Alignment mark preparation method and semiconductor structure

By forming filled alignment marks on the substrate during semiconductor manufacturing, the problem of degradation of the alignment accuracy of the epitaxial layer is solved, and higher alignment accuracy and alignment mark shape protection are achieved.

CN118571863BActive Publication Date: 2024-11-12NEXCHIP SEMICON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411027253.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

During semiconductor manufacturing, the alignment marks of the epitaxial layer decrease in alignment accuracy due to differences in physical shrinkage and growth rate, which affects the interlacing accuracy.

Method used

Provided a method of preparing an alignment mark by forming a front layer alignment pattern on a substrate, including an initial groove arranged in parallel, and forming a layer alignment pattern thereon, filling the initial grooves so as to align the layers. The top surface of the pattern is higher than the top surface of the initial groove and then covers the epitaxial layer to form an alignment mark including the front layer, the when layer and the epitaxial layer.

Benefits of technology

The alignment accuracy after the protrusion is improved, the shape of the initial groove is protected, the alignment mark is avoided, and the alignment accuracy is improved through signal strengths of different height differences.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118571863B_ABST
    Figure CN118571863B_ABST
Patent Text Reader

Abstract

The present application relates to a method for preparing an alignment mark and a semiconductor structure, by providing a substrate, the substrate includes an alignment mark area formed with a front-layer alignment pattern, wherein the front-layer alignment pattern includes a plurality of initial grooves arranged in parallel, a current-layer alignment pattern is formed on the front-layer alignment pattern, the current-layer alignment pattern fills the plurality of initial grooves, and exposes the surface of the substrate where the initial grooves are not formed, so that the top surface of the current-layer alignment pattern is higher than the top surface of the initial grooves, and an epitaxial layer is covered on the front-layer alignment pattern and the current-layer alignment pattern, wherein the alignment mark includes the front-layer alignment pattern, the current-layer alignment pattern and the epitaxial layer, thereby improving the alignment accuracy after epitaxy. The present application makes the top surface of the current-layer alignment pattern higher than the top surface of the initial grooves, so that there is a height difference between the current-layer alignment pattern and the front-layer alignment pattern, and the signal strengths of different height differences are different, thereby further improving the alignment accuracy after epitaxy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of integrated circuit technology, and in particular to a method for preparing an alignment mark and a semiconductor structure. Background Art

[0002] Overlay is an important step in the semiconductor manufacturing process, which involves accurately superimposing different levels of patterns on the substrate to construct complex circuits. During the overlay process, in order to ensure overlay accuracy, the machine needs to align the layers by identifying the alignment marks in the alignment mark area.

[0003] Epitaxial technology is widely used in chip manufacturing processes. However, in the process of forming the epitaxial layer, due to physical expansion and contraction, growth rate differences and other issues, the alignment marks of the epitaxial layer will be deformed, affecting the alignment accuracy of the alignment marks. Summary of the invention

[0004] Based on this, it is necessary to provide a method for preparing an alignment mark and a semiconductor structure to address the problem of decreased alignment accuracy after wafer epitaxy in the prior art.

[0005] In order to achieve the above-mentioned objectives, on the one hand, the present application provides a method for preparing an alignment mark, comprising: providing a substrate, the substrate comprising an alignment mark area formed with a front-layer alignment pattern; wherein the front-layer alignment pattern comprises a plurality of initial grooves arranged in parallel; forming a current-layer alignment pattern on the front-layer alignment pattern, the current-layer alignment pattern filling the plurality of initial grooves and exposing a surface of the substrate where the initial grooves are not formed; wherein the top surface of the current-layer alignment pattern is higher than the top surface of the initial grooves; covering the front-layer alignment pattern and the current-layer alignment pattern with an epitaxial layer; wherein the alignment mark comprises the front-layer alignment pattern, the current-layer alignment pattern and the epitaxial layer.

[0006] In one of the embodiments, forming the current layer alignment pattern on the previous layer alignment pattern includes: forming a sacrificial layer on the previous layer alignment pattern; wherein the sacrificial layer includes a plurality of first openings, and the plurality of first openings expose the plurality of initial grooves; using a spin coating process to fill a target solution in a target groove formed by the first openings and the initial grooves; using a first preset temperature to treat the target solution to form the current layer alignment pattern; and removing the sacrificial layer.

[0007] In one embodiment, after the target solution is filled in the target groove formed by the first opening and the initial groove by the spin coating process, and before the target solution is treated at a first preset temperature, the process further includes: treating the target solution at a second preset temperature to form a solidified target solution; and planarizing the solidified target solution to form a target solution of a preset height.

[0008] In one embodiment, the first preset temperature ranges from 500 degrees Celsius to 800 degrees Celsius; the second preset temperature ranges from 60 degrees Celsius to 120 degrees Celsius.

[0009] In one embodiment, forming a sacrificial layer on the front layer alignment pattern comprises: forming a photoresist layer on the front layer alignment pattern; and etching the photoresist layer using an auxiliary mask including a first pattern to form the sacrificial layer.

[0010] In one embodiment, forming a sacrificial layer on the front-layer alignment pattern comprises: forming a photoresist layer on the front-layer alignment pattern; and etching the photoresist layer using a light shield to form the sacrificial layer.

[0011] In one embodiment, the target solution includes one or more of silica sol, ethyl orthosilicate, and methyl orthosilicate.

[0012] In one of the embodiments, the depth of the initial groove ranges from 50nm to 1000nm; and the difference between the thickness of the current layer alignment pattern and the depth of the initial groove ranges from 500nm to 3000nm.

[0013] In one embodiment, the material of the layer alignment pattern is selected from one or more of silicon oxide, raw material hydrated yttrium nitrate, raw material hydrated zirconium nitrate, and raw material nano-alumina powder.

[0014] On the other hand, the present application also provides a semiconductor structure, comprising: a substrate, the substrate comprising an alignment mark area formed with a front layer alignment pattern; wherein the front layer alignment pattern comprises a plurality of initial grooves arranged in parallel; a current layer alignment pattern, located on the front layer alignment pattern, the current layer alignment pattern fills the plurality of initial grooves and exposes the surface of the substrate where the initial grooves are not formed; wherein the top surface of the current layer alignment pattern is higher than the top surface of the initial grooves; an epitaxial layer, covering the front layer alignment pattern and the current layer alignment pattern; wherein the alignment mark comprises the front layer alignment pattern, the current layer alignment pattern and the epitaxial layer.

[0015] The method for preparing the alignment mark and the semiconductor structure of the present application have the following beneficial effects:

[0016] The preparation method of the alignment mark and the semiconductor structure of the present application provide a substrate, wherein the substrate includes an alignment mark area formed with a front-layer alignment pattern, wherein the front-layer alignment pattern includes a plurality of initial grooves arranged in parallel, a current-layer alignment pattern is formed on the front-layer alignment pattern, the current-layer alignment pattern fills the plurality of initial grooves, and exposes the surface of the substrate where the initial grooves are not formed, so that the top surface of the current-layer alignment pattern is higher than the top surface of the initial grooves, and an epitaxial layer is covered on the front-layer alignment pattern and the current-layer alignment pattern, wherein the alignment mark includes the front-layer alignment pattern, the current-layer alignment pattern and the epitaxial layer, thereby improving the alignment accuracy after epitaxy. The present application protects the shape of the initial groove and avoids deformation of the alignment mark by filling the initial groove with the current-layer alignment pattern, and the top surface of the current-layer alignment pattern is higher than the top surface of the initial groove, so that there is a height difference between the current-layer alignment pattern and the front-layer alignment pattern, and the signal strength of the film layers with different height differences is different, further improving the alignment accuracy after epitaxy. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0018] Figure 1 is a schematic structural diagram of an alignment mark provided in an embodiment;

[0019] Figure 2a is a schematic diagram of an alignment mark before forming an epitaxial layer in one embodiment;

[0020] Figure 2b is a schematic diagram of an alignment mark after forming an epitaxial layer in one embodiment;

[0021] Figure 2c is a schematic diagram of an optical signal before forming an epitaxial layer in one embodiment;

[0022] Figure 2d is a schematic diagram of an optical signal after an epitaxial layer is formed in one embodiment;

[0023] Figure 3 is a flow chart of a method for preparing an alignment mark in one embodiment;

[0024] Figure 4 is a flow chart of a method for forming a layer alignment pattern in one embodiment;

[0025] Figure 5 A schematic cross-sectional view of a structure obtained in step S302 in a method for preparing an alignment mark provided in an embodiment;

[0026] Figure 6 A schematic cross-sectional view of a structure obtained in step S402 of a method for preparing an alignment mark provided in an embodiment;

[0027] Figure 7 A schematic cross-sectional view of a structure obtained in step S404 in a method for preparing an alignment mark provided in an embodiment;

[0028] Figure 8 A schematic cross-sectional view of a structure obtained in step S404 in a method for preparing an alignment mark provided in an embodiment;

[0029] Fig. 9 A schematic cross-sectional view of a structure obtained in step S406 of a method for preparing an alignment mark provided in an embodiment;

[0030] Fig.10 A schematic cross-sectional view of a structure obtained in step S408 in a method for preparing an alignment mark provided in an embodiment;

[0031] Fig.11 A schematic cross-sectional view of a structure obtained in step S402 of a method for preparing an alignment mark provided in an embodiment;

[0032] Fig.12 is a schematic structural diagram of a sunshade in one embodiment;

[0033] Fig.13 A schematic flow chart of a specific process of a method for preparing an alignment mark in an embodiment;

[0034] Fig.14 FIG. 4 is a schematic diagram of the structure of an alignment mark in an embodiment.

[0035] Description of reference numerals:

[0036] 10. substrate; 102. initial groove; 20. sacrificial layer; 210. photoresist layer; 30. epitaxial layer; 40. target solution; 50. layer alignment pattern; 60. auxiliary mask; 70. light shield. DETAILED DESCRIPTION

[0037] In order to facilitate understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present application are given in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thorough and comprehensive.

[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0039] It should be understood that when an element or layer is referred to as being "on, adjacent to, connected to or coupled to other elements or layers, it may be directly on, adjacent to, connected to or coupled to other elements or layers, or there may be intervening elements or layers. On the contrary, when an element is referred to as being "directly on, directly adjacent to, directly connected to or directly coupled to other elements or layers, there are no intervening elements or layers. It should be understood that although the terms first, second, third, etc. may be used to describe various elements, components, regions, layers, doping types and / or parts, these elements, components, regions, layers, doping types and / or parts should not be limited by these terms. These terms are merely used to distinguish one element, component, region, layer, doping type or part from another element, component, region, layer, doping type or part. Therefore, without departing from the teachings of the present application, the first element, component, region, layer, doping type or portion discussed below may be represented as a second element, component, region, layer or portion; for example, the first doping type may be referred to as the second doping type, and similarly, the second doping type may be referred to as the first doping type; the first doping type and the second doping type are different doping types, for example, the first doping type may be P-type and the second doping type may be N-type, or the first doping type may be N-type and the second doping type may be P-type.

[0040] Spatially relative terms such as "under," "beneath," "below," "under," "above," "above," and the like may be used herein to describe the relationship of an element or feature shown in the figures to other elements or features. It should be understood that, in addition to the orientations shown in the figures, spatially relative terms also include different orientations of the device in use and operation. For example, if the device in the accompanying drawings is flipped, an element or feature described as "under other elements" or "under it" or "under it" will be oriented as being "above" the other elements or features. Thus, the exemplary terms "under" and "under" may include both upper and lower orientations. In addition, the device may also include additional orientations (e.g., rotated 90 degrees or other orientations), and the spatial descriptors used herein are interpreted accordingly.

[0041] When used herein, the singular forms "a", "an", and "said / the" may also include plural forms, unless the context clearly indicates otherwise. It should also be understood that when the terms "consisting of" and / or "comprising" are used in this specification, the presence of the features, integers, steps, operations, elements and / or parts can be determined, but the presence or addition of one or more other features, integers, steps, operations, elements, parts and / or groups is not excluded. At the same time, when used herein, the term "and / or" includes any and all combinations of the relevant listed items.

[0042] Embodiments of the invention are described herein with reference to cross-sectional views which are schematic diagrams of ideal embodiments (and intermediate structures) of the present application, so that variations in the shapes shown due to, for example, manufacturing techniques and / or tolerances can be expected. Therefore, embodiments of the present application should not be limited to the specific shapes of the regions shown herein, but rather include shape deviations due to, for example, manufacturing techniques. For example, an implanted region shown as a rectangle typically has rounded or curved features and / or an implant concentration gradient at its edges, rather than a binary change from an implanted region to a non-implanted region. Similarly, a buried region formed by implantation may result in some implantation in the region between the buried region and the surface through which the implantation is performed. Therefore, the regions shown in the figures are schematic in nature, their shapes do not represent the actual shape of the region of the device, and do not limit the scope of the present application.

[0043] In an embodiment of the present application, the substrate may include a top surface located on the front side and a bottom surface located on the back side opposite to the front side. Ignoring the planarity of the top surface and the bottom surface, the direction perpendicular to the top surface and the bottom surface of the substrate is defined as a third direction. A first direction and a second direction that intersect each other (e.g., are perpendicular to each other) are defined in the directions of the top surface and the bottom surface of the substrate (i.e., the plane where the substrate is located), wherein the first direction, the second direction, and the third direction are perpendicular to each other. In an embodiment of the present invention, the first direction is defined as the X-axis direction, the second direction is defined as the Y-axis direction, and the third direction is defined as the Z-axis direction.

[0044] Overlay is an important step in the semiconductor manufacturing process, which involves accurately superimposing different levels of patterns on the substrate to construct complex circuits. During the overlay process, in order to ensure overlay accuracy, the machine needs to align the layers by identifying the alignment marks in the alignment mark area.

[0045] In general technology, please refer to Figure 1 , the alignment pattern of the epitaxial layer 30 can be formed based on the alignment pattern of the substrate 10, but during the epitaxial process, due to the different growth rates of the epitaxial layer 30 on the bottom surface of the groove, the top corner, and the top surface of the substrate, the alignment pattern after epitaxy is deformed compared with the alignment pattern of the substrate 10, affecting the alignment accuracy after epitaxy. For example, please refer to Figure 2a-2dBefore forming the epitaxial layer 30, the alignment patterns of each layer present a standard line pattern under optical recognition, and the signal fluctuation of the alignment mark is large, which is easy to identify. However, after forming the epitaxial layer, the alignment pattern of the epitaxial layer is deformed and expanded, covering the alignment pattern of the previous layer, causing the signal of the alignment mark after growing the epitaxial layer 30 to be flattened, thereby reducing the alignment accuracy.

[0046] In some related technologies, the optical signal strength can be improved by optimizing the alignment mark pattern, sidewall protection, deposition filling, etc. However, traditional deposition, coating and other methods will inevitably affect the pattern of the device area, not only the protection effect is poor, but also the filling effect of the groove is poor, and the alignment accuracy cannot be improved well.

[0047] Based on the above questions, please refer to Figure 3 , the present application provides a method for preparing an alignment mark, including: step S302-step S306.

[0048] Step S302: providing a substrate, wherein the substrate includes an alignment mark area formed with a front-layer alignment pattern; wherein the front-layer alignment pattern includes a plurality of initial grooves arranged in parallel.

[0049] As an example, the substrate can be made of semiconductor material, insulating material, conductor material or any combination thereof. The substrate can be a single-layer structure or a multi-layer structure. For example, the substrate can be a silicon (Si) substrate, a silicon germanium (SiGe) substrate, a silicon germanium carbon (SiGeC) substrate, a silicon carbide (SiC) substrate, a gallium arsenide (GaAs) substrate, an indium arsenide (InAs) substrate, an indium phosphide (InP) substrate or other III / V semiconductor substrates or II / VI semiconductor substrates. Alternatively, for example, the substrate can be a layered substrate including Si / SiGe, Si / SiC, silicon on insulator (SOI) or silicon germanium on insulator. Therefore, the type of substrate should not limit the scope of protection of the present disclosure.

[0050] As an example, the substrate may further include a device region, and the device region is used to form a device film layer with certain functions.

[0051] As an example, the shape of the projection of the initial groove on the ZOY plane can be a rectangle, a regular trapezoid, an inverted trapezoid, or an irregular shape. The present application does not impose any specific restrictions on the shape of the initial groove.

[0052] Step S304: forming a current layer alignment pattern on the previous layer alignment pattern, wherein the current layer alignment pattern fills a plurality of initial grooves and exposes a surface of the substrate where no initial grooves are formed; wherein a top surface of the current layer alignment pattern is higher than a top surface of the initial grooves.

[0053] As an example, when the material properties of the layer alignment pattern are different from the material properties of the substrate.

[0054] Step S306: Covering the epitaxial layer on the front-layer alignment pattern and the current-layer alignment pattern; wherein the alignment mark includes the front-layer alignment pattern, the current-layer alignment pattern and the epitaxial layer.

[0055] In the above embodiment, a substrate is provided, the substrate includes an alignment mark area formed with a front layer alignment pattern, wherein the front layer alignment pattern includes a plurality of initial grooves arranged in parallel, a current layer alignment pattern is formed on the front layer alignment pattern, the current layer alignment pattern fills the plurality of initial grooves, and exposes the surface of the substrate where the initial grooves are not formed, so that the top surface of the current layer alignment pattern is higher than the top surface of the initial grooves, and the epitaxial layer is covered on the front layer alignment pattern and the current layer alignment pattern, wherein the alignment mark includes the front layer alignment pattern, the current layer alignment pattern and the epitaxial layer, thereby improving the alignment accuracy after epitaxy. The present application forms the current layer alignment pattern by using a material with different material properties from the substrate, so that the current layer alignment pattern, the substrate and the epitaxial layer can be distinguished during exposure of the machine, and the shape of the initial groove is protected by filling the initial groove with the current layer alignment pattern, so as to avoid deformation of the alignment mark, and the top surface of the current layer alignment pattern is higher than the top surface of the initial groove, so that there is a height difference between the current layer alignment pattern and the front layer alignment pattern, and the signal strength of different height differences is different, further improving the alignment accuracy after epitaxy.

[0056] In one embodiment, please refer to Figure 4 The forming of the current layer alignment pattern on the previous layer alignment pattern includes: step S402-step S408.

[0057] Step S402: forming a sacrificial layer on the front-layer alignment pattern; wherein the sacrificial layer includes a plurality of first openings, and the plurality of first openings expose a plurality of initial grooves.

[0058] As an example, see Figure 5 and Figure 6 , the depth of the initial groove 102 ranges from 50nm to 1000nm, for example: 100nm, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, etc.; when the difference between the thickness of the layer alignment pattern and the depth of the initial groove (i.e., the thickness of the sacrificial layer 20) ranges from 500nm to 3000nm, for example: 600nm, 700nm, 800nm, 900nm, 1000nm, 1200nm, 1500nm, 1800nm, 2000nm, 2200nm, 2500nm, 2800nm, 2900nm, etc.

[0059] As an example, the material of the sacrificial layer 20 may include but is not limited to organic materials such as polyimide-based photoresist materials, phenolic resin-based photoresist materials, and cyclized rubber-based photoresist materials. The present application does not impose any specific restrictions on the material of the sacrificial layer 20, as long as it can meet the requirements of being able to be selectively etched with the material of the layer alignment pattern and the material of the substrate 10.

[0060] Step S404: using a spin coating process to fill the target solution into the target groove formed by the first opening and the initial groove.

[0061] As an example, see Figure 7 , the spin coating thickness of the target solution 40 ranges from 800nm ​​to 4000nm, such as 900nm, 1000nm, 1200nm, 1500nm, 1800nm, 2000nm, 2200nm, 2500nm, 2800nm, 3000nm, 3200nm, 3500nm, 3800nm, etc. In the above example, the spin coating thickness of the target solution 40 is greater than the thickness of the current layer alignment pattern, so that it is convenient to subsequently planarize the target solution 40, improve the flatness of the current layer alignment pattern, and reserve a certain threshold for the shrinkage of the target solution 40 to avoid the height of the subsequent current layer alignment pattern not meeting the requirements.

[0062] As an example, the target solution 40 includes one or more of silica sol, ethyl orthosilicate, and methyl orthosilicate. In the above example, the target solution 40 such as silica sol is used to fill the target groove to generate silicon oxide, which not only ensures the crystal orientation matching degree of the epitaxial layer and the current layer alignment pattern, avoiding affecting the film quality of the epitaxial layer deposited subsequently, but also the target solution 40 such as silica sol has a high silicon content, which can improve the growth rate of the current layer alignment pattern.

[0063] In one embodiment, after the target solution is filled in the target groove formed by the first opening and the initial groove by the spin coating process, and before the target solution is treated at the first preset temperature, the step also includes: treating the target solution at a second preset temperature to form a solidified target solution, and planarizing the solidified target solution to form a target solution of a preset height.

[0064] The second preset temperature ranges from 60 degrees Celsius to 120 degrees Celsius, such as 70 degrees Celsius, 80 degrees Celsius, 90 degrees Celsius, 100 degrees Celsius, 110 degrees Celsius, etc. The preset height is the height of the current layer alignment pattern.

[0065] As an example, please refer to Figure 7 and Figure 8The target solution 40 on the top surface of the sacrificial layer 20 can be removed along the thickness direction by wet etching, dry etching, chemical mechanical polishing (CMP) or push etching process, so that the top surface of the solidified target solution 40 is flush with the top surface of the sacrificial layer 20.

[0066] In the above embodiment, the target solution 40 is first treated at a low temperature using a second preset temperature to solidify the target solution 40, thereby facilitating adjustment of the filling height of the target solution 40 and avoiding direct high temperature treatment of the target solution 40 to form hard materials such as silicon oxide, which makes it difficult to adjust the filling height.

[0067] Step S406: treating the target solution with a first preset temperature to form an alignment pattern in the current layer.

[0068] The first preset temperature ranges from 500 degrees Celsius to 800 degrees Celsius, such as 550 degrees Celsius, 600 degrees Celsius, 650 degrees Celsius, 700 degrees Celsius, 750 degrees Celsius, etc. As an example, please refer to Fig. 9 A first preset temperature high temperature annealing is performed to make the target solution, such as silica sol, generate silicon oxide to form the current layer alignment pattern 50, fill the initial groove, and protect the previous layer alignment pattern.

[0069] Step S408: removing the sacrificial layer.

[0070] As an example, see Fig.10 The material of the sacrificial layer is an organic material, and the sacrificial layer can be dry-etched by using an oxide gas such as oxygen, or wet-etched by using an acid or alkaline process. Since the physical and chemical properties of the current layer alignment pattern 50 are relatively stable, the sacrificial layer is formed by using an organic material, and then selectively etching the sacrificial layer by using a dry or wet etching process can avoid damaging the current layer alignment pattern 50 and the substrate 10.

[0071] In the above embodiment, a sacrificial layer is formed on the previous layer alignment pattern, and then a spin coating process is used to fill the target solution in the target groove formed by the first opening of the sacrificial layer and the initial groove, and then high-temperature annealing is performed to form the target solution into the current layer alignment pattern. Compared with the deposition process that requires crystal orientation matching between each film layer, the deposition process has a low growth rate, low growth quality, and a thin thickness of the film layer formed by deposition. The spin coating process in the present application is not limited by the crystal orientation and the thickness of the growing film layer, and has a fast growth rate and high growth quality, thereby improving the filling quality of the target groove and enhancing the alignment accuracy of the alignment mark.

[0072] In one embodiment, forming a sacrificial layer on the front-layer alignment pattern comprises: forming a photoresist layer on the front-layer alignment pattern, and etching the photoresist layer using an auxiliary mask including a first pattern to form the sacrificial layer.

[0073] Among them, please refer to Fig.11 The first pattern is located in the area corresponding to the alignment mark area in the auxiliary light mask 60, and covers the area corresponding to the device area to prevent light leakage from causing an erroneous pattern to be formed in the device area. The photoresist layer 210 at least covers the front alignment pattern of the alignment mark area. The shape of the first pattern corresponds to the shape of the first opening. When the material of the photoresist layer is positive photoresist, the position of the opening on the first pattern is the same as the position of the first opening; when the material of the photoresist layer is negative photoresist, the position of the opening on the first pattern is complementary to the position of the first opening.

[0074] As an example, the material of the photoresist layer 210 may include but is not limited to organic materials such as polyimide-based photoresist materials, phenolic resin-based photoresist materials, and cyclized rubber-based photoresist materials. The present application does not impose any specific restrictions on the material of the photoresist layer 210, as long as it can be selectively etched with the material of the layer alignment pattern and the material of the substrate 10.

[0075] In one embodiment, the forming of the sacrificial layer on the front-layer alignment pattern comprises the steps of forming a photoresist layer on the front-layer alignment pattern and etching the photoresist layer using a light shield to form the sacrificial layer.

[0076] As an example, see Fig.12 The covering size of the light shielding plate 70 can be changed by adjusting the linear distance L between the exposure center and the left frame of the light shielding plate 70, the linear distance T between the exposure center and the upper frame of the light shielding plate 70, the linear distance R between the exposure center and the right frame of the light shielding plate 70, and the linear distance B between the exposure center and the lower frame of the light shielding plate 70, and then the photoresist layer is etched in combination with the device mask, wherein the device mask includes an alignment mark area having a first pattern and a device area having a device pattern.

[0077] In the above embodiment, the photoresist layer is etched by combining a shading plate and a device mask, thereby avoiding the production of an auxiliary mask and reducing the economic cost. In addition, since the shading plate can limit the size of the exposure area, it avoids light leakage that causes the device area to form an erroneous pattern, thereby ensuring the accuracy of etching.

[0078] In one embodiment, the material of the layer alignment pattern is selected from one or more of silicon oxide, raw material hydrated yttrium nitrate, raw material hydrated zirconium nitrate, raw material nano-alumina powder, and the like.

[0079] As an example, the material of the layer alignment pattern may be other oxides besides silicon oxide, such as raw material hydrated yttrium nitrate, etc. The layer alignment pattern is formed by spin coating and annealing with a solution corresponding to the raw material.

[0080] In one embodiment, please refer to Fig.13 The method for preparing the alignment mark may specifically include:

[0081] Step 1: providing a substrate;

[0082] Step 2: performing a first photolithography-development process on the substrate to form a front layer alignment pattern;

[0083] Step 3: Apply photoresist, the thickness of which is greater than the depth of the target groove;

[0084] Step 4: using an exposure machine shield to define an exposure area, performing an exposure-development process, or using an auxiliary mask including a pattern of an alignment mark area to perform a second exposure-development process;

[0085] Step 5: obtaining a structure in which the initial trench is not filled with photoresist;

[0086] Step 6: Spin-coat the substrate with alkaline silica sol to fill the target groove with the silica sol, and use high-speed centrifugal force to remove part of the silica sol on the top surface of the photoresist;

[0087] Step 7: Bake at 60°C-120°C to solidify the silica sol, and remove the solidified silica sol on the top surface of the photoresist by CMP;

[0088] Step 8: removing the photoresist by wet method to form a protective structure of the solidified silica sol filling the target groove;

[0089] Step nine: high temperature baking at 500°C-800°C is used to generate a silicon dioxide protection structure in situ in the target groove;

[0090] Step 10: Obtain alignment marks with high contrast and high signal accuracy after epitaxy.

[0091] It should be understood that although Figure 3 , Figure 4 and Fig.13 The steps in the flowchart are shown in sequence as indicated by the arrows, but these steps are not necessarily executed in the order indicated by the arrows. Unless otherwise specified in this document, there is no strict order restriction for the execution of these steps, and these steps can be executed in other orders. Figure 3 , Figure 4 and Fig.13 At least part of the steps may include multiple steps or multiple stages. These steps or stages are not necessarily performed at the same time, but can be performed at different times. The execution order of these steps or stages is not necessarily sequential, but can be performed in turn or alternately with other steps or at least part of the steps or stages in other steps.

[0092] See also Fig.14 , the present application also provides a semiconductor structure, comprising:

[0093] The substrate 10 includes an alignment mark area formed with a front-layer alignment pattern; wherein the front-layer alignment pattern includes a plurality of initial grooves arranged in parallel.

[0094] As an example, multiple initial grooves can be arranged along the Y-axis direction, along the X-axis direction, or along any direction in the XOY plane. The present application does not impose any specific limitation on the arrangement direction of the initial grooves.

[0095] The layer alignment pattern 50 is located on the previous layer alignment pattern, and the layer alignment pattern fills a plurality of initial grooves and exposes the surface of the substrate 10 where no initial grooves are formed; wherein the top surface of the layer alignment pattern is higher than the top surface of the initial grooves.

[0096] The epitaxial layer 30 covers the front layer alignment pattern and the current layer alignment pattern 50; wherein the alignment mark includes the front layer alignment pattern, the current layer alignment pattern 50 and the epitaxial layer.

[0097] In the above embodiments, the present application forms a current layer alignment pattern on the front layer alignment pattern of the substrate, and the current layer alignment pattern fills the initial groove, thereby protecting the shape of the initial groove and avoiding deformation of the alignment mark. The top surface height of the current layer alignment pattern is higher than the top surface of the initial groove. Since the optical signal intensity is related to the thickness of the film layer, the current layer alignment pattern and the front layer alignment pattern have a height difference, thereby improving the alignment accuracy after epitaxy.

[0098] In one embodiment, the depth of the initial groove ranges from 50 nm to 1000 nm; and the difference between the thickness of the layer alignment pattern and the depth of the initial groove ranges from 500 nm to 3000 nm.

[0099] In one embodiment, the material of the layer alignment pattern includes but is not limited to silicon oxide, raw material hydrated yttrium nitrate, raw material hydrated zirconium nitrate, and raw material nano-aluminum oxide powder.

[0100] The method for preparing the alignment mark and the semiconductor structure of the present application have the following beneficial effects:

[0101] The preparation method of the alignment mark and the semiconductor structure of the present application provide a substrate, wherein the substrate includes an alignment mark area formed with a front-layer alignment pattern, wherein the front-layer alignment pattern includes a plurality of initial grooves arranged in parallel, a current-layer alignment pattern is formed on the front-layer alignment pattern, the current-layer alignment pattern fills the plurality of initial grooves, and exposes the surface of the substrate where the initial grooves are not formed, so that the top surface of the current-layer alignment pattern is higher than the top surface of the initial grooves, and an epitaxial layer is covered on the front-layer alignment pattern and the current-layer alignment pattern, wherein the alignment mark includes the front-layer alignment pattern, the current-layer alignment pattern and the epitaxial layer, thereby improving the alignment accuracy after epitaxy. The present application protects the shape of the initial groove and avoids deformation of the alignment mark by filling the initial groove with the current-layer alignment pattern, and the top surface of the current-layer alignment pattern is higher than the top surface of the initial groove, so that there is a height difference between the current-layer alignment pattern and the front-layer alignment pattern, and the signal strength of different height differences is different, further improving the alignment accuracy after epitaxy.

[0102] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features of the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0103] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.

Claims

1. A method for preparing an alignment mark, characterized in that: include: Providing a substrate, the substrate comprising an alignment mark area formed with a front layer alignment pattern; wherein the front layer alignment pattern comprises a plurality of initial grooves arranged in parallel; forming a sacrificial layer on the front layer alignment pattern; wherein the sacrificial layer comprises a plurality of first openings, and the plurality of first openings expose the plurality of initial grooves; Filling a target solution into a target groove formed by the first opening and the initial groove by a spin coating process; Treating the target solution with a first preset temperature to form an alignment pattern; The sacrificial layer is removed; the current layer alignment pattern fills the multiple initial grooves and exposes the surface of the substrate where the initial grooves are not formed; wherein the top surface of the current layer alignment pattern is higher than the top surface of the initial grooves; Covering the epitaxial layer on the front layer alignment pattern and the current layer alignment pattern; wherein the alignment mark includes the front layer alignment pattern, the current layer alignment pattern and the epitaxial layer; Wherein, after the target solution is filled into the target groove formed by the first opening and the initial groove by the spin coating process, and before the target solution is treated at a first preset temperature, the method further includes: Treating the target solution with a second preset temperature to form a solidified target solution; The solidified target solution is leveled to form a target solution with a preset height.

2. The method for preparing an alignment mark according to claim 1, characterized in that: The first preset temperature ranges from 500 degrees Celsius to 800 degrees Celsius; the second preset temperature ranges from 60 degrees Celsius to 120 degrees Celsius.

3. The method for preparing an alignment mark according to claim 1, characterized in that: The forming of a sacrificial layer on the front layer alignment pattern comprises: forming a photoresist layer on the front layer alignment pattern; The photoresist layer is etched using an auxiliary mask including a first pattern to form the sacrificial layer.

4. The method for preparing an alignment mark according to claim 1, characterized in that: The forming of a sacrificial layer on the front layer alignment pattern comprises: forming a photoresist layer on the front layer alignment pattern; The photoresist layer is etched by using a light shielding plate to form the sacrificial layer.

5. The method for preparing an alignment mark according to claim 1, characterized in that: The target solution includes one or more of silica sol, ethyl orthosilicate, and methyl orthosilicate.

6. The method for preparing an alignment mark according to claim 1, characterized in that: The depth of the initial groove ranges from 50nm to 1000nm; the difference between the thickness of the current layer alignment pattern and the depth of the initial groove ranges from 500nm to 3000nm.

7. The method for preparing an alignment mark according to claim 1, characterized in that: The material of the layer alignment pattern is selected from one or more of silicon oxide, raw material hydrated yttrium nitrate, raw material hydrated zirconium nitrate, and raw material nano-alumina powder.

8. The method for preparing an alignment mark according to claim 1, characterized in that: The spin coating thickness of the target solution ranges from 800nm ​​to 4000nm.

9. The method for preparing an alignment mark according to claim 1, characterized in that: The material of the sacrificial layer is an organic material.

10. A semiconductor structure, characterized in that: The alignment mark is prepared by the method for preparing the alignment mark according to claim 1.