A yellowing and aging-resistant PVC film material and its application in the preparation of car cover film

By adding homemade resin and modified fillers to the PVC film, combining physical and chemical mechanisms, the aging problem of PVC film under ultraviolet rays and high temperatures is solved, and the anti-yellowing and anti-aging properties are improved, and the service life of the material is extended And enhances ultraviolet barrier and wear resistance.

CN118562235BActive Publication Date: 2024-11-26FOSHAN TIANJIN PLASTICS
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411036653.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-26
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The commercially available PVC film materials are prone to aging under long-term exposure to ultraviolet rays, high temperatures and other environmental factors, resulting in yellowing, losing transparency and luster, and lacking anti-aging properties, which cannot effectively resist ultraviolet rays, acid rain and other damages, affecting the protection of car paint. Effect.

Method used

A PVC film material is used to improve the comprehensive performance of the material, reduce the influence of ultraviolet rays, and improve durability and wear resistance by adding homemade resin and modified fillers to the PVC powder. The specific method includes reacting dicyclopentadiene, monophenylene cycloolefin and acrylate in a hot polykettle, adding xylene and an inert gas, distilling and removing unreacted substances, forming a homemade resin, and mixing titanium dioxide, diatomaceous earth and dichloride. Materials such as silicon oxide are prepared to prepare modified fillers, and finally undergo hot mixing, cold mixing and cold calendering treatment.

Benefits of technology

It significantly improves the anti-yellowing and anti-aging properties of the film, extends the service life of the material, reduces the tendency of yellowing, enhances the ultraviolet barrier ability and wear resistance, and ensures the long-term protection effect of the car paint.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention provides an anti-yellowing and anti-aging PVC film material and its application in preparing a car cover film. The PVC film material comprises the following raw materials in parts by mass: 100 parts of PVC powder, 16-20 parts of self-made resin, 35-40 parts of DOP plasticizer, 1-5 parts of barium zinc stabilizer, 1-2 parts of ultraviolet absorber, 1-1.5 parts of light stabilizer, 0.2-1 parts of antioxidant and 9-14 parts of modified filler. The present invention adds modified filler and self-made resin to PVC powder, and the addition of modified filler and self-made resin can work together through physical and chemical mechanisms to improve the comprehensive performance of the film material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of film materials, and in particular relates to an anti-yellowing and anti-aging PVC film material and an application thereof in preparing a car cover film. Background Art

[0002] Car film, also known as car protection film, invisible car film or paint protection film, is a transparent polyurethane film that is mainly used to protect the paint surface of the vehicle from scratches, wear, corrosion and UV damage. Car film can enhance the appearance of the vehicle, maintain the feeling of a new car, and at the same time improve the value retention rate of the vehicle to a certain extent. The advantages of car film include: Scratch resistance: It can effectively prevent minor scratches and wear and tear, and protect the original car paint. Self-repair: Some high-end products have thermoplastic memory function and can self-repair some minor scratches. Corrosion resistance: It can resist the erosion of car paint by natural factors such as acid rain, bird droppings, and gum. Anti-ultraviolet: Prevent ultraviolet damage to the car paint and delay the aging of the car paint. Improve brightness: Some products can increase the gloss of the car paint, making the vehicle look brighter.

[0003] Car wraps need to be resistant to yellowing and aging, and are usually made of high-performance polymer materials. However, all polymer materials may undergo an aging process when exposed to UV rays, heat and other environmental factors for a long time, which will cause the material to change color, the most common being yellowing. The purpose of a car wrap is to maintain the appearance and value of the vehicle. If it turns yellow, it will seriously affect the appearance and give the impression that the protection has failed. Yellowing car wraps may mean that its protective layer has been damaged, so it can no longer effectively resist the damage of UV rays, acid rain, bird droppings, etc. to the car paint. Car wraps with strong anti-aging properties can ensure that their physical properties, such as toughness, tensile strength and adhesion, are maintained for a longer period of time, thereby providing continuous protection. Although high-quality car wraps have a higher initial investment, they do not need to be replaced frequently due to their anti-aging ability, so they are more economical in the long run. Vehicles may be driven in a variety of extreme conditions, including hot, cold, wet and dry environments, and anti-aging properties can ensure that the car wrap remains effective under these conditions.

[0004] Commercially available PVC (polyvinyl chloride) film materials have poor anti-yellowing and anti-aging effects when used for car cover films. The main reasons are as follows: UV sensitivity: PVC is sensitive to UV rays. Long-term exposure to sunlight will accelerate the breakage of its molecular chains, leading to material aging, embrittlement and discoloration, especially yellowing. Plasticizer migration: PVC film usually contains a large amount of plasticizers (such as phthalates) to improve its flexibility and processability. However, these plasticizers will gradually migrate out of the material over time, causing the film to harden, become brittle and eventually crack. At the same time, the loss of plasticizers will also accelerate the aging of PVC. Insufficient chemical stability: Compared with other advanced materials such as TPU (thermoplastic polyurethane), PVC has poor chemical stability and is more susceptible to environmental pollutants such as acid rain, bird droppings, and tree sap, resulting in performance degradation and appearance changes. Temperature sensitivity: PVC is not as thermally stable as TPU. It is easy to deform at high temperatures and become hard and brittle at low temperatures, which limits its use under extreme temperature conditions. Lack of self-repairing ability: Advanced materials such as TPU have a certain self-repairing ability, that is, they can recover from minor scratches when heated. PVC film does not have this property and is difficult to recover once damaged. Transparency and gloss retention: PVC film will not only turn yellow during the aging process, but may also lose its original transparency and gloss, affecting the appearance of the vehicle.

[0005] Therefore, there is an urgent need for an anti-yellowing and anti-aging PVC film material and its application in the preparation of car cover film. Summary of the invention

[0006] The purpose of the present invention is to provide a yellowing and aging resistant PVC film material and application thereof in the preparation of car cover film.

[0007] In order to achieve the above object, the present invention provides the following technical solutions:

[0008] An anti-yellowing and anti-aging PVC film material comprises the following raw materials in parts by mass: 100 parts of PVC powder, 16-20 parts of self-made resin, 35-40 parts of DOP plasticizer, 1-5 parts of barium zinc stabilizer, 1-2 parts of ultraviolet absorber, 1-1.5 parts of light stabilizer, 0.2-1 parts of antioxidant and 9-14 parts of modified filler.

[0009] Furthermore, the method for preparing the self-made resin comprises the following steps:

[0010] S1: Weigh the following raw materials in parts by mass: 78-82 parts of dicyclopentadiene, 13-17 parts of monophenyl ring olefin, 11-16 parts of acrylate, and 55-60 parts of xylene;

[0011] S2: adding a certain amount of dicyclopentadiene, monophenyl ring olefin, acrylate and xylene into a hot polymerization kettle, stirring evenly, introducing an inert gas to squeeze out the air in the hot polymerization kettle, maintaining the pressure in the hot polymerization kettle, and heating and stirring to react;

[0012] S3: After the hot polymerization kettle is cooled and depressurized, the materials in the hot polymerization kettle are transferred to a distillation kettle for heating, and unreacted materials are removed by distillation to obtain a self-made resin.

[0013] Furthermore, the monophenyl ring olefin is styrene.

[0014] Furthermore, the acrylate is methyl acrylate.

[0015] Furthermore, the inert gas is nitrogen.

[0016] Furthermore, the heating temperature of step S2 is 210-230° C., the pressure in the hot polymerization reactor of step S1 is 0.6-0.9 MPa, the reaction time is 6-8 h, and the stirring speed is 120-150 r / min.

[0017] Furthermore, the distillation temperature of step S3 is 190-200°C.

[0018] Furthermore, the preparation method of the modified filler is:

[0019] (1) Mixing titanium dioxide, silicon dioxide and diatomaceous earth in a mass ratio of 1:1.3-1.6:0.3-0.8 to obtain a mixed filler;

[0020] (2) Mix a mixed filler in a mass ratio of 1:10-15:0.02-0.04, a 65-75wt% ethanol aqueous solution, and a silane coupling agent KH570, stir and react at 60-65°C for 3-4h, filter and obtain a solid, wash and dry it, and obtain a modified filler.

[0021] Furthermore, the particle size of the titanium dioxide is 30-80 nm, the particle size of the silicon dioxide is 100-200 nm, and the particle size of the diatomaceous earth is 200-300 meshes.

[0022] Furthermore, the preparation method of the anti-yellowing and anti-aging PVC film material is:

[0023] S1, weigh the above raw materials according to the proportion, put them into a high-speed mixer for hot mixing;

[0024] S2, performing secondary cold mixing on the mixed raw materials;

[0025] S3, putting the cold mixed raw materials into a mixing extruder for mixing;

[0026] S4. The mixed product is conveyed to a five-roll calender through a pulley for layer-by-layer calendering and shaping. Cold calendering is adopted, and the temperature between each roller is 35-40℃;

[0027] S5, peeling off and air-cooling the calendered film to obtain an anti-yellowing and anti-aging PVC film material.

[0028] The invention provides application of the anti-yellowing and anti-aging PVC film material in preparing a car cover film.

[0029] Compared with the prior art, the advantages and beneficial effects of the present invention are as follows: the present invention adds modified fillers and self-made resins to PVC powder, and the addition of modified fillers and self-made resins can work together through physical and chemical mechanisms to improve the comprehensive performance of the film material. The self-made resin can provide chemical stability, reduce the degradation of PVC under the action of heat and light, thereby improving aging resistance, can be better compatible with the PVC matrix, form a more stable mixed system, reduce stress concentration inside the material, and improve overall durability. The various components in the film material work together to absorb or scatter ultraviolet rays, reduce their impact on PVC, and thus reduce the tendency to yellowing. The modified filler through surface treatment has better dispersibility, which helps to improve the compatibility and bonding between the filler and the system components, reduce the formation of microcracks, and thus improve the aging resistance and wear resistance of the material. DETAILED DESCRIPTION

[0030] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Some of the raw materials of the present invention are purchased from the following manufacturers:

[0032] DOP plasticizer (dioctyl phthalate): Jiangsu Yangnong Jinhu Chemical Co., Ltd.

[0033] Barium zinc composite stabilizer, model: HZ-2000. Manufacturer: Suzhou Polyplastics Co., Ltd.

[0034] UV absorber, model: Tinuvin 328. Manufacturer: BASF.

[0035] Light stabilizer, model: Chimassorb 944, manufacturer: BASF.

[0036] Antioxidant, model: Antioxidant 1010. Manufacturer: BASF.

[0037] Example 1

[0038] The present embodiment provides an anti-yellowing and anti-aging PVC film material, comprising the following raw materials in parts by mass: 100 parts of PVC powder, 18 parts of homemade resin, 38 parts of DOP plasticizer, 3 parts of barium zinc stabilizer, 1.4 parts of ultraviolet absorber, 1.2 parts of light stabilizer, 0.6 parts of antioxidant and 12 parts of modified filler.

[0039] The method for preparing the self-made resin comprises the following steps:

[0040] S1: Weigh the following raw materials in parts by mass: 80 parts of dicyclopentadiene, 15 parts of monophenyl ring olefin, 13 parts of acrylate, and 58 parts of xylene;

[0041] S2: adding a certain amount of dicyclopentadiene, monophenyl ring olefin, acrylate and xylene into a hot polymerization kettle, stirring evenly, introducing an inert gas to squeeze out the air in the hot polymerization kettle, maintaining the pressure in the hot polymerization kettle, and heating and stirring to react;

[0042] S3: After the hot polymerization kettle is cooled and depressurized, the materials in the hot polymerization kettle are transferred to a distillation kettle for heating, and unreacted materials are removed by distillation to obtain a self-made resin.

[0043] The monophenyl ring olefin is styrene.

[0044] The acrylic acid ester is methyl acrylate.

[0045] The inert gas is nitrogen.

[0046] The heating temperature of step S2 is 220° C., the pressure in the hot polymerization reactor of step S1 is 0.7 MPa, the reaction time is 7 h, and the stirring speed is 140 r / min.

[0047] The distillation temperature of step S3 is 195°C.

[0048] The preparation method of the modified filler is:

[0049] (1) titanium dioxide, silicon dioxide and diatomaceous earth are mixed in a mass ratio of 1:1.5:0.6 to obtain a mixed filler;

[0050] (2) A mixed filler with a mass ratio of 1:12:0.03, a 70 wt % ethanol aqueous solution, and a silane coupling agent KH570 were mixed, stirred at 62° C. for 3.5 h, and the solid was filtered, washed, and dried to obtain a modified filler.

[0051] The particle size of the titanium dioxide is 30-80 nm, the particle size of the silicon dioxide is 100-200 nm, and the particle size of the diatomite is 200-300 mesh. Titanium dioxide was purchased from Jiangsu Hushen Titanium Dioxide Technology Co., Ltd. Silicon dioxide was purchased from Hubei Huifu Nanomaterial Co., Ltd. Diatomite was purchased from Yixing Junlian Diatomite Co., Ltd.

[0052] The preparation method of the anti-yellowing and anti-aging PVC film material is as follows:

[0053] S1, weigh the above raw materials according to the proportion, put them into a high-speed mixer for hot mixing;

[0054] S2, performing secondary cold mixing on the mixed raw materials;

[0055] S3, putting the cold mixed raw materials into a mixing extruder for mixing;

[0056] S4, the mixed product is conveyed to a five-roll calender through a pulley, and is calendered layer by layer to shape it. Cold calendering is adopted, and the temperature between each roller is 37°C;

[0057] S5, peeling off and air-cooling the calendered film to obtain an anti-yellowing and anti-aging PVC film material.

[0058] Example 2

[0059] The present embodiment provides an anti-yellowing and anti-aging PVC film material, comprising the following raw materials in parts by weight: 100 parts of PVC powder, 16 parts of homemade resin, 40 parts of DOP plasticizer, 1 part of barium zinc stabilizer, 2 parts of ultraviolet absorber, 1 part of light stabilizer, 1 part of antioxidant and 9 parts of modified filler.

[0060] The method for preparing the self-made resin comprises the following steps:

[0061] S1: Weigh the following raw materials in parts by mass: 78 parts of dicyclopentadiene, 17 parts of monophenyl ring olefin, 11 parts of acrylate, and 60 parts of xylene;

[0062] S2: adding a certain amount of dicyclopentadiene, monophenyl ring olefin, acrylate and xylene into a hot polymerization kettle, stirring evenly, introducing an inert gas to squeeze out the air in the hot polymerization kettle, maintaining the pressure in the hot polymerization kettle, and heating and stirring to react;

[0063] S3: After the hot polymerization kettle is cooled and depressurized, the materials in the hot polymerization kettle are transferred to a distillation kettle for heating, and unreacted materials are removed by distillation to obtain a self-made resin.

[0064] The monophenyl ring olefin is styrene.

[0065] The acrylic acid ester is methyl acrylate.

[0066] The inert gas is nitrogen.

[0067] The heating temperature of step S2 is 210° C., the pressure in the hot polymerization reactor of step S1 is 0.9 MPa, the reaction time is 6 h, and the stirring speed is 150 r / min.

[0068] The distillation temperature in step S3 is 190°C.

[0069] The preparation method of the modified filler is:

[0070] (1) titanium dioxide, silicon dioxide and diatomaceous earth are mixed in a mass ratio of 1:1.6:0.3 to obtain a mixed filler;

[0071] (2) A mixed filler with a mass ratio of 1:15:0.02, a 75 wt% ethanol aqueous solution, and a silane coupling agent KH570 were mixed, stirred at 60°C for 4 hours, and the solid was filtered, washed, and dried to obtain a modified filler.

[0072] The particle size of the titanium dioxide is 30-80 nm, the particle size of the silicon dioxide is 100-200 nm, and the particle size of the diatomite is 200-300 mesh. Titanium dioxide was purchased from Jiangsu Hushen Titanium Dioxide Technology Co., Ltd. Silicon dioxide was purchased from Hubei Huifu Nanomaterial Co., Ltd. Diatomite was purchased from Yixing Junlian Diatomite Co., Ltd.

[0073] The preparation method of the anti-yellowing and anti-aging PVC film material is as follows:

[0074] S1, weigh the above raw materials according to the proportion, put them into a high-speed mixer for hot mixing;

[0075] S2, performing secondary cold mixing on the mixed raw materials;

[0076] S3, putting the cold mixed raw materials into a mixing extruder for mixing;

[0077] S4, the mixed product is conveyed to a five-roll calender through a pulley, and is calendered layer by layer for shaping. Cold calendering is adopted, and the temperature between each roller is 35°C;

[0078] S5, peeling off and air-cooling the calendered film to obtain an anti-yellowing and anti-aging PVC film material.

[0079] Example 3

[0080] The present embodiment provides an anti-yellowing and anti-aging PVC film material, comprising the following raw materials in parts by weight: 100 parts of PVC powder, 20 parts of homemade resin, 35 parts of DOP plasticizer, 5 parts of barium zinc stabilizer, 1 part of ultraviolet absorber, 1.5 parts of light stabilizer, 0.2 parts of antioxidant and 14 parts of modified filler.

[0081] The method for preparing the self-made resin comprises the following steps:

[0082] S1: Weigh the following raw materials in parts by mass: 78 parts of dicyclopentadiene, 17 parts of monophenyl ring olefin, 11 parts of acrylate, and 60 parts of xylene;

[0083] S2: adding a certain amount of dicyclopentadiene, monophenyl ring olefin, acrylate and xylene into a hot polymerization kettle, stirring evenly, introducing an inert gas to squeeze out the air in the hot polymerization kettle, maintaining the pressure in the hot polymerization kettle, and heating and stirring to react;

[0084] S3: After the hot polymerization kettle is cooled and depressurized, the materials in the hot polymerization kettle are transferred to a distillation kettle for heating, and unreacted materials are removed by distillation to obtain a self-made resin.

[0085] The monophenyl ring olefin is styrene.

[0086] The acrylic acid ester is methyl acrylate.

[0087] The inert gas is nitrogen.

[0088] The heating temperature of step S2 is 210° C., the pressure in the hot polymerization reactor of step S1 is 0.9 MPa, the reaction time is 6 h, and the stirring speed is 150 r / min.

[0089] The distillation temperature in step S3 is 190°C.

[0090] The preparation method of the modified filler is:

[0091] (1) titanium dioxide, silicon dioxide and diatomaceous earth are mixed in a mass ratio of 1:1.6:0.3 to obtain a mixed filler;

[0092] (2) A mixed filler with a mass ratio of 1:15:0.02, a 75 wt% ethanol aqueous solution, and a silane coupling agent KH570 were mixed, stirred at 60°C for 4 hours, and the solid was filtered, washed, and dried to obtain a modified filler.

[0093] The particle size of the titanium dioxide is 30-80 nm, the particle size of the silicon dioxide is 100-200 nm, and the particle size of the diatomite is 200-300 mesh. Titanium dioxide was purchased from Jiangsu Hushen Titanium Dioxide Technology Co., Ltd. Silicon dioxide was purchased from Hubei Huifu Nanomaterial Co., Ltd. Diatomite was purchased from Yixing Junlian Diatomite Co., Ltd.

[0094] The preparation method of the anti-yellowing and anti-aging PVC film material is as follows:

[0095] S1, weigh the above raw materials according to the proportion, put them into a high-speed mixer for hot mixing;

[0096] S2, performing secondary cold mixing on the mixed raw materials;

[0097] S3, putting the cold mixed raw materials into a mixing extruder for mixing;

[0098] S4, the mixed product is conveyed to a five-roll calender through a pulley, and is calendered layer by layer for shaping. Cold calendering is adopted, and the temperature between each roller is 35°C;

[0099] S5, peeling off and air-cooling the calendered film to obtain an anti-yellowing and anti-aging PVC film material.

[0100] Comparative Example 1

[0101] The difference between this comparative example and Example 1 is that the added amounts of the homemade resin and the modified filler are different.

[0102] A yellowing and aging-resistant PVC film material comprises the following raw materials in parts by mass: 100 parts of PVC powder, 13 parts of self-made resin, 38 parts of DOP plasticizer, 3 parts of barium zinc stabilizer, 1.4 parts of ultraviolet absorber, 1.2 parts of light stabilizer, 0.6 parts of antioxidant and 17 parts of modified filler.

[0103] The method for preparing the self-made resin comprises the following steps:

[0104] S1: Weigh the following raw materials in parts by mass: 80 parts of dicyclopentadiene, 15 parts of monophenyl ring olefin, 13 parts of acrylate, and 58 parts of xylene;

[0105] S2: adding a certain amount of dicyclopentadiene, monophenyl ring olefin, acrylate and xylene into a hot polymerization kettle, stirring evenly, introducing an inert gas to squeeze out the air in the hot polymerization kettle, maintaining the pressure in the hot polymerization kettle, and heating and stirring to react;

[0106] S3: After the hot polymerization kettle is cooled and depressurized, the materials in the hot polymerization kettle are transferred to a distillation kettle for heating, and unreacted materials are removed by distillation to obtain a self-made resin.

[0107] The monophenyl ring olefin is styrene.

[0108] The acrylic acid ester is methyl acrylate.

[0109] The inert gas is nitrogen.

[0110] The heating temperature of step S2 is 220° C., the pressure in the hot polymerization reactor of step S1 is 0.7 MPa, the reaction time is 7 h, and the stirring speed is 140 r / min.

[0111] The distillation temperature of step S3 is 195°C.

[0112] The preparation method of the modified filler is:

[0113] (1) titanium dioxide, silicon dioxide and diatomaceous earth are mixed in a mass ratio of 1:1.5:0.6 to obtain a mixed filler;

[0114] (2) A mixed filler with a mass ratio of 1:12:0.03, a 70 wt % ethanol aqueous solution, and a silane coupling agent KH570 were mixed, stirred at 62° C. for 3.5 h, and the solid was filtered, washed, and dried to obtain a modified filler.

[0115] The particle size of the titanium dioxide is 30-80 nm, the particle size of the silicon dioxide is 100-200 nm, and the particle size of the diatomite is 200-300 mesh. Titanium dioxide was purchased from Jiangsu Hushen Titanium Dioxide Technology Co., Ltd. Silicon dioxide was purchased from Hubei Huifu Nanomaterial Co., Ltd. Diatomite was purchased from Yixing Junlian Diatomite Co., Ltd.

[0116] The preparation method of the anti-yellowing and anti-aging PVC film material is as follows:

[0117] S1, weigh the above raw materials according to the proportion, put them into a high-speed mixer for hot mixing;

[0118] S2, performing secondary cold mixing on the mixed raw materials;

[0119] S3, putting the cold mixed raw materials into a mixing extruder for mixing;

[0120] S4, the mixed product is conveyed to a five-roll calender through a pulley, and is calendered layer by layer to shape it. Cold calendering is adopted, and the temperature between each roller is 37°C;

[0121] S5, peeling off and air-cooling the calendered film to obtain an anti-yellowing and anti-aging PVC film material.

[0122] Comparative Example 2

[0123] The difference between this comparative example and Example 1 is that the added amounts of the homemade resin and the modified filler are different.

[0124] An anti-yellowing and anti-aging PVC film material comprises the following raw materials in parts by mass: 100 parts of PVC powder, 23 parts of self-made resin, 38 parts of DOP plasticizer, 3 parts of barium zinc stabilizer, 1.4 parts of ultraviolet absorber, 1.2 parts of light stabilizer, 0.6 parts of antioxidant and 5 parts of modified filler.

[0125] The method for preparing the self-made resin comprises the following steps:

[0126] S1: Weigh the following raw materials in parts by mass: 80 parts of dicyclopentadiene, 15 parts of monophenyl ring olefin, 13 parts of acrylate, and 58 parts of xylene;

[0127] S2: adding a certain amount of dicyclopentadiene, monophenyl ring olefin, acrylate and xylene into a hot polymerization kettle, stirring evenly, introducing an inert gas to squeeze out the air in the hot polymerization kettle, maintaining the pressure in the hot polymerization kettle, and heating and stirring to react;

[0128] S3: After the hot polymerization kettle is cooled and depressurized, the materials in the hot polymerization kettle are transferred to a distillation kettle for heating, and unreacted materials are removed by distillation to obtain a self-made resin.

[0129] The monophenyl ring olefin is styrene.

[0130] The acrylic acid ester is methyl acrylate.

[0131] The inert gas is nitrogen.

[0132] The heating temperature of step S2 is 220° C., the pressure in the hot polymerization reactor of step S1 is 0.7 MPa, the reaction time is 7 h, and the stirring speed is 140 r / min.

[0133] The distillation temperature of step S3 is 195°C.

[0134] The preparation method of the modified filler is:

[0135] (1) titanium dioxide, silicon dioxide and diatomaceous earth are mixed in a mass ratio of 1:1.5:0.6 to obtain a mixed filler;

[0136] (2) A mixed filler with a mass ratio of 1:12:0.03, a 70 wt % ethanol aqueous solution, and a silane coupling agent KH570 were mixed, stirred at 62° C. for 3.5 h, and the solid was filtered, washed, and dried to obtain a modified filler.

[0137] The particle size of the titanium dioxide is 30-80 nm, the particle size of the silicon dioxide is 100-200 nm, and the particle size of the diatomite is 200-300 mesh. Titanium dioxide was purchased from Jiangsu Hushen Titanium Dioxide Technology Co., Ltd. Silicon dioxide was purchased from Hubei Huifu Nanomaterial Co., Ltd. Diatomite was purchased from Yixing Junlian Diatomite Co., Ltd.

[0138] The preparation method of the anti-yellowing and anti-aging PVC film material is as follows:

[0139] S1, weigh the above raw materials according to the proportion, put them into a high-speed mixer for hot mixing;

[0140] S2, performing secondary cold mixing on the mixed raw materials;

[0141] S3, putting the cold mixed raw materials into a mixing extruder for mixing;

[0142] S4, the mixed product is conveyed to a five-roll calender through a pulley, and is calendered layer by layer to shape it. Cold calendering is adopted, and the temperature between each roller is 37°C;

[0143] S5, peeling off and air-cooling the calendered film to obtain an anti-yellowing and anti-aging PVC film material.

[0144] Comparative Example 3

[0145] The difference between this comparative example and Example 1 is that the mass ratio of titanium dioxide, silicon dioxide and diatomaceous earth is 1:1:1.

[0146] A yellowing and aging-resistant PVC film material comprises the following raw materials in parts by mass: 100 parts of PVC powder, 18 parts of self-made resin, 38 parts of DOP plasticizer, 3 parts of barium zinc stabilizer, 1.4 parts of ultraviolet absorber, 1.2 parts of light stabilizer, 0.6 parts of antioxidant and 12 parts of modified filler.

[0147] The method for preparing the self-made resin comprises the following steps:

[0148] S1: Weigh the following raw materials in parts by mass: 80 parts of dicyclopentadiene, 15 parts of monophenyl ring olefin, 13 parts of acrylate, and 58 parts of xylene;

[0149] S2: adding a certain amount of dicyclopentadiene, monophenyl ring olefin, acrylate and xylene into a hot polymerization kettle, stirring evenly, introducing an inert gas to squeeze out the air in the hot polymerization kettle, maintaining the pressure in the hot polymerization kettle, and heating and stirring to react;

[0150] S3: After the hot polymerization kettle is cooled and depressurized, the materials in the hot polymerization kettle are transferred to a distillation kettle for heating, and unreacted materials are removed by distillation to obtain a self-made resin.

[0151] The monophenyl ring olefin is styrene.

[0152] The acrylic acid ester is methyl acrylate.

[0153] The inert gas is nitrogen.

[0154] The heating temperature of step S2 is 220° C., the pressure in the hot polymerization reactor of step S1 is 0.7 MPa, the reaction time is 7 h, and the stirring speed is 140 r / min.

[0155] The distillation temperature of step S3 is 195°C.

[0156] The preparation method of the modified filler is:

[0157] (1) mixing titanium dioxide, silicon dioxide and diatomaceous earth in a mass ratio of 1:1:1 to obtain a mixed filler;

[0158] (2) A mixed filler with a mass ratio of 1:12:0.03, a 70 wt % ethanol aqueous solution, and a silane coupling agent KH570 were mixed, stirred at 62° C. for 3.5 h, and the solid was filtered, washed, and dried to obtain a modified filler.

[0159] The particle size of the titanium dioxide is 30-80 nm, the particle size of the silicon dioxide is 100-200 nm, and the particle size of the diatomite is 200-300 mesh. Titanium dioxide was purchased from Jiangsu Hushen Titanium Dioxide Technology Co., Ltd. Silicon dioxide was purchased from Hubei Huifu Nanomaterial Co., Ltd. Diatomite was purchased from Yixing Junlian Diatomite Co., Ltd.

[0160] The preparation method of the anti-yellowing and anti-aging PVC film material is as follows:

[0161] S1, weigh the above raw materials according to the proportion, put them into a high-speed mixer for hot mixing;

[0162] S2, performing secondary cold mixing on the mixed raw materials;

[0163] S3, putting the cold mixed raw materials into a mixing extruder for mixing;

[0164] S4, the mixed product is conveyed to a five-roll calender through a pulley, and is calendered layer by layer to shape it. Cold calendering is adopted, and the temperature between each roller is 37°C;

[0165] S5, peeling off and air-cooling the calendered film to obtain an anti-yellowing and anti-aging PVC film material.

[0166] Comparative Example 4

[0167] The difference between this comparative example and Example 1 is that the particle size of the titanium dioxide is 300-500 nm, the particle size of the silicon dioxide is 10-50 nm, and the particle size of the diatomaceous earth is 100-200 mesh.

[0168] A yellowing and aging-resistant PVC film material comprises the following raw materials in parts by mass: 100 parts of PVC powder, 18 parts of self-made resin, 38 parts of DOP plasticizer, 3 parts of barium zinc stabilizer, 1.4 parts of ultraviolet absorber, 1.2 parts of light stabilizer, 0.6 parts of antioxidant and 12 parts of modified filler.

[0169] The method for preparing the self-made resin comprises the following steps:

[0170] S1: Weigh the following raw materials in parts by mass: 80 parts of dicyclopentadiene, 15 parts of monophenyl ring olefin, 13 parts of acrylate, and 58 parts of xylene;

[0171] S2: adding a certain amount of dicyclopentadiene, monophenyl ring olefin, acrylate and xylene into a hot polymerization kettle, stirring evenly, introducing an inert gas to squeeze out the air in the hot polymerization kettle, maintaining the pressure in the hot polymerization kettle, and heating and stirring to react;

[0172] S3: After the hot polymerization kettle is cooled and depressurized, the materials in the hot polymerization kettle are transferred to a distillation kettle for heating, and unreacted materials are removed by distillation to obtain a self-made resin.

[0173] The monophenyl ring olefin is styrene.

[0174] The acrylic acid ester is methyl acrylate.

[0175] The inert gas is nitrogen.

[0176] The heating temperature of step S2 is 220° C., the pressure in the hot polymerization reactor of step S1 is 0.7 MPa, the reaction time is 7 h, and the stirring speed is 140 r / min.

[0177] The distillation temperature of step S3 is 195°C.

[0178] The preparation method of the modified filler is:

[0179] (1) titanium dioxide, silicon dioxide and diatomaceous earth are mixed in a mass ratio of 1:1.5:0.6 to obtain a mixed filler;

[0180] (2) A mixed filler with a mass ratio of 1:12:0.03, a 70 wt % ethanol aqueous solution, and a silane coupling agent KH570 were mixed, stirred at 62° C. for 3.5 h, and the solid was filtered, washed, and dried to obtain a modified filler.

[0181] The particle size of the titanium dioxide is 300-500 nm, the particle size of the silicon dioxide is 10-50 nm, and the particle size of the diatomite is 100-200 mesh. Titanium dioxide was purchased from Jiangsu Hushen Titanium Dioxide Technology Co., Ltd. Silicon dioxide was purchased from Hubei Huifu Nanomaterial Co., Ltd. Diatomite was purchased from Yixing Junlian Diatomite Co., Ltd.

[0182] The preparation method of the anti-yellowing and anti-aging PVC film material is as follows:

[0183] S1, weigh the above raw materials according to the proportion, put them into a high-speed mixer for hot mixing;

[0184] S2, performing secondary cold mixing on the mixed raw materials;

[0185] S3, putting the cold mixed raw materials into a mixing extruder for mixing;

[0186] S4, the mixed product is conveyed to a five-roll calender through a pulley, and is calendered layer by layer to shape it. Cold calendering is adopted, and the temperature between each roller is 37°C;

[0187] S5, peeling off and air-cooling the calendered film to obtain an anti-yellowing and anti-aging PVC film material.

[0188] Performance Testing

[0189] The products of Examples 1-3 and Comparative Examples 1-4 were subjected to performance tests.

[0190] The wear rate test standard is to rub the surface of the PVC film with a clean, dry cheese cloth plate that meets the CCC-C-440 standard. The Knoop hardness applied to the base material is less than 450 / mm2, and there is no obvious damage to the film.

[0191] The test method for the UV blocking rate is to directly irradiate the test light onto the PVC film, and then measure it under the PVC film using a UV blocking rate tester.

[0192] With reference to GB / T 2409-1980 “Test method for yellowness index of plastics”, the yellowness index of PVC film after 90 days was measured with a colorimeter.

[0193] Cut each PVC film into the same size (50cm 50cm) squares, the cut films were pasted on the cars under the same conditions, and according to the method specified in the national standard (GB / T3978-94): the films were evenly irradiated under the same light, humidity and other environments, and the anti-aging strength of the anti-aging film of the anti-aging coating for 3000h (the color difference between 0h and 3000h) was detected.

[0194] Table 1 Performance test results

[0195]

[0196] It can be seen from the above performance test results that the comprehensive performance of Examples 1-3 is the most outstanding. In Comparative Examples 1-2, the addition amount of the homemade resin and the modified filler was changed, and in Comparative Examples 3-4, the mass ratio and particle size of titanium dioxide, silicon dioxide and diatomaceous earth were changed. Because the necessary technical solutions were not adopted, the wear rate, UV blocking rate, anti-yellowing and anti-aging properties were significantly worse than those of the examples. The above experimental results further prove the importance of the technical solutions defined in the present invention for its technical effects.

[0197] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. An anti-yellowing and anti-aging PVC film material, characterized in that: The invention comprises the following raw materials in parts by weight: 100 parts of PVC powder, 16-20 parts of self-made resin, 35-40 parts of DOP plasticizer, 1-5 parts of barium zinc stabilizer, 1-2 parts of ultraviolet absorber, 1-1.5 parts of light stabilizer, 0.2-1 parts of antioxidant and 9-14 parts of modified filler; the preparation method of the self-made resin comprises the following steps: S1: Weigh the following raw materials in parts by mass: 78-82 parts of dicyclopentadiene, 13-17 parts of monophenyl ring olefin, 11-16 parts of acrylate, and 55-60 parts of xylene; S2: adding a certain amount of dicyclopentadiene, monophenyl ring olefin, acrylate and xylene into a hot polymerization kettle, stirring evenly, introducing an inert gas to squeeze out the air in the hot polymerization kettle, maintaining the pressure in the hot polymerization kettle, and heating and stirring to react; S3: After the hot polymerization kettle is cooled and depressurized, the materials in the hot polymerization kettle are transferred to a distillation kettle for heating, and unreacted materials are removed by distillation to obtain a self-made resin; the preparation method of the modified filler is: (1) Mix titanium dioxide, silicon dioxide and diatomaceous earth in a mass ratio of 1:1.3-1.6:0.3-0.8 to obtain a mixed filler; (2) Mix a mixed filler in a mass ratio of 1:10-15:0.02-0.04, a 65-75wt% ethanol aqueous solution, and a silane coupling agent KH570, stir and react at 60-65°C for 3-4h, filter the solid, wash and dry it to obtain a modified filler; the particle size of the titanium dioxide is 30-80nm, the particle size of the silicon dioxide is 100-200nm, and the particle size of the diatomaceous earth is 200-300 mesh.

2. The anti-yellowing and anti-aging PVC film material according to claim 1, characterized in that: The monophenyl ring olefin is styrene.

3. The anti-yellowing and anti-aging PVC film material according to claim 1, characterized in that: The acrylic acid ester is methyl acrylate.

4. The anti-yellowing and anti-aging PVC film material according to claim 1, characterized in that: The heating temperature of step S2 is 210-230° C., the pressure in the hot polymerization reactor of step S2 is 0.6-0.9 MPa, the reaction time is 6-8 hours, and the stirring speed is 120-150 r / min.

5. The anti-yellowing and anti-aging PVC film material according to claim 1, characterized in that: The distillation temperature of step S3 is 190-200°C.

6. The anti-yellowing and anti-aging PVC film material according to claim 1, characterized in that: The preparation method of the anti-yellowing and anti-aging PVC film material is as follows: S1, weigh the above raw materials according to the proportion, put them into a high-speed mixer for hot mixing; S2, performing secondary cold mixing on the mixed raw materials; S3, putting the cold mixed raw materials into a mixing extruder for mixing; S4. The mixed product is conveyed to a five-roll calender through a pulley for layer-by-layer calendering and shaping. Cold calendering is adopted, and the temperature between each roller is 35-40℃; S5, peeling off and air-cooling the calendered film to obtain an anti-yellowing and anti-aging PVC film material.

7. Use of the anti-yellowing and anti-aging PVC film material according to any one of claims 1 to 6 in the preparation of car cover films.

Citation Information

Patent Citations

  • Anti-yellowing and anti-ultraviolet car cover film

    CN110467785A

  • PVC plate and manufacturing method thereof

    CN113861584A

  • Polyolefin-based polymer alloy

    JP1994340781A

  • Polyvinyl chloride resin sheets for flooring