A pressure-resistant shell polymer material for LED lamp and preparation method thereof
Through the use of composite modified fillers and modified resins, the heat conductivity, heat dissipation, waterproofing, aging resistance and pressure resistance of LED lamp shell materials are improved, and the performance degradation of existing materials under external forces is solved and the service life is extended.
Patent Information
- Application Number
- CN202411046407.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-01
AI Technical Summary
While improving the thermal conductivity and heat dissipation performance, the shell materials of existing LED lamps ignore waterproofing, aging resistance and mechanical properties, resulting in reduced performance under external forces and shortened service life.
Using composite modified fillers and modified resins, the hydrogen bonding and connection effect are enhanced through the three-dimensional composite of frame particles, nanoparticles and chopped fibers, forming a carbon fiber support, improving the waterproof, aging resistance and mechanical properties of the material, and through modification Chemical hydrogen bonding and long molecular chain guidance of the elastic resin enhance the structural strength and ductility of the material.
It realizes excellent thermal conductivity, waterproofness, aging resistance and pressure resistance of LED lamp housing materials, extends service life and improves the overall performance of the material.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to the field of polymer materials, and in particular to a pressure-resistant shell polymer material for an LED lamp and a preparation method thereof. Background Art
[0002] LED (Light Emitting Diode) lamps are rapidly gaining popularity around the world due to their high efficiency, long life, and environmental protection, and are gradually replacing traditional lighting sources. The core of LED lamps is the LED chip, but its performance and service life depend largely on the design of the lamp, especially the choice of shell material.
[0003] LED lamps generate heat when working. If it is not dissipated in time, it will cause the LED chip to overheat, thereby reducing the luminous efficiency and shortening the service life. Therefore, the shell material of LED lamps not only needs to have good mechanical properties, weather resistance and electrical insulation properties, but also needs to have excellent thermal conductivity to help dissipate heat. At the same time, LED lamps will be subjected to different degrees of external forces, such as pressure or tensile force, in different application fields and application environments. Therefore, how to ensure that LED lamps can withstand a certain degree of external forces when in use and maintain good product form and performance.
[0004] However, the selection of existing LED lamp shell materials focuses more on improving the thermal conductivity and heat dissipation performance, while ignoring some other properties, such as the waterproof performance, aging resistance and mechanical properties of the shell material. Especially after the addition of thermal conductive materials, the mechanical properties of the shell material are greatly affected, which usually leads to a decrease in the material's pressure resistance, tensile resistance and cracking resistance. Therefore, in order to effectively solve the above problems, the present application provides a pressure-resistant shell polymer material for LED lamps and a preparation method thereof. The pressure-resistant shell polymer material for LED lamps prepared by the present application not only has excellent thermal conductivity and heat dissipation performance, but also can maintain excellent shell material waterproofness, aging resistance and pressure resistance and other mechanical properties, effectively avoiding the technical problems existing in existing LED shell polymer materials, and has very excellent market application value. Summary of the invention
[0005] In order to solve the above problems, the first aspect of the present application provides a pressure-resistant shell polymer material for LED lamps. The raw materials are, by mass: 90 to 130 parts of polyamide material, 20 to 30 parts of epoxy block resin, 20 to 40 parts of composite modified filler, 10 to 25 parts of modified resin, 2 to 4 parts of antioxidant, 5 to 15 parts of plasticizer, 5 to 10 parts of dispersant, and 5 to 15 parts of additives.
[0006] As a preferred solution, the mass ratio of the polyamide material, the composite modified filler and the modified resin is (9.5-12): (2.5-3.5): (1.5-2.5).
[0007] As a preferred solution, the mass ratio of the polyamide material, the composite modified filler and the modified resin is (10-11.5): (2.5-3): (1.5-2).
[0008] As a preferred solution, the mass ratio of the polyamide material, epoxy block resin and additive is (9.5-12): (2-2.5): (1-1.5).
[0009] As a preferred solution, the mass ratio of the polyamide material, epoxy block resin and additive is (10-11.5): (2.2-2.5): (1-1.2).
[0010] As a preferred solution, the glass fiber content of the polyamide material is 15-35wt%.
[0011] As a preferred solution, the glass fiber content of the polyamide material is 20-30wt%.
[0012] As a preferred solution, the epoxy block resin is a block copolymer resin of ethylene oxide and propylene oxide.
[0013] As a preferred solution, the weight average molecular weight of the epoxy block resin is 4000-8000.
[0014] As a preferred solution, the weight average molecular weight of the epoxy block resin is 4000-6000.
[0015] As a preferred solution, the preparation method of the composite modified filler comprises the following steps: S1: adding aluminum nitrate and acetic acid to deionized water and stirring at room temperature, then adding them to a closed reactor, gradually heating the temperature to 200-210°C at a heating rate of 2°C / min, and controlling the pressure in the reactor to be 2.0-2.4MPa, during which a deionized water solution containing terephthalic acid is added dropwise, and the dropping temperature range is 40-120°C. After the heating is completed, the reaction is stirred continuously for 8-10 hours, and the product is washed. Filtration and drying; S2: The S1 product, alumina and chopped carbon fibers are mixed and ultrasonically dispersed in a DMF solution, and then succinic anhydride and 3-aminopropyltriethoxysilane are added, and the temperature is raised to 60-70°C and kept for reaction for 3-4 hours, and then the temperature is continued to be kept for ultrasonic oscillation at a power of 300-500W for 4-5 hours; S3: After the oscillation is completed, citric acid, ethanol and dicyclopentadiene are added and the temperature is raised to 75-85°C and the reaction is continued with stirring for 6-8 hours. The product is centrifuged and filtered, and then washed and dried to obtain the product.
[0016] As a preferred solution, the mass ratio of aluminum nitrate, acetic acid and terephthalic acid is (3-4): (25-30): (1.5-2).
[0017] As a preferred solution, the mass ratio of the S1 product, alumina and chopped carbon fibers is (1.2~1.5): (0.8~1.2): (3.5~4).
[0018] As a preferred solution, the mass ratio of succinic anhydride to 3-aminopropyltriethoxysilane is (2.5-4): (0.5-1).
[0019] As a preferred solution, the mass ratio of the chopped carbon fiber to dicyclopentadiene is (3.5-4): (1-1.2).
[0020] As a preferred solution, the average length of the chopped carbon fibers is 5-7 mm, and the average diameter is 4-5.5 μm.
[0021] In the present application, by adding the above-mentioned composite modified filler, it is possible to significantly improve the waterproof, aging resistance and mechanical properties of the polymer material of the LED lamp shell while maintaining good thermal conductivity and heat dissipation performance. First, the composite modified filler added in the present application can form linear composite particles with carbon fiber as the main support through the three-dimensional composite of framework particles, nanoparticles and chopped fibers. The particles can significantly enhance the hydrogen bonding and connection effect with the raw materials of the polymer system through the modification and modification of their surface groups, thereby playing a good connection role while forming micropores, thereby playing a good stress connection and dissipation role when external forces such as external pressure and stretching act.
[0022] Secondly, the formed composite structure can form a rough surface on the surface of the polymer material through the laying effect of carbon fiber in the polymer system, utilizing its good low surface energy and surface roughness, thereby greatly reducing the formation rate of the surface hydration layer. The existing framework particles can greatly absorb the water molecules inside the material, thereby cutting off the penetration path of the water molecules, and no water desorption will occur at a limited temperature, thereby maintaining excellent waterproof and water-resistant properties during long-term use.
[0023] Finally, the added modified composite particles can not only construct a thermal conductive path through carbon fiber and zinc oxide particles to achieve heat dissipation effect, but also form a good electronic path structure under the action of light energy through the coordination structure formed between the above composite particles. Moreover, due to the continuous input of light energy and the existence of the coordination structure, the occurrence of electronic reset phenomenon can be greatly reduced, thereby maintaining good anti-static and anti-aging properties of the particles for a long time, effectively reducing the probability of aging, yellowing and static electricity accumulation of LED lamps during long-term use, thereby greatly improving the above performance.
[0024] As a preferred solution, the preparation method of the modified resin comprises the following steps: S1: adding acrylonitrile, 2-ethylhexyl acrylate and isobornyl acrylate to an organic solvent, introducing nitrogen, adding an initiator, heating to 65-75°C and reacting for 2-4 hours to generate a prepolymer; S2: adding the prepolymer to a container containing acrylamide, and supplementing with deionized water and an initiator, after nitrogen fully replaces the reaction system gas, reacting at 75-80°C for 4-6 hours; S3: filtering the product obtained in S2, adding acetone to the filtered product to wash the homopolymer, and then mixing and stirring with a low concentration of sodium hydroxide solution at 50-55°C and keeping warm for 30-40 minutes, washing with deionized water after completion, and obtaining the product after complete ventilation and drying.
[0025] As a preferred solution, the mass ratio of acrylonitrile, 2-ethylhexyl acrylate, isobornyl acrylate and acrylamide is (5-8): (2-4): (1-3): (20-30).
[0026] As a preferred solution, the mass ratio of acrylonitrile, 2-ethylhexyl acrylate, isobornyl acrylate and acrylamide is (6-7): (2-3): (1.5-2): (22-25).
[0027] As a preferred solution, the initiator is potassium persulfate or ammonium persulfate.
[0028] As a preferred solution, the mass ratio of the filtered product to the sodium hydroxide solution is (1.3-1.5):0.8.
[0029] As a preferred solution, the concentration of the sodium hydroxide solution is 2-4wt%.
[0030] The resin added in this application can effectively improve the heat dissipation, waterproof, aging resistance and pressure resistance of the shell polymer material. The added modified resin can provide a stable guiding effect for the modified composite particles added in the application through its good chemical hydrogen bonding effect. Through the guiding effect of its long molecular chain, the flow dispersion of carbon fiber in the polymer material can be greatly enhanced, and then a good extension effect can be achieved under the formed three-dimensional network system, and due to the good connection between them, the structural strength of the three-dimensional network system can also be enhanced, so as to play a composite mechanical support role under the external force compression; on the other hand, the addition of modified resin can effectively improve the molecular network density of the system, and then suppress the contact frequency of internal active molecules or water molecules under the active environment, avoiding the probability of excessive aggregation and mutual collision to produce reactions, and then obtaining excellent aging resistance and waterproof performance, and having excellent service life.
[0031] As a preferred solution, the antioxidant is at least one of antioxidant 1010, antioxidant 1076, antioxidant 164, antioxidant CA, antioxidant 168, DSTDP, and DNP.
[0032] As a preferred solution, the antioxidant is at least one of antioxidant 1010, antioxidant 168, and DSTDP.
[0033] As a preferred solution, the plasticizer is at least one of dioctyl adipate, dioctyl sebacate, dioctyl phthalate, polyethylene glycol, polytetramethylene ether glycol, and epoxy compounds.
[0034] As a preferred solution, the plasticizer is dioctyl phthalate.
[0035] As a preferred solution, the dispersant is at least one of lauryl alcohol polyoxyethylene ether, cetyl alcohol polyoxyethylene ether, sodium dodecylbenzene sulfonate, betaine, alkyl glycoside, and polyethylene glycol ether.
[0036] As a preferred solution, the dispersant is at least one of lauryl alcohol polyoxyethylene ether, cetyl alcohol polyoxyethylene ether, and sodium dodecylbenzene sulfonate.
[0037] As a preferred solution, the dispersant is lauryl alcohol polyoxyethylene ether.
[0038] As a preferred solution, the auxiliary agent at least includes a flame retardant and a lubricant.
[0039] As a preferred solution, the mass ratio of the flame retardant to the lubricant is (5-8):(2-4).
[0040] As a preferred solution, the flame retardant is at least one of chlorinated polyethylene, chlorinated paraffin, triphenyl phosphate, ammonium polyphosphate, ammonium phosphate salt, and melamine.
[0041] As a preferred solution, the lubricant is at least one of butyl stearate, isooctyl stearate, oleamide, ethylene bisstearamide, polyethylene wax, zinc stearate, calcium stearate, and glyceryl stearate.
[0042] As a preferred solution, the lubricant is a combination of isooctyl stearate and zinc stearate.
[0043] As a preferred solution, the mass ratio of isooctyl stearate to zinc stearate is (3-5): (1-1.5).
[0044] The second aspect of the present application provides a method for preparing the above-mentioned pressure-resistant housing polymer material for LED lamps, comprising the following specific steps: S1: After pre-mixing the polyamide material and the epoxy block resin, place them in a drying oven at 90~100℃ for ventilation and drying for 3~4h, and add them to a high-speed mixer after drying; S2: add the remaining raw materials in the high-speed mixer in sequence, heat the temperature to 50~65℃, and stir at 200~400rpm for 3~4h to obtain a mixture; S3: add the mixture to a twin-screw extruder, control the extrusion temperature to 260~300℃ and the screw speed to 200~240rpm for melt extrusion granulation, and obtain the mixture after completion.
[0045] The beneficial effects of this application are:
[0046] 1. The pressure-resistant polymer material for the LED lamp provided in the present application not only has excellent thermal conductivity and heat dissipation performance, but also can simultaneously maintain excellent mechanical properties such as waterproofness, aging resistance and pressure resistance of the shell material, effectively avoiding the technical problems existing in existing LED shell polymer materials, and has very excellent market application value.
[0047] 2. A pressure-resistant shell polymer material for LED lamps provided in the present application forms a three-dimensional composite of framework particles, nanoparticles and chopped fibers by adding composite modified fillers to form linear composite particles with carbon fibers as the main support. The particles can greatly enhance the hydrogen bonding and connection effects with the raw materials of the polymer system through the modification and modification of their surface groups, thereby playing a good connection role while forming micropores, thereby playing a good stress connection and dissipation role when external forces such as external pressure and stretching act, thereby enhancing the tensile and compressive strength of the material.
[0048] 3. A pressure-resistant polymer material for an LED lamp provided in the present application, through the addition of a composite modified filler, forms a composite structure that can form a rough surface on the surface of the polymer material through the paving effect of carbon fiber in the polymer system and its good low surface energy and surface roughness, thereby greatly reducing the formation rate of the surface hydration layer, and the existing framework particles can greatly absorb the water molecules inside the material, thereby cutting off the penetration path of the water molecules, and no water desorption will occur at a limited temperature, thereby maintaining excellent waterproof and water-resistant properties during long-term use.
[0049] 4. A pressure-resistant polymer material for an LED lamp provided in the present application, the added modified resin can provide stable guiding effect for the modified composite particles added in the application through its good chemical hydrogen bonding effect, and through the guiding effect of its long molecular chain, it can greatly enhance the flow dispersion of carbon fiber in the polymer material, and thus play a good extension effect in the formed three-dimensional network system, and due to the good connection between them, it can also enhance the structural strength of the three-dimensional network system, thereby playing a composite mechanical support role under the action of external force; on the other hand, the addition of modified resin can effectively improve the density of the system molecular network, and thus suppress the contact frequency of internal active molecules or water molecules in an active environment, avoiding the probability of excessive aggregation and mutual collision to produce reactions, thereby obtaining excellent aging resistance and waterproof performance, and having an excellent service life. DETAILED DESCRIPTION
[0050] The following will further explain and demonstrate the technical solutions in the above invention content of this application in the form of specific implementation schemes. The following embodiments are only practical examples used to illustrate and explain the contents of the technical solutions in the specification, and should not limit the scope of the claims to be protected by this application. All technical products based on the technical solutions described in the invention content of this application should be included in the scope to be protected by this application.
[0051] In the following examples, unless otherwise specified, the raw materials are all commercially available products, or can be prepared by methods well known to those skilled in the art.
[0052] Example 1
[0053] Embodiment 1 The first aspect provides a pressure-resistant housing polymer material for LED lamps. The raw materials are, by mass, 110 parts of polyamide material, 24 parts of epoxy block resin, 28 parts of composite modified filler, 18 parts of modified resin, 3 parts of antioxidant, 10.5 parts of plasticizer, 6.5 parts of dispersant, and 10.5 parts of additive.
[0054] The glass fiber content of the polyamide material is 30wt%, and the polyamide material is purchased from Kuraray under the model number PA9T-GN2330.
[0055] The epoxy block resin is a block copolymer resin of ethylene oxide and propylene oxide, has a weight average molecular weight of 4600, and is purchased from BASF as an L85 epoxy block resin product.
[0056] The preparation method of the composite modified filler comprises the following steps, calculated by mass: S1: adding 3.2 parts of aluminum nitrate and 28.5 parts of acetic acid to 180 parts of deionized water and stirring at room temperature, then adding to a closed reactor, gradually heating to 200°C at a heating rate of 2°C / min, and controlling the pressure in the reactor to be 2.1MPa, during which a deionized water solution containing 1.8 parts of terephthalic acid (a total of 25 parts) is added dropwise, and the dropping temperature range is 40 to 120°C. After the heating is completed, the reaction is stirred and reacted for 8.5 hours, and the product is washed, filtered and dried; S2: adding 1 .45 parts of S1 product, 1.05 parts of alumina and 3.6 parts of chopped carbon fibers are mixed and ultrasonically dispersed evenly in 60 parts of DMF solution, then 2.85 parts of succinic anhydride and 0.62 parts of 3-aminopropyltriethoxysilane are added, the temperature is raised to 65°C and the reaction is kept warm for 3.5 hours, and then the heat is continued to be kept warm and ultrasonically oscillated at 350 W for 4.5 hours; S3: after the oscillation is completed, 2.6 parts of citric acid, 15 parts of ethanol and 1.1 parts of dicyclopentadiene are added, the temperature is raised to 80°C and the reaction is continued with stirring for 7.5 hours. The product is centrifuged and filtered, washed and dried to obtain.
[0057] The average length of the chopped carbon fiber is 6 mm, the average diameter is 4.5 μm, and the corresponding size products are purchased from Jiangxi Shuobang New Material Technology Co., Ltd.
[0058] The preparation method of the modified resin comprises the following steps, calculated by mass: S1: adding 6.5 parts of acrylonitrile, 2.5 parts of 2-ethylhexyl acrylate and 1.8 parts of isobornyl acrylate to an acryloyl chloride solution, introducing nitrogen, adding 0.08 parts of potassium persulfate, heating to 65°C for reaction for 3 hours to generate a prepolymer; S2: adding the prepolymer to a container containing 24.5 parts of acrylamide, and supplementing with 200 parts of deionized water and 0.14 parts of potassium persulfate, after nitrogen fully replaces the reaction system gas, reacting at 75°C for 5 hours; S3: filtering the product obtained in S2, adding acetone to the filtered product to wash the homopolymer, and then mixing with a low concentration of sodium hydroxide solution, stirring and keeping warm at 55°C for 40 minutes, washing with deionized water after completion, and obtaining the product after complete ventilation and drying.
[0059] The mass ratio of the filtered product to the sodium hydroxide solution is 1.5:0.8, and the concentration of the sodium hydroxide solution is 2.5wt%.
[0060] The antioxidant is antioxidant 1010; the plasticizer is dioctyl phthalate; the dispersant is lauryl alcohol polyoxyethylene ether, purchased from the MOA-4 product sold by Hai'an Guoyun Chemical.
[0061] The additives are flame retardant and lubricant, and the mass ratio of the two is 7.5:3.
[0062] The flame retardant is triphenyl phosphate; the lubricant is a composition of isooctyl stearate and zinc stearate, and the mass ratio of the two is 4:1.2.
[0063] The second aspect of the present embodiment provides a method for preparing the above-mentioned pressure-resistant housing polymer material for LED lamps, comprising the following specific steps: S1: After pre-mixing the polyamide material and the epoxy block resin, place them in a drying oven for ventilation and drying at 100°C for 4 hours, and add them to a high-speed mixer after drying; S2: add the remaining raw materials to the high-speed mixer in sequence, heat the temperature to 60°C, and stir at 350rpm for 4 hours to obtain a mixture; S3: add the mixture to a twin-screw extruder, control the extrusion temperature to 290°C and the screw speed to 220rpm for melt extrusion and granulation, and the mixture is obtained after completion.
[0064] Example 2
[0065] Embodiment 2 The first aspect provides a pressure-resistant housing polymer material for LED lamps. The raw materials are, by mass, 100 parts of polyamide material, 24 parts of epoxy block resin, 25 parts of composite modified filler, 25 parts of modified resin, 3 parts of antioxidant, 10.5 parts of plasticizer, 6.5 parts of dispersant, and 10.5 parts of additive.
[0066] The glass fiber content of the polyamide material is 30wt%, and the polyamide material is purchased from Kuraray under the model number PA9T-GN2330.
[0067] The epoxy block resin is a block copolymer resin of ethylene oxide and propylene oxide, has a weight average molecular weight of 4600, and is purchased from BASF as an L85 epoxy block resin product.
[0068] The preparation method of the composite modified filler comprises the following steps, calculated by mass: S1: adding 3.2 parts of aluminum nitrate and 28.5 parts of acetic acid to 180 parts of deionized water and stirring at room temperature, then adding to a closed reactor, gradually heating to 200°C at a heating rate of 2°C / min, and controlling the pressure in the reactor to be 2.1MPa, during which a deionized water solution containing 1.8 parts of terephthalic acid (a total of 25 parts) is added dropwise, and the dropping temperature range is 40 to 120°C. After the heating is completed, the reaction is stirred and reacted for 8.5 hours, and the product is washed, filtered and dried; S2: adding 1 .45 parts of S1 product, 1.05 parts of alumina and 3.6 parts of chopped carbon fibers are mixed and ultrasonically dispersed evenly in 60 parts of DMF solution, then 2.85 parts of succinic anhydride and 0.62 parts of 3-aminopropyltriethoxysilane are added, the temperature is raised to 65°C and the reaction is kept warm for 3.5 hours, and then the heat is continued to be kept warm and ultrasonically oscillated at 350 W for 4.5 hours; S3: after the oscillation is completed, 2.6 parts of citric acid, 15 parts of ethanol and 1.1 parts of dicyclopentadiene are added, the temperature is raised to 80°C and the reaction is continued with stirring for 7.5 hours. The product is centrifuged and filtered, washed and dried to obtain.
[0069] The average length of the chopped carbon fiber is 6 mm, the average diameter is 4.5 μm, and the corresponding size products are purchased from Jiangxi Shuobang New Material Technology Co., Ltd.
[0070] The preparation method of the modified resin comprises the following steps, calculated by mass: S1: adding 6.5 parts of acrylonitrile, 2.5 parts of 2-ethylhexyl acrylate and 1.8 parts of isobornyl acrylate to an acryloyl chloride solution, introducing nitrogen, adding 0.08 parts of potassium persulfate, heating to 65°C for reaction for 3 hours to generate a prepolymer; S2: adding the prepolymer to a container containing 24.5 parts of acrylamide, and supplementing with 200 parts of deionized water and 0.14 parts of potassium persulfate, after nitrogen fully replaces the reaction system gas, reacting at 75°C for 5 hours; S3: filtering the product obtained in S2, adding acetone to the filtered product to wash the homopolymer, and then mixing with a low concentration of sodium hydroxide solution, stirring and keeping warm at 55°C for 40 minutes, washing with deionized water after completion, and obtaining the product after complete ventilation and drying.
[0071] The mass ratio of the filtered product to the sodium hydroxide solution is 1.5:0.8, and the concentration of the sodium hydroxide solution is 2.5wt%.
[0072] The antioxidant is antioxidant 1010; the plasticizer is dioctyl phthalate; the dispersant is lauryl alcohol polyoxyethylene ether, purchased from the MOA-4 product sold by Hai'an Guoyun Chemical.
[0073] The additives are flame retardant and lubricant, and the mass ratio of the two is 7.5:3.
[0074] The flame retardant is triphenyl phosphate; the lubricant is a composition of isooctyl stearate and zinc stearate, and the mass ratio of the two is 4:1.2.
[0075] The second aspect of the present embodiment provides a method for preparing the above-mentioned pressure-resistant housing polymer material for LED lamps, comprising the following specific steps: S1: After pre-mixing the polyamide material and the epoxy block resin, place them in a drying oven for ventilation and drying at 100°C for 4 hours, and add them to a high-speed mixer after drying; S2: add the remaining raw materials to the high-speed mixer in sequence, heat the temperature to 60°C, and stir at 350rpm for 4 hours to obtain a mixture; S3: add the mixture to a twin-screw extruder, control the extrusion temperature to 290°C and the screw speed to 220rpm for melt extrusion and granulation, and the mixture is obtained after completion.
[0076] Comparative Example 1
[0077] The specific implementation of this comparative example is basically the same as that of Example 1, except that the weight average molecular weight of the epoxy block resin is 10,800, and the epoxy block resin is purchased from BASF L88.
[0078] Comparative Example 2
[0079] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the preparation method of the composite modified filler comprises the following steps, calculated by mass: S1: 5.5 parts of aluminum nitrate and 10 parts of acetic acid are added to 180 parts of deionized water and stirred at room temperature, then added to a closed reactor, and the temperature is gradually increased to 200°C at a heating rate of 2°C / min, and the pressure in the reactor is controlled to be 2.1MPa. During this period, a deionized water solution containing 1.2 parts of terephthalic acid (a total of 25 parts) is added dropwise, and the dropping temperature range is 40 to 120°C. After the heating is completed, the reaction is stirred for 8.5 hours to produce The product was washed, filtered and dried; S2: 1.45 parts of S1 product, 1.05 parts of alumina and 3.6 parts of chopped carbon fibers were mixed and ultrasonically dispersed in 60 parts of DMF solution, and then 2.85 parts of succinic anhydride and 0.62 parts of 3-aminopropyltriethoxysilane were added, the temperature was raised to 65°C and the reaction was kept warm for 3.5 hours, and then the heat was continued to be kept warm and ultrasonically oscillated at 350 W for 4.5 hours; S3: After the oscillation was completed, 2.6 parts of citric acid, 15 parts of ethanol and 1.1 parts of dicyclopentadiene were added and the temperature was raised to 80°C and the reaction was continued with stirring for 7.5 hours. The product was centrifuged and filtered, washed and dried to obtain.
[0080] Comparative Example 3
[0081] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the preparation method of the composite modified filler comprises the following steps, calculated by mass: S1: 3.2 parts of aluminum nitrate and 28.5 parts of acetic acid are added to 180 parts of deionized water and stirred at room temperature, then added to a closed reactor, and the temperature is gradually increased to 200°C at a heating rate of 2°C / min, and the pressure in the reactor is controlled to be 2.1 MPa. During this period, a deionized water solution containing 1.8 parts of terephthalic acid (a total of 25 parts) is added dropwise, and the dropping temperature ranges from 40 to 120°C. After the heating is completed, the reaction is stirred continuously for 8.5 minutes. h, the product was washed, filtered and dried; S2: 3.5 parts of S1 product, 0.5 parts of alumina and 3.5 parts of chopped carbon fibers were mixed and ultrasonically dispersed in 100 parts of DMF solution, and then 3.8 parts of succinic anhydride and 0.8 parts of 3-aminopropyltriethoxysilane were added, the temperature was raised to 65°C and the reaction was kept warm for 3.5 hours, and then the heat was continued to be kept warm and ultrasonically oscillated at a power of 350W for 4.5 hours; S3: After the oscillation was completed, 2.6 parts of citric acid, 15 parts of ethanol and 1.1 parts of dicyclopentadiene were added and the temperature was raised to 80°C and the reaction was continued with stirring for 7.5 hours. The product was centrifuged and filtered, washed and dried to obtain.
[0082] Comparative Example 4
[0083] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the preparation method of the composite modified filler comprises the following steps, calculated by mass: S1: 3.2 parts of aluminum nitrate and 28.5 parts of acetic acid are added to 180 parts of deionized water and stirred at room temperature, then added to a closed reactor, and the temperature is gradually increased to 200°C at a heating rate of 2°C / min, and the pressure in the reactor is controlled to be 2.1MPa. During this period, a deionized water solution containing 1.8 parts of terephthalic acid (a total of 25 parts) is added dropwise, and the dropping temperature range is 40 to 120°C. After the heating is completed, the reaction is stirred for 8.5 hours. , the product is washed, filtered and dried; S2: 1.45 parts of S1 product, 1.05 parts of alumina and 3.6 parts of chopped carbon fibers are mixed and ultrasonically dispersed in 60 parts of DMF solution, then 4.5 parts of succinic anhydride and 0.25 parts of 3-aminopropyltriethoxysilane are added, the temperature is raised to 65°C and the reaction is kept warm for 3.5 hours, and then the heat is continued to be kept warm and ultrasonically oscillated at 350W for 4.5 hours; S3: After the oscillation is completed, 2.6 parts of citric acid, 10 parts of ethanol and 0.5 parts of dicyclopentadiene are added and the temperature is raised to 80°C and the reaction is continued with stirring for 7.5 hours. The product is centrifuged and filtered, washed and dried to obtain.
[0084] Comparative Example 5
[0085] The specific implementation of this comparative example is basically the same as that of Example 1, except that the average length of the chopped carbon fibers is 12.5 mm and the average diameter is 7 μm.
[0086] Comparative Example 6
[0087] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the preparation method of the modified resin comprises the following steps, calculated by mass: S1: adding 15 parts of acrylonitrile, 1.5 parts of 2-ethylhexyl acrylate and 1 part of isobornyl acrylate to an acryloyl chloride solution, introducing nitrogen, adding 0.1 part of potassium persulfate, heating to 65°C and reacting for 3 hours to generate a prepolymer; S2: adding the prepolymer to a container containing 25.5 parts of acrylamide, and supplementing with 200 parts of deionized water and 0.18 parts of potassium persulfate, after nitrogen fully replaces the reaction system gas, reacting at 75°C for 5 hours; S3: filtering the product obtained in S2, adding acetone to the filtered product to wash the homopolymer, and then mixing with a low concentration of sodium hydroxide solution, stirring and keeping warm at 55°C for 40 minutes, washing with deionized water after completion, and obtaining the product after complete ventilation and drying.
[0088] Comparative Example 7
[0089] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the preparation method of the modified resin comprises the following steps, calculated by mass: S1: adding 4.5 parts of acrylonitrile, 2.5 parts of 2-ethylhexyl acrylate and 1.8 parts of isobornyl acrylate to an acryloyl chloride solution, introducing nitrogen, adding 0.08 parts of potassium persulfate, heating to 65°C and reacting for 3 hours to generate a prepolymer; S2: adding the prepolymer to a container containing 40.5 parts of acrylamide, and supplementing with 200 parts of deionized water and 0.16 parts of potassium persulfate, after nitrogen fully replaces the reaction system gas, reacting at 75°C for 5 hours; S3: filtering the product obtained in S2, adding acetone to the filtered product to wash the homopolymer, and then mixing with a low concentration of sodium hydroxide solution, stirring and keeping warm at 55°C for 40 minutes, washing with deionized water after completion, and obtaining the product after complete ventilation and drying.
[0090] Comparative Example 8
[0091] The specific implementation of this comparative example is basically the same as that of Example 1, except that the mass ratio of the filtered product to the sodium hydroxide solution is 1:1, and the concentration of the sodium hydroxide solution is 10 wt %.
[0092] Performance Evaluation
[0093] Thermal conductivity: The shell polymer materials prepared in the examples and comparative examples were injection molded into standard test specimens at 300° C., and the thermal conductivity was tested according to ISO 22007-2-2008 standard. The test values were averaged over 10 tests and recorded in Table 1.
[0094] Waterproof performance: The shell polymer materials prepared in the examples and comparative examples were injection molded at 300° C. into standard test specimens, and the water vapor transmission rate was tested according to ASTM E96 standard. The test values were averaged from 10 tests and recorded in Table 1.
[0095] Compression resistance: The shell polymer materials prepared in the examples and comparative examples were injection molded at 300° C. into standard test specimens, and the compressive strength was tested according to ASTM D695 standard. The test values were taken as the average of 10 tests and recorded in Table 1.
[0096] Aging resistance: The shell polymer materials prepared in the embodiments and comparative examples were injection molded at 300°C into standard test specimens, and the test specimens were placed in a constant temperature and humidity environment at 65°C and 75% relative humidity for 3 months. After 3 months, the test specimens were observed to see if there were obvious cracking, blistering, yellowing and curling. If not, they were marked as unqualified, otherwise they were qualified. 50 specimens were tested in each group, and the qualified rate (%) = number of qualified test specimens / 50×100%. The results are recorded in Table 1.
[0097] Table 1 Performance test results
[0098]
[0099] From the examples and comparative examples of the present application and the data results in Table 1, it can be seen that examples 1 and 2 of the present application have obvious performance advantages over comparative examples 1 to 8 in terms of compression resistance, waterproof performance, heat dissipation performance and aging resistance, which is mainly due to the compounding and addition of modified composite particles and modified resins in examples 1 and 2. However, comparative examples 1 to 8 have obvious disadvantages in the above-mentioned performances because they do not adopt the correct technical solution defined in the present application, which further proves the necessity of the technical solution defined in the present application for the technical effect of the present application and solving the technical problems.
Claims
1. A pressure-resistant housing polymer material for LED lamps, characterized in that: The raw materials are as follows: 90-130 parts of polyamide material, 20-30 parts of epoxy block resin, 20-40 parts of composite modified filler, 10-25 parts of modified resin, 2-4 parts of antioxidant, 5-15 parts of plasticizer, 5-10 parts of dispersant, and 5-15 parts of auxiliary agent by weight. The mass ratio of the polyamide material, the composite modified filler and the modified resin is (9.5-12): (2.5-3.5): (1.5-2.5); The glass fiber content of the polyamide material is 15-35wt%; The epoxy block resin is a block copolymer resin of ethylene oxide and propylene oxide; the weight average molecular weight of the epoxy block resin is 4000-8000; The auxiliary agent is a flame retardant and a lubricant; the mass ratio of the flame retardant and the lubricant is (5-8): (2-4); The preparation method of the composite modified filler comprises the following steps: S1: adding aluminum nitrate and acetic acid to deionized water and stirring them evenly at room temperature, then adding them to a closed reaction kettle, gradually heating them to 200-210°C at a heating rate of 2°C / min, and controlling the pressure in the kettle to be 2.0-2.4MPa, during which a deionized water solution containing terephthalic acid is added dropwise, and the dropping temperature range is 40-120°C. After the heating is completed, the reaction is stirred continuously for 8-10 hours, and the product is washed, filtered, and dried; S2: The product of S1, alumina and chopped carbon fiber are mixed and ultrasonically dispersed in a DMF solution, and then succinic anhydride and 3-aminopropyltriethoxysilane are added, and the temperature is raised to 60-70°C for reaction for 3-4 hours, and then the temperature is continued to be ultrasonically shaken at a power of 300-500W for 4-5 hours; S3: After the shaking is completed, citric acid, ethanol and dicyclopentadiene are added, and the temperature is raised to 75-85°C and the reaction is continued with stirring for 6-8 hours. The product is centrifuged and filtered, and then washed and dried to obtain; The mass ratio of aluminum nitrate, acetic acid and terephthalic acid is (3-4): (25-30): (1.5-2); the mass ratio of S1 product, aluminum oxide and chopped carbon fiber is (1.2-1.5): (0.8-1.2): (3.5-4); The mass ratio of succinic anhydride to 3-aminopropyltriethoxysilane is (2.5-4): (0.5-1); the mass ratio of chopped carbon fiber to dicyclopentadiene is (3.5-4): (1-1.2); The average length of the chopped carbon fibers is 5-7 mm, and the average diameter is 4-5.5 μm; The preparation method of the modified resin comprises the following steps: S1: adding acrylonitrile, 2-ethylhexyl acrylate and isobornyl acrylate to an organic solvent, introducing nitrogen, adding an initiator, heating to 65-75°C for reaction for 2-4 hours to generate a prepolymer; S2: adding the prepolymer to a container containing acrylamide, and supplementing with deionized water and an initiator, after nitrogen fully replaces the reaction system gas, reacting at 75-80°C for 4-6 hours; S3: filtering the product obtained in S2, adding acetone to the filtered product to wash the homopolymer, and then mixing and stirring with a low-concentration sodium hydroxide solution at 50-55°C for 30-40 minutes, and then washing with deionized water, and drying through ventilation to obtain the product; The mass ratio of acrylonitrile, 2-ethylhexyl acrylate, isobornyl acrylate and acrylamide is (5-8): (2-4): (1-3): (20-30); The mass ratio of the filtered product to the sodium hydroxide solution is (1.3-1.5):0.8; the concentration of the sodium hydroxide solution is 2-4wt%.
2. The pressure-resistant housing polymer material for LED lamp according to claim 1, characterized in that: The mass ratio of the polyamide material, epoxy block resin and auxiliary agent is (9.5-12): (2-2.5): (1-1.5).
3. The pressure-resistant housing polymer material for LED lamp according to claim 2, characterized in that: The antioxidant is at least one of antioxidant 1010, antioxidant 1076, antioxidant 164, antioxidant CA, antioxidant 168, DSTDP, and DNP.
4. The pressure-resistant housing polymer material for LED lamp according to claim 3, characterized in that: The plasticizer is at least one of dioctyl adipate, dioctyl sebacate, dioctyl phthalate, polyethylene glycol, polytetramethylene ether glycol, and epoxy compounds.
5. The pressure-resistant housing polymer material for LED lamp according to claim 4, characterized in that: The dispersant is at least one of lauryl alcohol polyoxyethylene ether, cetyl alcohol polyoxyethylene ether, sodium dodecylbenzene sulfonate, betaine, alkyl glycoside, and polyethylene glycol ether.
6. A method for preparing a pressure-resistant housing polymer material for an LED lamp according to any one of claims 1 to 5, characterized in that: The method comprises the following specific steps: S1: pre-mixing a polyamide material and an epoxy block resin uniformly, placing the mixture in a drying oven at 90-100° C. for ventilation drying for 3-4 hours, and adding the mixture to a high-speed mixer after drying; S2: adding the remaining raw materials in the high-speed mixer in sequence, heating the mixture to 50-65° C., and stirring the mixture at a speed of 200-400 rpm for 3-4 hours to obtain a mixture; S3: adding the mixture to a twin-screw extruder, controlling the extrusion temperature to 260-300° C. and the screw speed to 200-240 rpm for melt extrusion granulation, and obtaining the mixture after completion.