076] The operation was carried out in accordance with the method described in Example 1, except that the carbon nanotube fiber raw material with a radius of 30 μm was twisted.
[0077] Example 2-2
[0078] The operation was carried out in accordance with the method described in Example 1, except that the carbon nanotube fiber raw material with a radius of 60 μm was twisted.
[0079] Example 3
[0080] This embodiment is used to illustrate carbon nanotube / silicon carbide composite fibers produced under different twisting times and twisting speeds.
[0081] Example 3-1
[0082] The operation was carried out in accordance with the method described in Example 1, except that the twisting time was 70 s and the twisting speed was 150 r / min.
[0083] Example 3-2
[0084] The operation was carried out in accordance with the method described in Example 1, except that the twisting time was 220 s and the twisting speed was 320 r / min.
[0085] Example 4
[0086] This embodiment is used to illustrate carbon nanotube / silicon carbide composite fibers produced by stretching homogenized carbon nanotube fibers to different degrees in the length direction.
[0087] Example 4-1
[0088] The operation was carried out according to the method described in Example 1, except that the stretching force was 6N.
[0089] Example 4-2
[0090] The operation was carried out according to the method described in Example 1, except that the stretching force was 9N.
[0091] Example 5
[0092] This example is used to illustrate carbon nanotube / silicon carbide composite fibers deposited under different vapor deposition conditions.
[0093] Example 5-1
[0094] The method described in Example 1 was followed, except that the deposition temperature was 950°C.
[0095] Example 5-2
[0096] The method described in Example 1 was followed, except that the deposition temperature was 1400°C.
[0097] Example 5-3
[0098] The operation was carried out in accordance with the method described in Example 1, except that the deposition pressure was 10 kPa.
[0099] Example 5-4
[0100] The operation was carried out in accordance with the method described in Example 1, except that the deposition pressure was 35 kPa.
[0101] Example 5-5
[0102] The operation was carried out according to the method described in Example 1, except that the deposition time was 15 minutes.
[0103] The radius of the carbon nanotube fiber finally obtained is 40 μm, the thickness of the silicon carbide shell is 2 μm, the content of the carbon nanotube fiber is 76 wt%, and the content of silicon carbide is 34 wt%.
[0104] Examples 5-6
[0105] The operation was carried out according to the method described in Example 1, except that the deposition time was 50 min.
[0106] The radius of the carbon nanotube fiber finally obtained is 40 μm, the thickness of the silicon carbide shell is 8 μm, the content of the carbon nanotube fiber is 58 wt%, and the content of silicon carbide is 42 wt%.
[0107] Examples 5-7
[0108] The operation was carried out according to the method described in Example 1, except that the flow ratio of MTS to hydrogen was 1:5.
[0109] Examples 5-8
[0110] The operation was carried out according to the method described in Example 1, except that the flow ratio of MTS to hydrogen was 1:25.
[0111] Example 6
[0112] This embodiment is used to illustrate carbon nanotube / silicon carbide composite fibers obtained by heat treating the material after depositing the silicon carbide shell at different temperatures.
[0113] Example 6-1
[0114] The process described in Example 1 was followed, except that the heat treatment temperature was 1500°C.
[0115] Example 6-2
[0116] The operation was carried out in accordance with the method described in Example 1, except that the heat treatment temperature was 1750°C.
[0117] Comparative Example 1
[0118] Comparative Example 1 is used to illustrate the preparation of carbon nanotube / silicon carbide composite fibers when the radius of the carbon nanotube fibers is not within the scope of protection of the present invention.
[0119] Comparative Example 1-1
[0120] The operation was carried out in accordance with the method described in Example 1, except that the radius of the carbon nanotube fiber was 10 μm.
[0121] Comparative Example 1-2
[0122] The operation was carried out according to the method described in Example 1, except that the radius of the carbon nanotube fiber was 100 μm.
[0123] Comparative Example 2
[0124] Comparative Example 2 is used to illustrate the preparation of carbon nanotube / silicon carbide composite fibers when the thickness of the shell layer is not within the scope of protection of the present invention.
[0125] Comparative Example 2-1
[0126] The operation was carried out according to the method described in Example 2, except that the thickness of the silicon carbide shell layer in the finally prepared carbon nanotube / silicon carbide composite fiber was 50 μm.
[0127] Comparative Example 2-2
[0128] The method described in Example 1 was followed, except that the thickness of the silicon carbide shell in the carbon nanotube / silicon carbide composite fiber finally obtained was less than 1 μm.
[0129] Comparative Examples 2-3
[0130] The operation was carried out according to the method described in Example 1, except that the thickness of the silicon carbide shell layer in the finally prepared carbon nanotube / silicon carbide composite fiber was 25 μm.
[0131] Comparative Example 3
[0132] The operation was carried out according to the method described in Example 1, except that the stretching force was 0N.
[0133] Test Case
[0134] The carbon nanotube / silicon carbide composite fibers obtained in the above examples and comparative examples were tested, and the test results are shown in Table 1.
[0135] Tensile strength of carbon nanotube / silicon carbide composite fibers: The mechanical properties of carbon nanotube / silicon carbide composite fibers were tested using Instron 3365. The test results are shown in Table 1.
[0136] Conductivity: The test method is to use the quadrupole method to measure the resistance at room temperature, and then calculate the conductivity based on the resistance value. The test results are shown in Table 1.
[0137] Thermal conductivity: measured by laser flash method using a laser thermal conductivity analyzer (LFA467). The test results are shown in Table 1.
[0138] Table 1
[0139]
[0140] Compared with the comparative example, the carbon nanotube / silicon carbide composite fiber of the present invention and the carbon nanotube / silicon carbide composite fiber obtained by the preparation method of the present invention have high electrical conductivity, high thermal conductivity and greater tensile strength.
[0141] Compared with other embodiments, the electrical conductivity, thermal conductivity and tensile strength of carbon nanotube / silicon carbide composite fiber of embodiment 1 are better than those of other embodiments, and are much better than those of the comparative example.
[0142] Example 2 is a carbon nanotube / silicon carbide composite fiber prepared when the carbon nanotube fiber radius is different. Comparative Example 1 is a carbon nanotube / silicon carbide composite fiber prepared when the radius of the carbon nanotube fiber is not within the scope of protection of the present invention. The tensile strength, electrical conductivity and thermal conductivity of the carbon nanotube / silicon carbide composite fiber of Example 2 are much better than those of Comparative Example 1.
[0143] Example 3 shows carbon nanotube / silicon carbide composite fibers produced at different twisting times and twisting speeds. Both twisting time and twisting speed affect the carbon nanotube / silicon carbide composite fibers. Example 4 shows carbon nanotube / silicon carbide composite fibers produced by stretching homogenized carbon nanotube fibers to varying degrees along their length. Different stretching forces lead to different ductility of the carbon nanotube fibers, as well as different uniformity and shedding of silicon carbide deposited on their surfaces.
[0144] Example 5 shows carbon nanotube / silicon carbide composite fibers produced under different vapor deposition conditions. Varying the deposition temperature, pressure, and time yielded varying silicon carbide structures and thicknesses. Comparative Example 2 illustrates the preparation of carbon nanotube / silicon carbide composite fibers when the shell thickness falls outside the scope of the present invention. Comparison of Example 5 with Comparative Example 2 reveals significantly lower tensile strength, electrical conductivity, and thermal conductivity than the carbon nanotube / silicon carbide composite fibers produced in Example 5.
[0145] The carbon nanotube / silicon carbide composite fibers in Example 6 were obtained by heat treatment at different temperatures. The degree of bonding between the carbon nanotube fibers and silicon carbide was different when the heat treatment temperature was different, and the mechanical properties of the carbon nanotube / silicon carbide composite fibers were also different.
[0146] It should be noted that, in this article, the terms "comprise", "include" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device comprising a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the statement "comprises a ..." does not exclude the presence of other identical elements in the process, method, article or device comprising the element. In addition, it should be noted that the scope of the methods and devices in the embodiments of the present application is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in the opposite order according to the functions involved. For example, the described method may be performed in an order different from that described, and various steps may also be added, omitted, or combined. In addition, the features described with reference to certain examples may be combined in other examples.
[0147] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing carbon nanotube / silicon carbide composite fibers, characterized in that: The method comprises depositing a silicon carbide shell layer on the surface of a carbon nanotube fiber to obtain a carbon nanotube / silicon carbide composite fiber; The preparation method of the carbon nanotube fiber comprises: (1) twisting a carbon nanotube fiber preform to obtain twisted carbon nanotube fibers; (2) performing a homogenization treatment on the twisted carbon nanotube fibers to obtain homogenized carbon nanotube fibers; the homogenization treatment is performed by performing a through-hole treatment on the carbon nanotube fibers; (3) stretching the homogenized carbon nanotube fibers in the length direction to obtain carbon nanotube fibers; The twisting conditions include: time of 60s-240s, twisting speed of 120r / min-350r / min; the stretching conditions include: stretching force of 5N-10N; The ratio of the radius of the carbon nanotube fiber to the thickness of the silicon carbide shell is 2-30:1, the thickness of the silicon carbide shell is 1µm-18µm, the radius of the carbon nanotube fiber is 15µm-80µm, and in the carbon nanotube / silicon carbide composite fiber, the content of the carbon nanotube fiber is 50wt%-80wt%, and the content of the silicon carbide is 20wt%-50wt%.
2. The method according to claim 1, characterized in that The deposition method of the silicon carbide shell layer deposited on the surface of the carbon nanotube fiber includes one of chemical vapor deposition, electrochemical deposition and physical vapor deposition.
3. The method according to claim 2, characterized in that The process parameters of chemical vapor deposition include deposition temperature of 900°C-1450°C, deposition pressure of 10kPa-40kPa, and deposition time of 10min-60min.
4. The method according to claim 2, characterized in that: The gas used in the chemical vapor deposition process includes a carbon silicon source gas and a reducing gas, and the flow ratio of the carbon silicon source gas to the reducing gas is 1:5-30.
5. The method according to claim 3, characterized in that: During the chemical vapor deposition process, the direction of the gas flow is perpendicular to the placement direction of the carbon nanotube fibers.
6. The method according to claim 1, characterized in that The method also includes heat treating the material after the silicon carbide shell layer is deposited; the heat treatment conditions include a temperature of 1350° C.-1800° C. and a time of 0.5 h-5 h.
7. The method according to claim 1, characterized in that The ratio of the radius of the carbon nanotube fiber to the thickness of the silicon carbide shell layer is 3-20:
1.
8. The method according to claim 7, characterized in that The thickness of the silicon carbide shell layer is 3 μm-12 μm; and / or, The radius of the carbon nanotube fiber is 30 μm-60 μm; and / or, The length of the carbon nanotube fiber is 50 cm-80 cm; and / or, The tensile strength of the carbon nanotube fiber is 1000MPa-1500MPa.
9. A carbon nanotube / silicon carbide composite fiber, characterized in that: The carbon nanotube / silicon carbide composite fiber is prepared by the method described in any one of claims 1-8.
10. The carbon nanotube / silicon carbide composite fiber according to claim 9, characterized in that: The tensile strength of the carbon nanotube / silicon carbide composite fiber is 1500MPa-3000MPa, the electrical conductivity of the carbon nanotube / silicon carbide composite fiber is 3500S / cm-6500S / cm, and the thermal conductivity of the carbon nanotube / silicon carbide composite fiber is 450w / mK-1000w / mK.