A cerium-based composite catalyst and its preparation method and application
By regulating the acid-base sites by transition metal doping in the cerium-based composite catalyst, the problems of large catalyst dosage, high toxicity and poor stability are solved, and efficient catalysis of the reaction of diphenyl urea and dimethyl carbonate is achieved, achieving high conversion rate and high yield of phenylcarbamate methyl ester, with optimized catalyst stability and cost.
Patent Information
- Application Number
- CN202411026124.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-30
AI Technical Summary
Existing catalysts have problems such as large catalyst dosage, high toxicity, poor stability, complex preparation process and high cost in catalyzing the reaction of diphenyl urea and dimethyl carbonate, which affects the efficient preparation of phenyl methyl carbamate.
Using a cerium-based composite catalyst, the acid-base active sites on the catalyst surface are controlled by doping transition metals (such as Ni, Ti, V, Mo or Nb) to form a cerium-based composite catalyst with high catalytic activity and stability for catalysis. Coupling reaction of diphenyl urea and dimethyl carbonate.
It achieves a high conversion rate of diphenyl urea and a high yield of phenyl methyl carbamate. The catalyst has a long service life and almost no performance degradation after multiple cycles. The preparation process is simple, the cost is low, and it is suitable for industrial applications.
Smart Images

Figure CN118543346B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalysts, and specifically relates to a cerium-based composite catalyst and a preparation method and application thereof, and in particular relates to a cerium-based composite catalyst for preparing methyl phenylcarbamate and a preparation method and application thereof. Background Art
[0002] Methyl phenylcarbamate (MPC) is an intermediate for the synthesis of diphenylmethane diisocyanate (MDI), which is one of the important raw materials for the synthesis of polyurethane. At present, the main production method of MPC is the phosgene method, which uses highly toxic raw materials and has high safety risks; it produces a large amount of chlorine-containing waste salts and by-product hydrochloric acid, resulting in a high risk of equipment corrosion; and the resulting product contains free chlorine that is difficult to remove, affecting the product quality. Therefore, in recent years, various non-phosgene routes for the synthesis of MPC have continued to emerge, mainly including oxidative carbonylation, reductive carbonylation, DMC ammonolysis, and diphenylurea alcoholysis. However, these methods have the generation of intermediates, low atomic utilization, low MPC yield, high cost of synthetic raw materials, and the required catalysts are expensive, large in dosage, poor in cyclic stability, and highly toxic.
[0003] CN102872912A discloses a catalyst for synthesizing methyl phenylcarbamate, and a preparation method and application method thereof, specifically a silica gel surface bonded zinc carboxylate catalyst, which is used to catalyze the reaction of aniline and dimethyl carbonate (DMC ammonolysis method) to generate methyl phenylcarbamate. The highest product yield is 95.9%, which still has room for improvement. The catalyst is still a supported catalyst, and the active components are also easily lost. In addition, its preparation process is very complicated, the raw material cost is high, and industrialization is difficult.
[0004] Zhang Lei et al. (Petrochemical Engineering, 2006 (11): 1048-1051) used diphenylurea and methanol as raw materials and CO2 as protective gas to synthesize methyl phenylcarbamate under the catalytic action of PbO / Al2O3 catalyst. However, the conversion rate of diphenylurea was only 95.7%, and the yield of methyl phenylcarbamate was only 84.4%, which still had a lot of room for improvement. In addition, the catalyst PbO / Al2O3 used in this method used toxic lead, which was highly toxic.
[0005] However, the coupling reaction of diphenyl urea and dimethyl carbonate is a greener route. This method only uses dimethyl carbonate and diphenyl urea as raw materials. Theoretically, the product is only methyl phenylcarbamate, and no by-products are generated. It has the advantages of high atom economy, mild synthesis conditions and high MPC yield. However, it still has the defects of catalyst poisoning, large dosage and poor stability.
[0006] CN101665411A discloses an alcohol lead compound catalyst, which is used to catalyze the reaction of synthesizing methyl phenylcarbamate using dimethyl carbonate and diphenylurea as raw materials. Although this method can obtain a higher MPC yield, the catalyst contains lead, which is highly toxic and has unstable catalytic activity. After repeated use, the MPC yield is greatly attenuated.
[0007] CN102513087A discloses a catalyst for synthesizing phenylcarbamate from diphenylurea, wherein a catalyst having RE1A is prepared by using rare earth compounds, transition metal compounds and / or aluminum compounds as raw materials. a B 1-a A composite oxide with an O3 molecular composition and a perovskite crystal form, wherein 0≤a≤1, RE is a rare earth element, A is a transition metal element, and B is an aluminum element, which is used to catalyze the reaction of diphenyl urea and dimethyl carbonate to produce MPC. The preparation conditions of this multiphase catalyst are harsh, the operation is complicated, the preparation cost is high, and a large amount of catalyst is required in the catalytic reaction.
[0008] Therefore, in view of the above defects, there is an urgent need to develop a new catalyst with high catalytic activity and high stability and a preparation method thereof, which can be used to catalyze the coupling reaction of diphenyl urea and dimethyl carbonate to prepare methyl phenylcarbamate, so as to solve the problems of large catalyst dosage and high toxicity. Summary of the invention
[0009] In view of the deficiencies in the prior art, the present invention aims to provide a cerium-based composite catalyst for preparing methyl phenylcarbamate, a preparation method thereof and an application thereof. By doping and combining a specific type of transition metal, the cerium element is effectively combined with the transition metal to regulate the acid-base active sites on the surface of the obtained catalyst, so as to form a cerium-based composite catalyst with high catalytic activity; and the cerium-based composite catalyst is used to catalyze the coupling reaction of diphenylurea and dimethyl carbonate to synthesize methyl phenylcarbamate, without generating intermediate products, showing a high conversion rate of diphenylurea and a high yield of methyl phenylcarbamate. At the same time, the cerium-based composite catalyst also has strong stability and a long service life. After being repeatedly used for 5 times, the catalytic performance is almost not attenuated. Moreover, the preparation process is simple, the raw materials are cheap, the production cost is low, and it is easy to industrialize.
[0010] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0011] In a first aspect, the present invention provides a cerium-based composite catalyst, which comprises a cerium-based oxide doped with a transition metal; the transition metal comprises any one of Ni, Ti, V, Mo or Nb, or a combination of at least two thereof.
[0012] The transition metal may be a combination of Ni and Ti, a combination of V and Mo, a combination of Ti and Mo, or a combination of Ti and Nb.
[0013] The cerium-based composite catalyst of the present invention dopes cerium with a specific type of transition metal element (any one of Ni, Ti, V, Mo or Nb or a combination of at least two of them) to cause lattice distortion, increase defects and oxygen vacancies, so as to effectively regulate the acid-base active sites on the surface of the obtained catalyst, especially to increase the acid sites, thereby improving the catalytic activity and stability of the catalyst.
[0014] It is worth noting that the present invention selects specific cerium to be doped with specific transition metals. The transition metals are not attached to the surface of the cerium-based oxide, but form a solid solution. The two act synergistically to improve the catalytic activity of the obtained catalyst. Among them, the controllable adjustment of the acidity and alkalinity of pure phase cerium oxide is limited, and the active sites are insufficient; while the ionic states of the transition metals such as Ni, Ti, V, Mo or Nb are all multivalent, and the ionic radius is smaller than Ce. 4+ The ions are small and can be effectively doped into the cerium oxide lattice to produce more lattice defects, thereby regulating the acid-base active sites on the catalyst surface, especially increasing the acid sites, thereby improving the catalytic activity and stability of the catalyst.
[0015] Preferably, the chemical formula of the cerium-based composite catalyst is a Ce 1-a O x , wherein M includes any one of Ni, Ti, V, Mo or Nb, or a combination of at least two thereof, such as a combination of Ni and Ti, a combination of V and Mo, a combination of Ti and Mo, or a combination of Ti and Nb, etc.; 0.01≤a≤0.2, such as 0.01, 0.03, 0.05, 0.08, 0.1, 0.12, 0.15, 0.18 or 0.2, etc., preferably 0.02≤a≤0.15; 1.8≤x≤2.6, such as 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5 or 2.6, etc.
[0016] Preferably, the content of cerium element in the cerium-based composite catalyst is 57.4-81.1wt%, for example, it can be 57.4wt%, 59.4wt%, 61.4wt%, 63.4wt%, 65.4wt%, 67.4wt%, 69.4wt%, 71.4wt%, 74.1wt%, 76.4wt%, 78.6wt% or 81.1wt%.
[0017] Preferably, the content of transition metal elements in the cerium-based catalyst is 0.24-11.6 wt%, for example, it can be 0.24 wt%, 0.50 wt%, 0.80 wt%, 1 wt%, 3 wt%, 5 wt%, 8 wt%, 10 wt%, 10.7 wt% or 11.6 wt%.
[0018] In a second aspect, the present invention provides a method for preparing the cerium-based composite catalyst according to the first aspect, the preparation method comprising the following steps:
[0019] (1) mixing a cerium source, a transition metal source, a precipitant and a solvent, and reacting to obtain a precursor solution of a cerium-based composite catalyst;
[0020] (2) subjecting the precursor solution of step (1) to solid-liquid separation to obtain a precursor of a cerium-based composite catalyst;
[0021] (3) calcining the precursor in step (2) to obtain a cerium-based composite catalyst.
[0022] The preparation method of the cerium-based composite catalyst of the present invention has the advantages of simple preparation process, easy control of conditions, easy availability of raw materials, low production cost, simple synthesis route and easy industrialization.
[0023] Preferably, the cerium source in step (1) comprises a cerium salt.
[0024] Preferably, the cerium source in step (1) comprises any one of cerium nitrate, cerium chloride, cerium sulfate or cerium acetate, or a combination of at least two thereof, wherein typical but non-limiting combinations include a combination of cerium nitrate and cerium chloride, a combination of cerium nitrate and cerium acetate, or a combination of cerium sulfate and cerium chloride, etc., preferably a combination of cerium nitrate and cerium chloride.
[0025] Preferably, the transition metal source in step (1) comprises a transition metal salt.
[0026] Preferably, the transition metal source in step (1) comprises any one of transition metal chlorides, transition metal nitrates, transition metal sulfates, transition metal acetates or transition metal oxalates, or a combination of at least two of them, wherein typical but non-limiting combinations include a combination of transition metal chlorides and transition metal nitrates, a combination of transition metal sulfates and transition metal acetates, or a combination of transition metal acetates and transition metal oxalates, and preferably a combination of transition metal chlorides and transition metal nitrates.
[0027] Preferably, the transition metal includes any one or a combination of at least two of Ni, Ti, V, Mo or Nb;
[0028] Preferably, the precipitant in step (1) comprises any one of urea, sodium hydroxide, potassium hydroxide, sodium bicarbonate, sodium carbonate, potassium carbonate, potassium bicarbonate or ammonia water, or a combination of at least two thereof, wherein typical but non-limiting combinations include a combination of urea and sodium hydroxide, a combination of sodium hydroxide and potassium hydroxide, a combination of sodium bicarbonate and sodium carbonate, or a combination of sodium carbonate and potassium carbonate, etc.
[0029] Preferably, the solvent in step (1) comprises any one of water, ethanol, methanol or dimethylformamide, or a combination of at least two of them, wherein typical but non-limiting combinations include a combination of water and ethanol, a combination of water and dimethylformamide, or a combination of ethanol and dimethylformamide, etc.
[0030] Preferably, the molar ratio of the transition metal source to the cerium source in step (1) is (0.01-0.25):1, for example, it can be 0.01:1, 0.05:1, 0.08:1, 0.1:1, 0.15:1, 0.20:1 or 0.25:1, etc.
[0031] The present invention further preferably has a molar ratio of the transition metal source to the cerium source in step (1) of (0.01-0.25):1, so that the transition metal is effectively doped and combined, thereby effectively regulating the acid-base active sites on the surface of the resulting catalyst and improving the catalytic activity of the catalyst; if the molar ratio of the transition metal source to the cerium source is too small, it will result in too few defects and limited regulation of the acid-base sites; if the molar ratio of the transition metal source to the cerium source is too large, that is, the doping amount of the transition metal is too large, the acid-base properties of the catalyst surface are reduced, thereby having a negative impact on the activity of the catalyst, resulting in a significant reduction in the catalytic activity of the catalyst.
[0032] Preferably, the molar ratio of the precipitant to the cerium source in step (1) is (4-100):1, for example, 4:1, 10:1, 20:1, 30:1, 40:1, 50:1, 60:1, 70:1, 80:1, 90:1 or 100:1, and preferably (20-50):1.
[0033] The present invention further preferably has a molar ratio of the precipitant to the cerium source of (4-100):1, which is conducive to the cerium ions and transition metal ions fully reacting with the precipitant to produce the precursor solution of the cerium-based composite catalyst; and improving the yield of the cerium-based composite catalyst. If the corresponding molar ratio is too small, most of the cerium ions and transition metal ions cannot react to obtain the precursor solution of the cerium-based composite catalyst, resulting in failure to obtain an ideal precursor morphology or crystal form; if the corresponding molar ratio is too large, it causes a waste of reagents and increases the cost of catalyst preparation.
[0034] Preferably, the mass volume ratio of the cerium source and the solvent in step (1) is 1:(10-100) g / mL, for example, it can be 1:10 g / mL, 1:20 g / mL, 1:30 g / mL, 1:40 g / mL, 1:50 g / mL, 1:60 g / mL, 1:70 g / mL, 1:80 g / mL, 1:90 g / mL or 1:100 g / mL, and is preferably 1:(20-40) g / mL.
[0035] Preferably, the mixing temperature in step (1) is 20-80°C, for example, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C or 80°C.
[0036] Preferably, the mixing time in step (1) is 0.5 to 3 h, for example, 0.5 h, 1 h, 1.5 h, 2 h, 2.5 h or 3 h.
[0037] Preferably, the mixing process is accompanied by stirring.
[0038] Preferably, the reaction temperature in step (1) is 60-140°C, for example, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C or 140°C.
[0039] Preferably, the reaction time of step (1) is 6 to 48 h, for example, it can be 6 h, 8 h, 10 h, 12 h, 15 h, 20 h, 24 h, 28 h, 32 h, 36 h, 42 h or 48 h.
[0040] Preferably, after the solid-liquid separation in step (2), washing and drying are performed in sequence.
[0041] Preferably, the number of washings is ≥ 3, for example, 3 times, 4 times or 5 times.
[0042] Preferably, the drying temperature is 90-120°C, for example, it may be 90°C, 95°C, 100°C, 105°C, 110°C, 115°C or 120°C.
[0043] Preferably, the drying time is 10 to 15 h, for example, 10 h, 11 h, 12 h, 13 h, 14 h or 15 h.
[0044] Preferably, the calcination temperature in step (3) is 300-700°C, for example, it can be 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C or 700°C.
[0045] Preferably, the calcination time in step (3) is 3 to 12 h, for example, 3 h, 6 h, 8 h, 10 h or 12 h.
[0046] Preferably, the calcination atmosphere in step (3) includes an air atmosphere.
[0047] As a further preferred technical solution of the present invention, the preparation method comprises the following steps:
[0048] (1) mixing a cerium source, a transition metal source, a precipitant and a solvent at 20-80° C. for 0.5-3 h, and then reacting at 60-140° C. for 6-48 h to obtain a precursor solution of a cerium-based composite catalyst; wherein the molar ratio of the cerium source, the transition metal source and the precipitant is 1:(0.01-0.25):(4-100); and the mass volume ratio of the cerium source and the solvent is 1:(10-100) g / mL;
[0049] (2) subjecting the precursor solution of step (1) to solid-liquid separation, washing and drying in sequence to obtain a precursor of a cerium-based composite catalyst;
[0050] (3) Washing the precursor in step (2), drying it at 90-120° C. for 10-15 h, and finally calcining it at 300-700° C. for 3-12 h to obtain a cerium-based composite catalyst.
[0051] In a third aspect, the present invention provides a method for preparing methyl phenylcarbamate, wherein the preparation method is carried out using the cerium-based composite catalyst described in the first aspect; the preparation method comprises the following steps: mixing diphenyl urea, dimethyl carbonate and the cerium-based composite catalyst to obtain methyl phenylcarbamate through a catalytic reaction.
[0052] The preparation method of methyl phenylcarbamate provided by the present invention directly uses diphenyl urea and dimethyl carbonate as raw materials, and prepares methyl phenylcarbamate under the catalytic action of the above-mentioned cerium-based composite catalyst. The conversion rate of diphenyl urea is preferably as high as 98.0% or more, and the yield of methyl phenylcarbamate is preferably as high as 96.6% or more; and the amount of the required cerium-based composite catalyst is relatively small, and the cost is low.
[0053] Preferably, the molar ratio of diphenyl urea to dimethyl carbonate is 1:(1.5-40), for example, it can be 1:1.5, 1:2, 1:5, 1:8, 1:10, 1:12, 1:15, 1:18, 1:20, 1:22, 1:25, 1:28, 1:30, 1:32, 1:35, 1:38 or 1:40, etc., preferably 1:(4-30).
[0054] Preferably, the mass ratio of the diphenyl urea to the cerium-based composite catalyst is 1:(0.01-0.5), for example, it can be 1:0.01, 1:0.03, 1:0.05, 1:0.08, 1:0.1, 1:0.15, 1:0.20, 1:0.25, 1:0.30, 1:0.35, 1:0.40, 1:0.45 or 1:0.5, etc.
[0055] Preferably, the temperature of the catalytic reaction is 120-180°C, for example, it can be 120°C, 130°C, 140°C, 150°C, 160°C, 170°C or 180°C.
[0056] Preferably, the catalytic reaction time is 0.5 to 6 h, for example, it can be 0.5 h, 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h, 5.5 h or 6 h.
[0057] As a further preferred technical solution of the present invention, the preparation method of methyl phenylcarbamate comprises the following steps:
[0058] Diphenyl urea, dimethyl carbonate and the cerium-based composite catalyst are mixed, wherein the molar ratio of the diphenyl urea to the dimethyl carbonate is 1:(1.5-40); the mass ratio of the diphenyl urea to the cerium-based composite catalyst is 1:(0.01-0.5); and then catalytic reaction is carried out at 120-180° C. for 0.5-6 h to obtain methyl phenylcarbamate.
[0059] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0060] Compared with the prior art, the present invention has the following beneficial effects:
[0061] (1) The cerium-based composite catalyst provided by the present invention is a catalyst that is doped with a specific transition metal by selecting a specific cerium element. The two are effectively combined to regulate the acid-base active sites on the surface of the resulting catalyst, thereby obtaining high catalytic activity and high stability, a long service life, and almost no attenuation of catalytic performance after multiple cycles of use. In addition, the cerium-based composite catalyst is low in price, non-toxic, easy to separate and recycle, and has broad application prospects.
[0062] (2) The method for preparing a cerium-based composite catalyst provided by the present invention adopts a solvothermal method to use a cerium source and a specific transition metal source as raw materials, add an alkaline additive, and prepare a cerium-based composite catalyst with both high catalytic activity and high stability under mild conditions; and by further regulating parameters such as the mass ratio of the cerium source and the specific transition metal source, the mass volume ratio of the cerium source and the solvent, the cerium and the transition metal are further effectively combined, and the acid-base active sites on the surface of the obtained cerium-based composite catalyst are regulated to further improve its catalytic activity and stability; and the raw materials for the preparation are widely available, the preparation process is simple and controllable, and it is easy to industrialize.
[0063] (3) The method for preparing methyl phenylcarbamate provided by the present invention uses dimethyl carbonate and diphenyl urea as raw materials, and the two undergo a coupling reaction under the catalytic action of the above-mentioned cerium-based composite catalyst to successfully prepare methyl phenylcarbamate, wherein the conversion rate of diphenyl urea is preferably as high as 98.0% or more, and the yield of methyl phenylcarbamate is as high as 96.6% or more; the highly selective synthesis of methyl phenylcarbamate from diphenyl urea is achieved; the preparation method requires a relatively small amount of cerium-based composite catalyst, is non-toxic and harmless, and is environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0064] Figure 1 is a TEM image of the cerium-based composite catalyst prepared in Example 1 of the present invention;
[0065] Figure 2 It is an XRD comparison diagram of the cerium-based composite catalyst prepared in Example 1 of the present invention and pure phase cerium oxide. DETAILED DESCRIPTION
[0066] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0067] The experimental methods in the following embodiments and comparative examples, application examples and comparative application examples are all conventional methods unless otherwise specified; the experimental materials used are all purchased from conventional biochemical reagent manufacturers unless otherwise specified.
[0068] 1. Implementation
[0069] Example 1
[0070] This embodiment provides a method for preparing a cerium-based composite catalyst, the preparation method comprising the following steps:
[0071] (1) 3.0 g Ce(NO3)3·6H2O, 0.21 g MoCl5 and 20 mL water were mixed under stirring conditions for 1 h to obtain a mixed solution; 10.0 g sodium hydroxide and 80 mL water were mixed under stirring conditions for 1 h to obtain a sodium hydroxide solution, and then the sodium hydroxide solution was added dropwise to the mixed solution while stirring and aged for 1 h to obtain a reaction slurry; and then the reaction slurry was transferred to a hydrothermal reactor and reacted at 120°C for 24 h to obtain a precursor solution of a cerium-based composite catalyst;
[0072] (2) filtering the precursor solution of step (1), washing the filtered solid with water three times, and then drying it in an oven at 100° C. for 12 h to obtain a precursor of a cerium-based composite catalyst;
[0073] (3) The precursor of step (2) is calcined in an air atmosphere at 500° C. for 8 h to obtain the cerium-based composite catalyst.
[0074] The chemical formula of the cerium-based composite catalyst obtained in this embodiment is Mo 0.1 Ce 0.9 O 2.05 , wherein the content of Ce element is 74.8wt%, and the content of transition metal Mo element is 5.7wt%.
[0075] like Figure 1 As shown, Figure 1 The TEM image of the cerium-based composite catalyst prepared in this embodiment shows that Mo 0.1 Ce 0.9 O 2.05 The lattice fringes of 0.19 nm, 0.27 nm, and 0.31 nm are respectively attributed to the (110), (001), and (111) crystal planes of CeO2, which are mainly the exposed crystal planes of rod-shaped CeO2. No lattice fringes attributed to Mo2O5 are observed, indicating that Mo 5+ Doped into the CeO2 lattice.
[0076] like Figure 2 As shown, Figure 2 The XRD comparison diagram of the cerium-based composite catalyst prepared in this example and pure phase cerium oxide shows that Mo 0.1 Ce 0.9 O 2.05 The catalyst shows typical characteristic peaks of CeO2 cubic fluorite structure. No obvious characteristic peaks of Mo2O5 or other impurity peaks are observed. Compared with pure CeO2, Mo 0.1 Ce 0.9 O 2.05 The catalyst diffraction peak shifted to a higher 2θ, indicating that Mo 5+ Replaced part of Ce 4+ , indicating that Mo species enter the CeO2 lattice to form a Ce-Mo solid solution.
[0077] Example 2
[0078] This embodiment provides a method for preparing a cerium-based composite catalyst, the preparation method comprising the following steps:
[0079] (1) 3.0 g Ce(NO3)3·6H2O, 0.0385 g MoCl5 and 30 mL water were mixed under stirring conditions for 0.5 h to obtain a mixed solution; 10.0 g potassium hydroxide and 70 mL water were mixed under stirring conditions for 0.5 h to obtain a potassium hydroxide solution, and then the potassium hydroxide solution was added dropwise to the mixed solution while stirring and aged for 1 h to obtain a reaction slurry; and then the reaction slurry was transferred to a hydrothermal reactor and reacted at 60°C for 48 h to obtain a precursor solution of a cerium-based composite catalyst;
[0080] (2) filtering the precursor solution of step (1), washing the filtered solid with water for 4 times, and then drying it in an oven at 90° C. for 15 h to obtain a precursor of a cerium-based composite catalyst;
[0081] (3) Calcine the precursor prepared in step (2) in an air atmosphere at 300° C. for 12 h to obtain the cerium-based composite catalyst.
[0082] The chemical formula of the cerium-based composite catalyst obtained in this embodiment is Mo 0.02 Ce 0.98 O 2.01 , wherein the content of Ce element is 80.1wt%, and the content of transition metal Mo element is 1.1wt%.
[0083] Example 3
[0084] This embodiment provides a method for preparing a cerium-based composite catalyst, the preparation method comprising the following steps:
[0085] (1) 3.0 g Ce(NO3)3·6H2O, 0.333 g MoCl5 and 40 mL water were mixed under stirring conditions for 0.5 h to obtain a mixed solution; 10.0 g sodium bicarbonate and 60 mL water were mixed under stirring conditions for 0.5 h to obtain a sodium bicarbonate solution, and then the sodium bicarbonate solution was added dropwise to the mixed solution while stirring and aged for 1.5 h to obtain a reaction slurry; and then the reaction slurry was transferred to a hydrothermal reactor and reacted at 140°C for 6 h to obtain a precursor solution of a cerium-based composite catalyst;
[0086] (2) filtering the precursor solution prepared in step (1), washing the filtered solid with water for 4 times, and then drying it in an oven at 120° C. for 10 h to obtain a precursor of a cerium-based composite catalyst;
[0087] (3) The precursor of step (2) is calcined in an air atmosphere at 700° C. for 3 h to obtain the cerium-based composite catalyst.
[0088] The chemical formula of the cerium-based composite catalyst obtained in this embodiment is Mo 0.15 Ce 0.85 O 2.08 , wherein the content of Ce element is 71.5wt%, and the content of transition metal Mo element is 8.6wt%.
[0089] Example 4
[0090] This embodiment provides a method for preparing a cerium-based composite catalyst, the preparation method comprising the following steps:
[0091] (1) 3.0 g Ce(NO3)3·6H2O, 0.022 g VCl3 and 20 mL water were mixed under stirring conditions for 0.5 h to obtain a mixed solution; 10 g sodium hydroxide and 80 mL water were mixed under stirring conditions for 0.5 h to obtain a sodium hydroxide solution, and then a sodium bicarbonate solution was added dropwise to the mixed solution while stirring and aged for 1 h to obtain a reaction slurry; and then the reaction slurry was transferred to a hydrothermal reactor and reacted at 120°C for 24 h to obtain a precursor solution of a cerium-based composite catalyst;
[0092] (2) filtering the precursor solution of step (1), washing the filtered solid with water three times, and then drying it in an oven at 100° C. for 12 h to obtain a precursor of a cerium-based composite catalyst;
[0093] (3) The precursor of step (2) is calcined in an air atmosphere at 500° C. for 3 h to obtain the cerium-based composite catalyst.
[0094] The chemical formula of the cerium-based composite catalyst obtained in this embodiment is V 0.02 Ce 0.98 O 2.01 , wherein the content of Ce element is 80.5wt%, and the content of transition metal V element is 0.6wt%.
[0095] Example 5
[0096] This embodiment provides a method for preparing a cerium-based composite catalyst, the preparation method comprising the following steps:
[0097] (1) 3.0 g CeCl3, 0.27 g Ni(NO3)3·6H2O and 20 mL water were mixed under stirring conditions for 0.5 h to obtain a mixed solution; 10 g sodium hydroxide and 80 mL water were mixed under stirring conditions for 0.5 h to obtain a sodium hydroxide solution, and then a sodium bicarbonate solution was added dropwise to the mixed solution while stirring and aged for 1 h to obtain a reaction slurry; and then the reaction slurry was transferred to a hydrothermal reactor and reacted at 100°C for 32 h to obtain a precursor solution of a cerium-based composite catalyst;
[0098] (2) filtering the precursor solution of step (1), washing the filtered solid with water three times, and then drying it in an oven at 100° C. for 12 h to obtain a precursor of a cerium-based composite catalyst;
[0099] (3) The precursor of step (2) is calcined in an air atmosphere at 600° C. for 3 h to obtain the cerium-based composite catalyst.
[0100] The chemical formula of the cerium-based composite catalyst obtained in this example is Ni 0.12 Ce 0.88 O 1.94 , wherein the content of Ce element in the cerium-based composite catalyst is 76.4wt%, and the content of transition metal Ni element is 4.4wt%.
[0101] Example 6
[0102] This embodiment provides a method for preparing a cerium-based composite catalyst, which is the same as that of Embodiment 1 except that step (1) contains 3.0 g Ce(NO3)3·6H2O and 0.019 g MoCl5, i.e., the molar ratio of Ce(NO3)3·6H2O to MoCl5 is 1:0.01.
[0103] The chemical formula of the cerium-based composite catalyst obtained in this embodiment is Mo 0.01 Ce 0.99 O 2.01 , wherein the content of Ce element is 80.1wt%, and the content of transition metal Mo element is 0.6wt%.
[0104] Example 7
[0105] This embodiment provides a method for preparing a cerium-based composite catalyst, which is the same as that of Embodiment 1 except that step (1) contains 3.0 g Ce(NO3)3·6H2O and 0.472 g MoCl5, i.e., the molar ratio of Ce(NO3)3·6H2O to MoCl5 is 1:0.25.
[0106] The chemical formula of the cerium-based composite catalyst obtained in this embodiment is Mo 0.2 Ce 0.8 O 2.1 , wherein the content of Ce element is 68.0wt%, and the content of transition metal Mo element is 11.6wt%.
[0107] Example 8
[0108] This embodiment provides a method for preparing a cerium-based composite catalyst. Except that the mass of the sodium hydroxide in step (1) is 4.15 g, that is, the molar ratio of Ce(NO3)3·6H2O to sodium hydroxide is 1:15, the rest is the same as that in Example 1.
[0109] The chemical formula of the cerium-based composite catalyst obtained in this example is the same as that of Example 1, but its crystal form has changed, resulting in a decrease in the acidic active sites on its surface and a decrease in catalytic performance.
[0110] Example 9
[0111] This embodiment provides a method for preparing a cerium-based composite catalyst. Except that the mass of the sodium hydroxide in step (1) is 15.2 g, that is, the molar ratio of Ce(NO3)3·6H2O to sodium hydroxide is 1:55, the rest is the same as that in Example 1.
[0112] The chemical formula of the cerium-based composite catalyst obtained in this example is the same as that of Example 1, but due to excessive precipitant, the system is too viscous, the catalyst carries too many impurity ions, and the crystal form of the cerium-based composite catalyst changes, resulting in reduced catalytic activity.
[0113] Example 10
[0114] This embodiment provides a method for preparing a cerium-based composite catalyst, which is the same as that of Embodiment 1 except that the calcination temperature in step (3) is 280°C.
[0115] The chemical formula of the cerium-based composite catalyst obtained in this embodiment is Mo 0.1 Ce 0.9 O 2.05 nH2O, the calcination temperature is too low, resulting in incomplete calcination, and the ideal product and crystal form cannot be obtained, resulting in reduced catalytic performance.
[0116] Embodiment 11
[0117] This embodiment provides a method for preparing a cerium-based composite catalyst, which is the same as that of Embodiment 1 except that the calcination temperature in step (3) is 750° C.
[0118] The chemical formula of the cerium-based composite catalyst obtained in this example is the same as that in Example 1, but the calcination temperature is too high, resulting in sintering of the catalyst, changes in the crystal form, and reduction of its catalytic activity.
[0119] 2. Comparison
[0120] Comparative Example 1
[0121] This comparative example provides a method for preparing a cerium-based composite catalyst, which is the same as Example 1 except that MoCl5 in step (1) is replaced by an equal mass of CuCl2.
[0122] Comparative Example 2
[0123] This comparative example provides a method for preparing a cerium-based composite catalyst, which is the same as Example 1 except that MoCl5 in step (1) is replaced by FeCl3 of an equal mass.
[0124] Comparative Example 3
[0125] This comparative example provides a method for preparing a cerium-based catalyst, which is the same as Example 1 except that MoCl5 is not added in step (1).
[0126] 3. Application Examples
[0127] Application Example 1
[0128] This application example provides a method for preparing methyl phenylcarbamate, comprising the following steps:
[0129] 3 g of diphenylurea, 0.75 g of the cerium-based composite catalyst obtained in Example 1 and 25.5 g of dimethyl carbonate were mixed in a 50 mL reactor, and reacted at 160° C. with magnetic stirring for 2 h. After the reaction was completed, the mixture was cooled to 22° C. and the cerium-based composite catalyst was separated by centrifugation.
[0130] Application Example 2
[0131] This application example provides a method for preparing methyl phenylcarbamate, comprising the following steps:
[0132] 3 g of diphenylurea, 0.15 g of the cerium-based composite catalyst obtained in Example 2 and 5.1 g of dimethyl carbonate were mixed in a 50 mL reactor, and reacted at 120° C. with magnetic stirring for 6 h. After the reaction was completed, the mixture was cooled to 20° C. and the cerium-based composite catalyst was separated by centrifugation.
[0133] Application Example 3
[0134] This application example provides a method for preparing methyl phenylcarbamate, comprising the following steps:
[0135] 3 g of diphenylurea, 1.5 g of the cerium-based composite catalyst obtained in Example 3 and 38.25 g of dimethyl carbonate were mixed in a 50 mL reactor, and reacted at 180° C. with magnetic stirring for 0.5 h. After the reaction was completed, the mixture was cooled to 25° C. and the cerium-based composite catalyst was separated by centrifugation.
[0136] Application Examples 4~11
[0137] The other conditions were kept the same as those in Application Example 1, and only the cerium-based composite catalyst used was changed. Specifically, Application Examples 4 to 11 used the cerium-based composite catalysts prepared in Examples 4 to 11 in sequence.
[0138] Application Example 12
[0139] This application example provides a method for preparing methyl phenylcarbamate, which is the same as that of Application Example 1 except that the mass of the cerium-based composite catalyst is 0.02 g, that is, the mass ratio of the diphenylurea to the cerium-based composite catalyst is 1:0.007.
[0140] Application Example 13
[0141] This application example provides a method for preparing methyl phenylcarbamate, which is the same as that of Application Example 1 except that the mass of the cerium-based composite catalyst is 1.6 g, that is, the mass ratio of the diphenylurea to the cerium-based composite catalyst is 1:0.53.
[0142] 4. Comparative Application Examples
[0143] Comparative application example 1
[0144] This comparative application example provides a method for preparing methyl phenylcarbamate, which is the same as Application Example 1 except that the cerium-based composite catalyst prepared in Example 1 is replaced by the cerium-based composite catalyst prepared in Comparative Example 1.
[0145] Comparative Application Example 2
[0146] This comparative application example provides a method for preparing methyl phenylcarbamate, which is the same as Application Example 1 except that the cerium-based composite catalyst prepared in Example 1 is replaced by the cerium-based composite catalyst prepared in Comparative Example 2.
[0147] Comparative Application Example 3
[0148] This comparative application example provides a method for preparing methyl phenylcarbamate, which is the same as Application Example 1 except that the cerium-based composite catalyst prepared in Example 1 is replaced by the cerium-based composite catalyst prepared in Comparative Example 3.
[0149] V. Test and its results
[0150] The supernatants obtained in the preparation methods of methyl phenylcarbamate provided in the above application examples and comparative application examples were respectively analyzed by liquid chromatography, and the conversion rate of diphenylurea in the first reaction and the yield of MPC were calculated; at the same time, the cerium-based composite catalysts obtained after centrifugation were recovered and used again for the preparation of MPC with reference to the original application examples, and were reused for a total of 5 times, and then the conversion rate of diphenylurea in the fifth reaction and the yield of MPC were calculated; the results are shown in Table 1.
[0151] Table 1
[0152]
[0153] From the data in Table 1, we can see that:
[0154] (1) It can be seen from the comprehensive application examples 1 to 5 that the present invention prepares a cerium-based composite catalyst with high catalytic activity and high stability by selecting a specific cerium element doped with a specific transition metal, which is used to catalyze the coupling reaction of diphenyl urea and dimethyl carbonate to prepare methyl phenylcarbamate, wherein the conversion rate of diphenyl urea in the first reaction is as high as 98.0% or more, and the yield of methyl phenylcarbamate is as high as 96.6% or more; and after the cerium-based composite catalyst is recycled for 5 times, the conversion rate of diphenyl urea in the fifth reaction can still be maintained at more than 98.0%, and the yield of methyl phenylcarbamate can still be maintained at more than 96.5%.
[0155] (2) Comprehensively considering Application Example 1 and Application Examples 6-7, it can be seen that since the cerium-based composite catalysts prepared by Example 6 and Example 7 respectively adopted in Application Example 6 and Application Example 7 have a low or high molar ratio of Ce(NO3)3·6H2O to MoCl5, the transition metal doping effect is not good, thereby reducing the catalytic performance and stability. The conversion rate of diphenylurea in the first reaction decreased to less than 97.8%, and the yield of methyl phenylcarbamate decreased to less than 96.0%. The conversion rate of diphenylurea after the fifth reaction decreased to less than 97.7%, and the yield of methyl phenylcarbamate decreased to less than 95.9%. This shows that the present invention further preferably has a molar ratio of the transition metal source to the cerium source of (0.02-0.15):1, which further improves the catalytic performance and stability of the obtained cerium-based composite catalyst.
[0156] (3) Comprehensively from Application Example 1 and Application Examples 8-9, it can be known that since the molar ratio of Ce(NO3)3·6H2O to sodium hydroxide in the cerium-based composite catalysts prepared in Example 8 and Example 9 respectively used in Application Example 8 and Application Example 9 is low or high, the generation effect of the cerium-based composite catalyst precursor is poor; the crystal form thereof is changed, thereby causing the catalytic performance and stability of the obtained cerium-based composite catalyst to deteriorate, and the conversion rate of diphenyl urea in the catalytic reaction to prepare methyl phenylcarbamate is reduced to less than 96.2%, and the yield of methyl phenylcarbamate is reduced to less than 95.1%; it can be seen that the present invention further preferably has a molar ratio of the precipitant to the cerium source in the range of (20-50):1, which further improves the catalytic performance and stability of the obtained cerium-based composite catalyst.
[0157] (4) It can be seen from Application Example 1 and Application Examples 10-11 that, since the cerium-based composite catalysts prepared by the preparation methods described in Example 10 and Example 11 respectively adopted in Application Example 10 and Application Example 11, the calcination temperature is too low or too high, which leads to a decrease in the catalytic performance and stability of the obtained cerium-based composite catalyst, thereby affecting the preparation of methyl phenylcarbamate. The conversion rate of diphenylurea and the yield of methyl phenylcarbamate are both reduced. Therefore, it can be seen that the present invention further preferably sets the calcination temperature to 300-700°C, which further improves the catalytic performance and stability of the obtained cerium-based composite catalyst.
[0158] (5) From Application Example 1 and Application Examples 12-13, it can be seen that since the amount of cerium-based composite catalyst added in Application Example 12 is relatively small, the catalytic effect is poor, the conversion rate of diphenylurea in the first reaction is only 82.1%, and the yield of methyl phenylcarbamate is only 81.2%. In Application Example 13, a large amount of cerium-based composite catalyst is added, but the catalytic effect is not significantly improved, and resources are wasted.
[0159] (6) It can be seen from the comprehensive application example 1 and comparative application examples 1 to 3 that since the transition metals doped in the cerium-based composite catalysts used in comparative application examples 1 and 2 are Cu and Fe, respectively, they cannot be regulated to obtain suitable acid-base sites; resulting in a very poor catalytic effect on the specific reaction of coupling diphenyl urea and dimethyl carbonate to prepare methyl phenylcarbamate. The conversion rate of diphenyl urea in the first reaction is only less than 72.6%, and the yield of methyl phenylcarbamate is only less than 67.0%. The cerium-based catalyst used in comparative application example 3 is not doped with any transition metal, and its catalytic effect is poor. The conversion rate of diphenyl urea in the first reaction is only 78.0%, and the yield of methyl phenylcarbamate is only 76.0%.
[0160] The applicant declares that the present invention illustrates the technical solution of the present invention through the above specific implementation methods, but the present invention is not limited thereto, that is, it does not mean that the present invention must rely on the above embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
[0161] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0162] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
Claims
1. Application of a cerium-based composite catalyst in the preparation of methyl phenylcarbamate, characterized in that: The preparation method of methyl phenylcarbamate comprises the following steps: mixing diphenyl urea, dimethyl carbonate and a cerium-based composite catalyst to obtain methyl phenylcarbamate through a catalytic reaction; The cerium-based composite catalyst comprises a cerium-based oxide doped with a transition metal; the transition metal comprises any one of Ni, Ti, V, Mo or Nb or a combination of at least two thereof; The cerium-based composite catalyst is a solid solution; The preparation method of the cerium-based composite catalyst comprises the following steps: (1) mixing a cerium source, a transition metal source, a precipitant and a solvent, and reacting to obtain a precursor solution of a cerium-based composite catalyst; (2) subjecting the precursor solution of step (1) to solid-liquid separation to obtain a precursor of a cerium-based composite catalyst; (3) calcining the precursor of step (2) to obtain a cerium-based composite catalyst; The molar ratio of the transition metal source to the cerium source in step (1) is (0.02-0.15):1; the molar ratio of the precipitant to the cerium source in step (1) is (20-50):
1.
2. The use according to claim 1, characterized in that: The chemical formula of the cerium-based composite catalyst is M a Ce 1-a O x , wherein M includes any one of Ni, Ti, V, Mo or Nb or a combination of at least two thereof, 0.02≤a≤0.15, and 1.8≤x≤2.
6.
3. The use according to claim 2, characterized in that: The content of cerium in the cerium-based composite catalyst is 57.4-81.1wt%; The content of transition metal elements in the cerium-based catalyst is 0.24-11.6 wt %.
4. The use according to claim 1, characterized in that: The cerium source in step (1) includes any one of cerium nitrate, cerium chloride, cerium sulfate or cerium acetate, or a combination of at least two thereof; The transition metal source in step (1) includes any one of transition metal chlorides, transition metal nitrates, transition metal sulfates, transition metal acetates or transition metal oxalates, or a combination of at least two thereof; The transition metal includes any one of Ni, Ti, V, Mo or Nb or a combination of at least two thereof; The precipitant in step (1) includes any one of urea, sodium hydroxide, potassium hydroxide, sodium bicarbonate, sodium carbonate, potassium carbonate, potassium bicarbonate or ammonia water, or a combination of at least two thereof; The solvent in step (1) includes any one of water, ethanol, methanol or dimethylformamide, or a combination of at least two of them.
5. The use according to claim 1, characterized in that: The mass volume ratio of the cerium source and the solvent in step (1) is 1:(10-100) g / mL.
6. The use according to claim 1, characterized in that: The reaction temperature in step (1) is 60-140°C; The reaction time of step (1) is 6 to 48 hours; The calcination temperature in step (3) is 300-700°C; The calcination time in step (3) is 3 to 12 h.
7. The use according to claim 1, characterized in that: The molar ratio of diphenylurea to dimethyl carbonate is 1:(1.5-40); The mass ratio of the diphenylurea to the cerium-based composite catalyst is 1:(0.01-0.5).
8. The use according to claim 1, characterized in that: The temperature of the catalytic reaction is 120-180°C; The catalytic reaction time is 0.5 to 6 h.
Citation Information
Patent Citations
Alcohol-lead compound, preparation method thereof and application thereof
CN101665411A
Catalyst for synthesizing phenyl carbamate from diphenyl urea, preparation method and application
CN102513087A
Catalyst for synthesizing methyl phenyl carbamate and preparation and application methods thereof
CN102872912A
Method for cleanly synthesizing phenylamido formate
CN101054351A
Ce-BASED COMPOSITE OXIDE CATALYST, PREPARATION METHOD AND APPLICATION THEREOF
US20130202513A1