A colorful environmentally friendly paving paint and preparation process

By adding maleic anhydride graft polymer to the MMA color environmentally friendly pavement coating, the problem of ceramic particles being unable to be immersed is solved, the compatibility and adhesion with the pavement coating are improved, the service life of the pavement is extended and the Weather resistance.

CN118580700BActive Publication Date: 2024-10-29ZHEJIANG TIANCHENG TRANSPORTATION TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411050817.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-10-29
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

Due to the fast curing speed of existing MMA color anti-skid road coatings, the ceramic particles cannot be completely immersed in the paint, resulting in poor adhesion firmness, the ceramic particles are easy to fall off, and the service life is shortened.

Method used

Maleic anhydride graft polymer is added to the MMA color environmentally friendly pavement coating. The maleic anhydride graft polymer improves the compatibility between the pavement coating and ceramic particles, so that the ceramic particles can be quickly immersed in the paint and cured. adhere tightly to avoid falling off.

Benefits of technology

It improves the service life of paved roads, enhances the adhesion between ceramic particles and coatings, prolongs the firmness and service life of the pavement, and improves the oxidation resistance and weather resistance of the coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118580700B_ABST
    Figure CN118580700B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of colored pavement coatings, and in particular to a colored environmentally friendly pavement coating and a preparation process thereof, comprising: a component A and a component B, wherein the ratio of the component A to the component B is 1:1; in parts by weight, the component A comprises 30-60 parts of methyl methacrylate monomer, 10-30 parts of functional acrylate monomer, 10-20 parts of pigment, 1-2 parts of leveling agent, 10-20 parts of maleic anhydride grafted polymer with a grafting rate of 12.5-14.5%, 0.5-2 parts of antioxidant, 2-4 parts of dispersant, and the like. 3-8 parts of solvent, 0.5-1.5 parts of accelerator, component B includes 30-60 parts of methyl methacrylate monomer, 10-30 parts of functional acrylate monomer, 5-15 parts of curing agent, 1-2 parts of leveling agent, 0.5-1 parts of dispersant, and 0.5-2 parts of antioxidant. By adding maleic anhydride grafted polymer to the existing MMA color environmentally friendly paving paint, the compatibility of the paving paint and ceramic particles is improved by using maleic anhydride grafted polymer, so that the ceramic particles can be quickly immersed in the paving paint.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of colored road paving paint, and in particular to a colored environmentally friendly paving paint and a preparation process thereof. Background Art

[0002] Colored paving paint is a material used for ground decoration and anti-skid treatment in roads, squares, parking lots, etc. It has a variety of colors to choose from, which can make the road surface present a bright and beautiful effect, while also providing good anti-skid performance.

[0003] The main performance characteristics of colored paving paint include: long-lasting bright colors that are not easy to fade, and various colors and patterns can be matched and designed according to needs to enhance visual effects and warnings; it has strong bonding strength with substrates such as asphalt, cement concrete, etc. to ensure that the coating is not easy to fall off; the construction period is short, and traffic can be opened quickly to reduce the impact on road use; it is not easy to crack, burst or fall off under the vibration of vehicle driving and slight deformation of the road surface; it has good corrosion resistance, weather resistance and temperature difference resistance, can adapt to different climatic conditions and extend the service life; it can effectively increase the friction coefficient of the road surface, shorten the braking distance, reduce slipping, and improve driving safety; it has a long service life; it can isolate the original road surface from water, enhance the road surface's resistance to rutting, and prevent the road surface from cracking; it is less affected by construction environmental factors, and conventional construction methods such as spraying and scraping can be used.

[0004] There are many kinds of color paving paint products on the market, and their performance and characteristics may vary. Common products include epoxy polyurethane adhesives, color pavement sprays, MMA color anti-skid pavement paints, etc. The color paving paint in this application is MMA color anti-skid pavement paint. MMA color anti-skid pavement paint has the characteristics of fast curing, allowing people to walk in 40 minutes, allowing traffic to pass in 2 hours, normal construction at minus 30 degrees Celsius, long-term durable use in various extreme environments, and strong bonding with various substrates, and is widely used in pavement construction.

[0005] However, due to the fast curing speed of MMA color anti-skid pavement coating and the fact that MMA color anti-skid pavement coating is a non-polar material with poor compatibility with polar ceramic particles, during construction, the ceramic particles have not been completely immersed in the paving coating, and the paving coating has already cured, which greatly affects the adhesion of the coating to the ceramic particles, and in turn causes the ceramic particles of the formed color paving pavement to fall off easily, greatly reducing the service life.

[0006] In a Chinese patent with patent application number 202211676175.5, an MMA polymer slow-release anti-icing colored anti-slip paving material and its preparation process and construction method are disclosed. A slow-release anti-icing component is added to the paving material, making the paving material self-melting, anti-icing, weather-resistant, water-resistant, and strong in tensile strength and flexural strength.

[0007] However, the above-mentioned MMA polymer slow-release anti-coagulation ice color anti-skid paving material does not solve the problem that the ceramic particles cannot be immersed in the coating due to rapid solidification, resulting in the ceramic particles easily falling off.

[0008] Therefore, there is an urgent need for a method that can, based on the existing MMA colored anti-slip paving paint, maintain the rapid curing of the paint while improving the compatibility between ceramic particles and the paint, so that the ceramic particles can be quickly immersed in the paint and the adhesion of the paint to the ceramic particles is enhanced. Summary of the invention

[0009] In view of the above problems, the present invention provides a colorful and environmentally friendly paving coating and a preparation process. On the basis of the existing MMA colorful and environmentally friendly paving coating, a maleic anhydride grafted polymer is added, and the compatibility of the paving coating and ceramic particles is improved by using the maleic anhydride grafted polymer, so that the ceramic particles can be quickly immersed in the paving coating, and then when the paving coating is quickly solidified, the ceramic particles have been tightly adhered to the paving coating, thereby avoiding the shedding of the ceramic particles and increasing the service life of the paved road surface.

[0010] To achieve the above object, the present invention provides the following technical solutions:

[0011] A colorful environmentally friendly paving paint, comprising:

[0012] Component A and component B, the ratio of component A to component B is 1:1;

[0013] In parts by weight, the component A includes 30-60 parts of methyl methacrylate monomer, 10-30 parts of functional acrylate monomer, 10-20 parts of pigment, 1-2 parts of leveling agent, 10-20 parts of maleic anhydride grafted polymer with a grafting rate of 12.5-14.5%, 0.5-2 parts of antioxidant, 2-4 parts of dispersant, 3-8 parts of compatibilizer, and 0.5-1.5 parts of accelerator;

[0014] The B component includes 30-60 parts of methyl methacrylate monomer, 10-30 parts of functional acrylate monomer, 5-15 parts of curing agent, 1-2 parts of leveling agent, 0.5-1 parts of dispersant and 0.5-2 parts of antioxidant.

[0015] Preferably, the functional acrylate monomer is one or more of isotridecyl acrylate, 1,4-cyclohexanedimethanol diacrylate, ethoxyethoxyethyl acrylate, 1,6-hexanediol dimethacrylate, and 2-propoxylated neopentyl glycol diacrylate.

[0016] Preferably, the maleic anhydride grafted polymer is one or more of polypropylene grafted maleic anhydride, polyethylene grafted maleic anhydride and polystyrene grafted maleic anhydride.

[0017] Preferably, the antioxidant is one or more of antioxidant 1010, antioxidant 168, and antioxidant 1076.

[0018] Preferably, in component A, the dispersant is a mixture of one or more of polyvinyl alcohol, cellulose, polyvinyl pyrrolidone and one or more of ethylene bisstearamide and zinc stearate;

[0019] In component B, the dispersant is one or more of polyvinyl alcohol, cellulose and polyvinyl pyrrolidone.

[0020] Preferably, the compatibilizer is one or more of styrene-maleic anhydride copolymer and methyl methacrylate-butadiene-styrene copolymer.

[0021] Preferably, the curing agent is one or more of dibenzoyl peroxide, dicumyl peroxide, tert-butyl peroxide, cyclohexanone peroxide, and methyl ethyl ketone peroxide.

[0022] Preferably, the accelerator is one or more of N,N-dimethyl-p-methylaniline, cobalt isooctanoate, cobalt naphthenate, and cobalt cyclohexaneate.

[0023] In addition, the present invention also provides a process for preparing the above-mentioned colorful environmentally friendly paving paint.

[0024] The preparation process of component A is:

[0025] a1. Add methyl methacrylate monomer, functional acrylate monomer, maleic anhydride grafted polymer, 3 / 4 of compatibilizer, leveling agent and 1 / 2 of dispersant in component A into a high-speed stirring kettle according to the proportion, stir at a speed of 1500 rpm for 15-25 min, heat to 65-70°C, stir for 10-15 min, heat to 80-100°C, stir at a speed of 1500 rpm, and stir for 30-60 min;

[0026] a2. Add pigment, remaining compatibilizer and dispersant into a high-speed stirring kettle according to the proportion, cool to 65-70°C, stir at 3000rpm, stir for 20-30min and let stand for 50-60min;

[0027] a3. Add antioxidant and accelerator into the high-speed stirring kettle according to the proportion, stir at a speed of 1500 rpm, stir for 15-20 minutes, cool to below 35°C, and obtain component A of the colored environmentally friendly paving coating;

[0028] The preparation process of component B is:

[0029] b1. Add methyl methacrylate monomer, functional acrylate monomer, leveling agent and dispersant in component B into a high-speed stirring kettle according to the proportion, stir at a speed of 3000 rpm, stir for 15-25 minutes, heat to 65-70°C, and stir for 10-15 minutes;

[0030] b2. Add the curing agent into the high-speed stirring kettle according to the proportion, stirring at a speed of 3000rpm for 15-25min;

[0031] b3. Add the antioxidant into the high-speed stirring kettle according to the proportion, the stirring speed is 1500rpm, stir for 15-20min, cool to below 35℃, and obtain component B of the colorful environmentally friendly paving coating.

[0032] Preferably, when preparing the maleic anhydride grafted polymer used in step a1, after the polymer, interfacial agent, initiator, antioxidant and maleic anhydride are melt-blended and extruded to form a grafted crude material, the grafted crude material circulates in an ultraviolet irradiation device and is irradiated with ultraviolet rays for 50-80 minutes, and the grafting rate of the grafted crude material after ultraviolet irradiation is set to increase as the cross-sectional thickness of the grafted crude material flowing inside the ultraviolet irradiation device decreases.

[0033] The beneficial effects of the present invention are:

[0034] (1) The present invention adds maleic anhydride grafted polymer to the existing MMA color environmentally friendly paving paint. The maleic anhydride grafted polymer can be used as a bridge to enhance the adhesion and compatibility between polar materials and non-polar materials. The maleic anhydride grafted polymer introduces a strongly polar side group on the molecular main chain, which can improve the polarity and reactivity of the MMA two-component resin, thereby improving its compatibility with ceramic particles. At the same time, the maleic anhydride grafted polymer can also be used as a polymer interface coupling agent to promote the chemical bonding between the MMA two-component resin and the ceramic particles, further improving the compatibility, so that the ceramic particles can be quickly immersed in the paving paint, and then when the paving paint is quickly cured, the ceramic particles have been tightly adhered to the paving paint, avoiding the shedding of the ceramic particles and increasing the service life of the paved road surface;

[0035] (2) The present invention utilizes the maleic anhydride grafted polymer to react chemically with the functional groups in the MMA color environmentally friendly paving paint to form chemical bonds, thereby improving the adhesion, enhancing the adhesion between the MMA color environmentally friendly paving paint and the road base, and thereby improving the firmness and service life of the constructed color paving road surface. The specific reaction principle is as follows:

[0036] Maleic anhydride reacts with hydroxyl group to undergo esterification reaction, and the hydrogen atom of hydroxyl group reacts with the carbonyl group of maleic anhydride to form an ester bond. The reaction equation is: R-OH+Maleic Anhydride→R-OCO-CH=CH-COOH. R is the organic group in MMA two-component resin.

[0037] Maleic anhydride reacts with the amine group to undergo an amidation reaction, and the nitrogen atom of the amine group reacts with the carbonyl group of maleic anhydride to form an amide bond. The reaction equation is: R-NH2+MaleicAnhydride→R-NHCO-CH=CH-COOH. R is the organic group in the MMA two-component resin.

[0038] Among them, the chemical properties and spatial structures of ester bonds and amide bonds will promote the viscosity of MMA color environmentally friendly paving coatings. In addition, ester bonds help to enhance the cross-linking degree of MMA color environmentally friendly paving coatings, while amide bonds help to enhance the interaction between molecules, which all help to enhance the viscosity of MMA color environmentally friendly paving coatings.

[0039] (3) The maleic anhydride grafted polymer in the present invention can absorb and disperse ultraviolet rays, reduce the damage of ultraviolet rays to the MMA color environmentally friendly paving paint, and at the same time can improve the antioxidant property of the MMA color environmentally friendly paving paint and delay the aging process of the MMA color environmentally friendly paving paint;

[0040] (4) The content of maleic anhydride grafted polymer in the present invention cannot be too much, as too much will destroy the original formula structure of MMA color environmentally friendly paving paint and generate a large amount of Voc gas. Therefore, it is necessary to form a higher grafting rate as much as possible on the basis of a certain amount of maleic anhydride grafted polymer, so as to form enough maleic anhydride groups for use in the compatibility modification of MMA color environmentally friendly paving paint. By using an ultraviolet irradiation device, the prepared maleic anhydride crude material is irradiated, so that the photoinitiator absorbs the energy of ultraviolet light and transitions from the ground state to the excited state. The excited state photoinitiator has a strong hydrogen abstraction effect, which can both open the maleic anhydride monomer and extract hydrogen from the polymer molecular chain, thereby generating polymer free radicals. These free radicals can trigger a grafting reaction between maleic anhydride monomers and polymer molecular chains, grafting maleic anhydride onto the polymer, thereby forming a maleic anhydride grafted polymer with a high grafting rate. In addition, the ultraviolet irradiation device can further increase the grafting rate of the maleic anhydride grafted polymer by regulating the liquid flow thickness and irradiation frequency of the grafted coarse material, so that the maleic anhydride grafted polymer of the present invention can also well improve the compatibility and viscosity of the MMA color environmentally friendly paving coating under the condition of controlling the addition amount.

[0041] (5) The transparent inner cylinder of the ultraviolet irradiation device of the present invention can automatically adjust the cross-sectional height of the annular flow channel when rotating, so that the single-ring annular flow channel can be adjusted to a double-ring annular flow channel. At the same time, in the process of switching from the single-ring annular flow channel to the double-ring annular flow channel, the switching can be carried out gradually, so that the grafting rate of the maleic anhydride grafted polymer can be adjusted in multiple levels, while the ultraviolet irradiation rate can be guaranteed.

[0042] In summary, the present invention has the advantages of being green and environmentally friendly, good compatibility of MMA colored environmentally friendly paving paint with ceramic particles, and long service life of the constructed paved road surface, and is particularly suitable for the technical field of colored pavement paint for pavement. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 This is a three-dimensional diagram of an ultraviolet irradiation device according to an embodiment of the present invention;

[0044] Figure 2 It is a transverse cross-sectional view of an ultraviolet irradiation device according to an embodiment of the present invention;

[0045] Figure 3 A longitudinal cross-sectional view of an ultraviolet irradiation device according to an embodiment of the present invention Figure 1 ;

[0046] Figure 4 A longitudinal cross-sectional view of an ultraviolet irradiation device according to an embodiment of the present invention Figure 2 ;

[0047] Figure 5This is a schematic diagram of the partial structure of the ultraviolet irradiation device according to an embodiment of the present invention;

[0048] Figure 6 This is a schematic diagram of the transparent outer cylinder structure of an embodiment of the present invention;

[0049] Figure 7 This is a schematic diagram of the partial structure of the transparent inner cylinder according to an embodiment of the present invention;

[0050] Figure 8 This is a schematic diagram of the three-dimensional structure of the middle section of the transparent inner cylinder according to an embodiment of the present invention;

[0051] Fig. 9 This is a schematic diagram of the three-dimensional structure of the tail section of the transparent inner tube according to an embodiment of the present invention;

[0052] Fig.10 This is a schematic diagram of the three-dimensional structure of the tail section of the transparent inner tube according to an embodiment of the present invention;

[0053] Fig.11 It is a schematic diagram of the cross-sectional structure of the transparent inner cylinder according to an embodiment of the present invention.

[0054] In the figure: feed area 100, discharge area 200, annular flow channel 300, single annular flow channel 300a, double annular flow channel 300b, shell 1, cylinder 11, feed nozzle 111, discharge nozzle 112, connecting line nozzle 113, sealing end cover 12, opening end cover 13, hole 131, transparent outer cylinder 2, inner convex block 201, inner groove 202, ring part 21, arc-shaped transparent cover 22, connecting port 221, transparent inner cylinder 3, head Segment 311, middle section 312, tail section 313, driven gear 31, motor 32, driving gear 33, driven ring gear 34, rotating shaft 35, linkage gear 351, transfer gear 36, transmission gear 37, driving gear 38, driving motor 39, outer protrusion 301, outer groove 302, outer light-emitting element 4, end light-emitting element 5, transparent spherical cover 51, spherical channel 511, central light-emitting element 6, mounting seat 61. DETAILED DESCRIPTION

[0055] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0056] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0057] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0058] Example:

[0059] A colorful environmentally friendly paving paint, comprising:

[0060] Component A and component B, the ratio of component A to component B is 1:1;

[0061] In parts by weight, the component A includes 30-60 parts of methyl methacrylate monomer, 10-30 parts of functional acrylate monomer, 10-20 parts of pigment, 1-2 parts of leveling agent, 10-20 parts of maleic anhydride grafted polymer with a grafting rate of 12.5-14.5%, 0.5-2 parts of antioxidant, 2-4 parts of dispersant, 3-8 parts of compatibilizer, and 0.5-1.5 parts of accelerator, wherein the functional acrylate monomer is preferably one or more of isotridecyl acrylate, 1,4-cyclohexanedimethanol diacrylate, ethoxyethoxyethyl acrylate, 1,6-hexanediol dimethacrylate, and 2-propoxy neopentyl glycol diacrylate. The maleic anhydride grafted polymer is preferably one or more of polypropylene grafted maleic anhydride, polyethylene grafted maleic anhydride and polystyrene grafted maleic anhydride, the antioxidant is preferably one or more of antioxidant 1010, antioxidant 168 and antioxidant 1076, the compatibilizer is preferably one or more of styrene-maleic anhydride copolymer and methyl methacrylate-butadiene-styrene copolymer, the accelerator is preferably one or more of N,N-dimethyl-p-methylaniline, cobalt isooctanoate, cobalt naphthenate and cobalt cyclohexaneate, the pigment is preferably one or more of titanium dioxide, iron oxide pigment, chrome yellow and chrome green, and the leveling agent is preferably silicone oil or polyether-modified silicone oil;

[0062] The B component includes 30-60 parts of methyl methacrylate monomer, 10-30 parts of functional acrylate monomer, 5-15 parts of curing agent, 1-2 parts of leveling agent, 0.5-1 parts of dispersant, and 0.5-2 parts of antioxidant. In the A component, the dispersant is preferably a mixture of one or more of polyvinyl alcohol, cellulose, and polyvinyl pyrrolidone and one or more of ethylene bisstearamide and zinc stearate;

[0063] In component B, the dispersant is preferably one or more of polyvinyl alcohol, cellulose, and polyvinyl pyrrolidone;

[0064] The curing agent is preferably one or more of dibenzoyl peroxide, dicumyl peroxide, tert-butyl peroxide, cyclohexanone peroxide, and methyl ethyl ketone peroxide.

[0065] Among them, methyl methacrylate monomer was purchased from Sinopec, functional acrylate monomer was purchased from Hangzhou Huiyun Chemical Co., Ltd., pigment was purchased from Jiangsu Yihua Chemical Co., Ltd., leveling agent was purchased from Zhejiang Xin'an Chemical Group Co., Ltd., antioxidant was purchased from Jiangsu Ruipu Biotechnology Co., Ltd., polyvinyl alcohol was purchased from Sinopec Shanghai Petrochemical Co., Ltd., cellulose was purchased from Shandong Hailide Biotechnology Co., Ltd., polyvinyl pyrrolidone was purchased from Shanghai Jiafeng Industrial Co., Ltd., ethylene bisstearamide was purchased from Ningbo Haiyue Chemical Co., Ltd., zinc stearate was purchased from Zhejiang Jiangshan Chemical Co., Ltd., curing agent was purchased from Taizhou Sanxin Chemical Co., Ltd., Zhejiang Province, and accelerator was purchased from Nanjing Nengde New Material Technology Co., Ltd.

[0066] A process for preparing the above-mentioned colored environmentally friendly paving coating, wherein the preparation process of component A is:

[0067] a1. Add methyl methacrylate monomer, functional acrylate monomer, maleic anhydride grafted polymer, 3 / 4 of compatibilizer, leveling agent and 1 / 2 of dispersant in component A into a high-speed stirring kettle according to the proportion, stir at a speed of 1500 rpm for 15-25 min, heat to 65-70°C, stir for 10-15 min, heat to 80-100°C, stir at a speed of 1500 rpm, and stir for 30-60 min;

[0068] a2. Add pigment, remaining compatibilizer and dispersant into a high-speed stirring kettle according to the proportion, cool to 65-70°C, stir at 3000rpm, stir for 20-30min and let stand for 50-60min;

[0069] a3. Add antioxidant and accelerator into the high-speed stirring kettle according to the proportion, stir at a speed of 1500 rpm, stir for 15-20 minutes, cool to below 35°C, and obtain component A of the colored environmentally friendly paving coating;

[0070] The preparation process of component B is:

[0071] b1. Add methyl methacrylate monomer, functional acrylate monomer, leveling agent and dispersant in component B into a high-speed stirring kettle according to the proportion, stir at a speed of 3000 rpm, stir for 15-25 minutes, heat to 65-70°C, and stir for 10-15 minutes;

[0072] b2. Add the curing agent into the high-speed stirring kettle according to the proportion, stirring at a speed of 3000rpm for 15-25min;

[0073] b3. Add the antioxidant into the high-speed stirring kettle according to the proportion, the stirring speed is 1500rpm, stir for 15-20min, cool to below 35℃, and obtain component B of the colorful environmentally friendly paving coating.

[0074] Preferably, when preparing the maleic anhydride grafted polymer used in step a1, after the polymer, interfacial agent, initiator, antioxidant and maleic anhydride are melt-blended and extruded to form a grafted crude material, the grafted crude material circulates in an ultraviolet irradiation device and is irradiated by ultraviolet light for 50-80 minutes, and the grafting rate of the grafted crude material after ultraviolet irradiation increases with the decrease of the cross-sectional thickness of the grafted crude material flowing inside the ultraviolet irradiation device, wherein the polymer is preferably one or more of polypropylene, polyethylene and polystyrene, the interfacial agent is preferably xylene, the initiator is a photoinitiator, preferably one or more of diisopropyl peroxide, isopropylthioxanthone, 4-dimethylaminoethyl ester or 2959, and the antioxidant is preferably one or more of antioxidant 1010 or antioxidant 168.

[0075] like Figures 1 to 11 As shown, in addition, the present invention also provides an ultraviolet irradiation device for improving the grafting rate of the prepared maleic anhydride grafted polymer, and the ultraviolet irradiation device comprises:

[0076] Shell 1, transparent outer tube 2, transparent inner tube 3, outer light emitting element 4, end light emitting element 5 and center light emitting element 6;

[0077] The housing 1 comprises a cylindrical body 11, a sealing end cover 12 and an opening end cover 13. The cylindrical body 11 is provided with openings at both ends. The sealing end cover 12 and the opening end cover 13 are respectively provided at the openings at both ends of the cylindrical body 11. The sealing end cover 12, the opening end cover 13 and the cylindrical body 11 are connected by threaded fasteners, and a sealing ring is provided on the sealing mating end surface.

[0078] The cylindrical body 11 is provided with a feed nozzle 111 and a discharge nozzle 112, which are respectively arranged at the two ends of the cylindrical body 11, and the feed nozzle 111 and the discharge nozzle 112 are respectively connected to the blending equipment of the maleic anhydride grafted polymer through pipelines, and the feed nozzle 111 is arranged at the upper part of the cylindrical body 11, and the discharge nozzle 112 is arranged at the lower part of the cylindrical body 11. The maleic anhydride grafted crude material after blending is input into the feed nozzle 111. In the ultraviolet irradiation device, after ultraviolet irradiation, the material is output through the discharge nozzle 112, and the output maleic anhydride grafted crude material flows into the blending device, and then output again, and is input into the ultraviolet irradiation device through the feed nozzle 111, and the cycle is repeated until the ultraviolet irradiation is completed, wherein the inner side walls of the cylinder 11, the sealing end cover 12 and the open end cover 13 are all coated with ultraviolet reflective material, which can reflect 80-90% of ultraviolet rays, and the ultraviolet reflective material is preferably polytetrafluoroethylene;

[0079] The two ends of the transparent outer cylinder 2 are open, and the middle protrusion of the transparent outer cylinder 2 is provided with two groups of parallel ring parts 21, and the ring parts 21 are in contact and sealed with the inner side wall of the cylindrical body 11, and an O-ring is also provided at the contact and sealed position for sealing; a feed area 100 and a discharge area 200 separated from each other are formed between the cylindrical body 11 and the transparent outer cylinder 2, and the feed area 100 is connected with the feed nozzle 111, and the discharge area 200 is connected with the discharge nozzle 112, and a plurality of external light-emitting elements 4 are installed in the side wall of the transparent outer cylinder 2, and the external light-emitting elements 4 are arranged in an array around the circumference of the side wall of the transparent outer cylinder 2, and the inner layer of the grafted coarse material flowing in the feed area 100 and the discharge area 200 is irradiated with ultraviolet rays, and the power supply connection line of the external light-emitting element 4 is connected to the external power supply device through the connection line nozzle 113 provided on the cylindrical body 11;

[0080] The transparent inner cylinder 3 is coaxially inserted inside the transparent outer cylinder 2, and an annular flow channel 300 is formed between the transparent inner cylinder 3 and the transparent outer cylinder 2. The feed area 100 and the discharge area 200 are connected through the annular flow channel 300. The central light-emitting element 6 is arranged at the inner central axis of the transparent inner cylinder 3. The central light-emitting element 6 irradiates the inner layer of the grafted crude material flowing in the annular flow channel 300 with ultraviolet rays, and the outer light-emitting element 4 irradiates the outer layer of the grafted crude material flowing in the annular flow channel 300 with ultraviolet rays.

[0081] The end light emitting element 5 is arranged at the feeding area 100, and the end light emitting element 5 is installed in the sealing end cover 12, and the end light emitting element 5 is separated from the feeding area 100 by a transparent spherical cover 51, and the end of the transparent outer cylinder 2 corresponding to the transparent spherical cover 51 is installed with an arc-shaped transparent cover 22 with a central opening, and a spherical channel 511 is formed between the arc-shaped transparent cover 22 and the transparent spherical cover 51, and the spherical channel 511 is connected with the feeding area 100 and the annular flow channel 300 through the connecting port 221 on the arc-shaped transparent cover 22, and the end light emitting element 5 irradiates the outer layer of the grafted coarse material flowing in the spherical channel 511 with ultraviolet rays;

[0082] The end of the transparent inner cylinder 3 corresponding to the spherical channel 511 is semi-spherical and sealed, and the semi-spherical end is roughly dispersed and diverted for the graft input into the connecting port 221. The other end of the transparent inner cylinder 3 is open, and the open end of the transparent inner cylinder 3 passes through the hole 131 on the open end cover 13 for the central light-emitting element 6 to be inserted into the transparent inner cylinder 3. The transparent inner cylinder 3 and the open end cover 13 are sealed and matched, and the central light-emitting element 6 is connected to the open end cover 13 through a mounting seat 61.

[0083] The blended maleic anhydride grafted crude material input by the feed nozzle 111 first enters the feed zone 100, and the inner layer of the feed zone is irradiated with ultraviolet light by the outer light-emitting element 4. Then, the maleic anhydride grafted crude material is transferred to the spherical channel 511, and the outer layer of the maleic anhydride grafted crude material located at the spherical channel 511 is irradiated with ultraviolet light by the end light-emitting element 5. Then, the maleic anhydride grafted crude material enters the annular flow channel 300, and the inner and outer layers of the maleic anhydride grafted crude material are irradiated with ultraviolet light by the outer light-emitting element 4 and the central light-emitting element 6. During the entire ultraviolet light irradiation process, the maleic anhydride grafted crude material is continuously and continuously irradiated with ultraviolet light.

[0084] In addition, the outer light-emitting element 4, the end light-emitting element 5 and the central light-emitting element 6 are preferably LED ultraviolet lamps purchased from Sanyo Electric of China. The ultraviolet wavelength is preferably 254nm, that is, the UVC band. The transparent outer cylinder 2, the transparent inner cylinder 3, the arc-shaped transparent cover 22, and the transparent spherical cover 51 can be quartz, glass, resin materials and other materials with high transmittance to ultraviolet rays. Glass is preferred. Quartz molding cost is high, and resin materials are prone to aging and discoloration.

[0085] In addition, a plurality of inner protrusions 201 and inner grooves 202 are arranged at intervals on the inner side wall of the circumference of the transparent outer cylinder 2, and a plurality of outer protrusions 301 and outer grooves 302 are arranged at intervals on the outer side of the circumference of the transparent inner cylinder 3. The transparent inner cylinder 3 and the open end cover 13 are arranged to rotate and seal with each other. When the inner protrusions 201 and the outer protrusions 301 are in contact with each other, the inner grooves 202 and the outer grooves 302 are correspondingly matched to form an intermittent single annular flow channel 300a. When the transparent inner cylinder 3 is rotated until the inner protrusions 201 and the outer grooves 302 are correspondingly matched, when the outer protrusions 301 and the inner grooves 202 are correspondingly matched, two circles of inner-outer and outer-disconnected double annular flow channels 300b are formed. No matter the single annular flow channel 300a or the double annular flow channel 300b, both are annular flow channels with intervals in cross section.

[0086] Furthermore, the transparent inner cylinder 3 is integrally arranged, and a driven gear 31 is sleeved at the open end of the transparent inner cylinder 3. The driven gear 31 is meshed with a driving gear 33 on a motor 32 installed on the open end cover 13. The motor 32 drives the transparent inner cylinder 3 to rotate through the cooperation between the driven gear 31 and the driving gear 33.

[0087] Specifically, when the motor 32 drives the driving gear 33 to rotate, the rotation of the driving gear 33 causes the driven gear 31 to rotate, thereby driving the transparent inner cylinder 3 to rotate, and the transparent inner cylinder 3 and the open end cover 13 are rotationally matched. At the same time, a sealing baffle is provided at the matching position of the transparent inner cylinder 3 and the open end cover 13 to cooperate with a sealing ring for sealing.

[0088] When the transparent inner tube 3 and the transparent outer tube 2 cooperate to form a single annular flow channel 300a, the cross-sectional height of the single annular flow channel 300a is relatively high. Although the outer light-emitting element 4 and the central light-emitting element 6 can cooperate to irradiate the inner and outer layers of the maleic anhydride grafted crude material in the single annular flow channel 300a with ultraviolet rays, due to the thickness of the fluid, it is difficult for the ultraviolet rays to completely penetrate the fluid, causing the photoinitiator inside the fluid to transition.

[0089] Therefore, by rotating the transparent inner cylinder 3, the single annular flow channel 300a is transformed into a double annular flow channel 300b, and the cross-sectional height is reduced. At the same time, the flow rate of maleic anhydride grafted crude material per unit time remains unchanged (because the flow channel cross-section formed by the combination of the double annular flow channels 300b is exactly the same as the flow channel cross-section of the single annular flow channel 300a). Therefore, within the same irradiation time, the ultraviolet irradiation efficiency formed by the double annular flow channel 300b is much higher than the ultraviolet irradiation efficiency of the single annular flow channel 300a.

[0090] In addition, the transparent inner cylinder 3 can also be arranged in sections, and the transparent inner cylinder 3 includes a head section 311, a middle section 312 and a tail section 313. The head section 311, the middle section 312 and the tail section 313 are connected and assembled with each other. The inner side walls of the head section 311, the middle section 312 and the tail section 313 are respectively provided with driven gear rings 34, and the driven gear rings 34 are correspondingly connected to the transfer gear 36 located outside the transparent inner cylinder 3 through the linkage gear 351 on the rotating shaft 35. A movable and adjustable transmission gear 37 is installed on one side of the transfer gear 36, and a driving gear 38 is arranged on the other side of the transmission gear 37 opposite to the transfer gear 36. The driving gear 38 is arranged in a one-to-one correspondence with the transfer gear 36, and the driving gear 38 is connected to the transfer gear 36 through the transmission gear 37. The driving gear 38 is driven to rotate by a driving motor 39.

[0091] When the transparent inner tube 3 is arranged in sections, the head section 311, the middle section 312 and the tail section 313 are spliced ​​with each other, and the spliced ​​parts are sealed with sealing rings. At the same time, the head section 311, the middle section 312 and the tail section 313 can be rotated independently of each other. Among them, at least one group of the middle section 312 is provided, and the number of the middle sections 312 is related to the length of the transparent inner tube 3. Moreover, each group of the head section 311, the middle section 312 and the tail section 313 is independently provided with a driven gear ring 34, and the position of the driven gear ring 34 is matched with a transfer gear 36, and the transfer gear 36 The linkage gears 351 on the rotating shaft 35 are respectively connected to the transfer gears 36 one by one, wherein the rotating shafts 35 at each driven gear ring 34 are sleeved with each other, and the outermost rotating shaft 35 is suspended below the central light-emitting element 6 through a connecting piece (not shown in the figure), and the transmission gear 37 is moved by the cylinder. When the transmission gear 37 and the corresponding driving gear 38 and the transfer gear 36 cooperate with each other, the corresponding driven gear ring 34 can be driven to rotate by mutual cooperation, and then the corresponding head section 311 or middle section 312 or tail section 313 can be driven to rotate.

[0092] When the segmented transparent inner cylinder 3 switches from the single annular flow channel 300a to the double annular flow channel 300b, it starts with the rotation of the head section 311, then the middle section 312, and finally the tail section 313. The difference between the segmented transparent cylinder 3 and the integrated transparent cylinder 3 is that, instead of directly switching the single annular flow channel 300a to the double annular flow channel 300b, the cross-section of the single annular flow channel 300a is gradually reduced from the head section 311 to the tail section 313, thereby forming a variety of structural forms of the single annular flow channel 300a in combination, and thus forming a variety of working states with different irradiation efficiencies, and then preparing maleic anhydride grafted polymers with different grafting rates, forming maleic anhydride grafted polymers with a grafting rate of 12.5-17%.

[0093] Embodiment 1:

[0094] a1) Add 30 parts of methyl methacrylate monomer, 10 parts of functional acrylate monomer, 10 parts of polypropylene grafted maleic anhydride with a grafting rate of 12.5% ​​in component A, 2.25 parts of compatibilizer, 1 part of leveling agent and 1 part of dispersant into a high-speed stirring kettle according to the proportion, stir at a speed of 1500 rpm for 15 minutes, heat to 65°C, stir for 10 minutes, heat to 80°C, stir at a speed of 1500 rpm and stir for 30 minutes;

[0095] a2) Add 10 parts of pigment, 0.75 parts of remaining compatibilizer and 1 part of dispersant into a high-speed stirring kettle according to the proportion, cool to 65°C, stir at 3000 rpm, stir for 20 minutes and then let stand for 50 minutes;

[0096] a3) Add 0.5 parts of antioxidant and 0.5 parts of accelerator into a high-speed stirring kettle according to the proportion, stir at a speed of 1500 rpm, stir for 15 minutes, cool to below 35°C, and obtain component A of the colored environmentally friendly paving coating;

[0097] The preparation process of component B is:

[0098] b1) Add 30 parts of methyl methacrylate monomer, 10 parts of functional acrylate monomer, 1 part of leveling agent and 0.5 parts of dispersant in component B into a high-speed stirring kettle at a stirring speed of 3000 rpm for 15 minutes, heat to 65°C and stir for 10 minutes;

[0099] b2) Add 5 parts of curing agent into the high-speed stirring kettle according to the proportion, stir at a speed of 3000 rpm, and stir for 15 minutes;

[0100] b3) Add 0.5 parts of antioxidant into the high-speed stirring kettle according to the proportion, stir at a speed of 1500 rpm, stir for 15 minutes, cool to below 35°C, and obtain component B of the colorful environmentally friendly paving coating.

[0101] Embodiment 2:

[0102] Same as Example 1, except that the maleic anhydride grafted polymer is polyethylene grafted maleic anhydride.

[0103] Embodiment 3:

[0104] Same as Example 1, except that the maleic anhydride grafted polymer is polystyrene grafted with maleic anhydride.

[0105] Embodiment 4:

[0106] a1) Add 45 parts of methyl methacrylate monomer, 20 parts of functional acrylate monomer, 15 parts of maleic anhydride graft polymer with a grafting rate of 13.5%, 4 parts of compatibilizer, 1.5 parts of leveling agent and 1.5 parts of dispersant in component A into a high-speed stirring kettle according to the proportion, stir at a speed of 1500 rpm for 20 minutes, heat to 67°C, stir for 12 minutes, heat to 90°C, stir at a speed of 1500 rpm and stir for 45 minutes;

[0107] a2) Add 15 parts of pigment, 1.5 parts of remaining compatibilizer and 1.5 parts of dispersant into a high-speed stirring kettle according to the proportion, cool to 67°C, stir at 3000 rpm, stir for 25 minutes and then let stand for 55 minutes;

[0108] a3) Add 1.25 parts of antioxidant and 1 part of accelerator into a high-speed stirring kettle according to the ratio, stir at a speed of 1500 rpm, stir for 17 minutes, cool to below 35°C, and obtain component A of the colored environmentally friendly paving coating;

[0109] The preparation process of component B is:

[0110] b1) Add 45 parts of methyl methacrylate monomer, 20 parts of functional acrylate monomer, 1.5 parts of leveling agent and 0.75 parts of dispersant in component B into a high-speed stirring kettle at a stirring speed of 3000 rpm for 20 minutes, heat to 67°C and stir for 13 minutes;

[0111] b2) Add 10 parts of curing agent into the high-speed stirring kettle according to the proportion, stir at a speed of 3000 rpm, and stir for 20 minutes;

[0112] b3) Add 1.5 parts of antioxidant into the high-speed stirring kettle according to the proportion, stir at a speed of 1500 rpm, stir for 17 minutes, cool to below 35°C, and obtain component B of the colorful environmentally friendly paving coating.

[0113] Embodiment 5:

[0114] Same as Example 4, except that the maleic anhydride grafted polymer is polyethylene grafted maleic anhydride.

[0115] Embodiment 6:

[0116] Same as Example 4, except that the maleic anhydride grafted polymer is polystyrene grafted maleic acid.

[0117] Embodiment 7:

[0118] a1) Add 60 parts of methyl methacrylate monomer, 30 parts of functional acrylate monomer, 20 parts of maleic anhydride graft polymer with a grafting rate of 14.5%, 6 parts of compatibilizer, 2 parts of leveling agent and 2 parts of dispersant in component A into a high-speed stirring kettle according to the proportion, stir at a speed of 1500 rpm for 25 minutes, heat to 70°C, stir for 15 minutes, heat to 100°C, stir at a speed of 1500 rpm and stir for 60 minutes;

[0119] a2) Add 20 parts of pigment, 2 parts of remaining compatibilizer and 2 parts of dispersant into a high-speed stirring kettle according to the proportion, cool to 70°C, stir at 3000 rpm, stir for 30 minutes and then let stand for 60 minutes;

[0120] a3) Add 2 parts of antioxidant and 1.5 parts of accelerator into a high-speed stirring kettle according to the ratio, stir at a speed of 1500 rpm, stir for 20 minutes, cool to below 35°C, and obtain component A of the colored environmentally friendly paving coating;

[0121] The preparation process of component B is:

[0122] b1) Add 60 parts of methyl methacrylate monomer, 30 parts of functional acrylate monomer, 2 parts of leveling agent and 1 part of dispersant in component B into a high-speed stirring kettle at a stirring speed of 3000 rpm for 25 minutes, heat to 70°C and stir for 10-15 minutes;

[0123] b2) Add 15 parts of curing agent into the high-speed stirring kettle according to the proportion, stir at a speed of 3000 rpm, and stir for 25 minutes;

[0124] b3) Add 2 parts of antioxidant into the high-speed stirring kettle according to the proportion, stir at a speed of 1500 rpm, stir for 20 minutes, cool to below 35°C, and obtain component B of the colorful environmentally friendly paving coating.

[0125] Embodiment 8:

[0126] Same as Example 7, except that the maleic anhydride grafted polymer is polyethylene grafted with maleic anhydride.

[0127] Embodiment 9:

[0128] Same as Example 7, except that the maleic anhydride grafted polymer is polystyrene grafted maleic acid.

[0129] Embodiment 10:

[0130] Same as Example 7, except that the amount of maleic anhydride grafted polymer is 10 parts.

[0131] Comparative Example 1:

[0132] The MMA polymer slow-release anti-coagulation ice color anti-slip paving material in the Chinese patent with patent number 202211676175.5 recorded in the background technology.

[0133] Comparative Example 2:

[0134] The comparative example is the same as Example 1, except that the grafting rate of maleic anhydride grafted onto polypropylene is 12.4%.

[0135] Comparative Example 3:

[0136] The comparative example is the same as Example 2, except that the grafting rate of polyethylene grafted with maleic anhydride is 15%.

[0137] Comparative Example 4:

[0138] The comparative example is the same as Example 3, except that the number of parts of polypropylene grafted with maleic anhydride is 21 parts.

[0139] Comparative Example 5:

[0140] The comparative example is the same as Example 7, except that the number of parts of polypropylene grafted with maleic anhydride is 9 parts.

[0141] Comparative Example 6:

[0142] The comparative example is the same as Example 8, except that the grafting rate of polyethylene grafted with maleic anhydride is 12.4%.

[0143] Comparative Example 7:

[0144] The comparative example is the same as Example 9, except that the grafting rate of polystyrene grafted with maleic anhydride is 15%.

[0145] Since there is no record of the compatibility of anti-skid road coatings in the standard of "Anti-skid Road Coatings" (JT / T712-2008), the compatibility test method of the colored environmentally friendly paving coating and ceramic particles in this application is as follows:

[0146] A suitable road surface is selected to apply the coatings in Examples 1-9 and Comparative Examples 1-7 to form a colored protective road surface, wherein during the construction process, the coating thickness is 4 mm, and the particle size of the selected ceramic particles is 2.5 mm. After rapid curing for 40 minutes and 2 hours, 10 blocks of 100X100 cm colored protective road surfaces are respectively cut off, and one side of the cross section on each colored protective road surface is arbitrarily selected, and the number of ceramic particles immersed in the coating is counted and the average value is taken. At the same time, a friction peeling test of ceramic particles is performed on the cut colored protective road surface. The test time is 1 hour. The viscosity of the coating is tested by counting the number of peeled ceramic particles and taking the average value. When performing the peeling test, a friction simulation peeling test of walking is performed on the colored protective road surface blocks that have been cured for 40 minutes, and a friction simulation peeling test of driving is performed on the colored protective road surface blocks that have been cured for 2 hours. The specific test results are shown in Table 1 below.

[0147]

[0148] Table 1

[0149] It can be seen from Table 1 that through the group comparison of Examples 1, 4, 7; 2, 5, 8; 3, 6, 9, it can be seen that the compatibility of the colored environmentally friendly paving coating and the ceramic particles does not continue to increase with the increase of the grafting rate and the increase of the amount of grafted polymer used. When the grafting rate and the amount of grafted polymer used exceed a certain range, the compatibility of the colored environmentally friendly paving coating and the ceramic particles will decrease. In addition, by comparing Example 10 with Examples 7-9, it can be seen that when the grafting rate is too high, or the amount of maleic anhydride grafted polymer used is high enough, the compatibility of the colored environmentally friendly paving coating and the ceramic particles will decrease.

[0150] At the same time, through the comparison of the three groups, it can be seen that when the dosage of maleic anhydride grafted polymer is 15 parts and the grafting rate is 13.5%, the compatibility and viscosity of the colored environmentally friendly paving coating with ceramic particles are optimal.

[0151] By comparing Example 1 with Comparative Examples 2-4 and Example 7 with Comparative Examples 5-7, it can be seen that when the grafting rate of the maleic anhydride grafted polymer is too high, or the usage is too high, the degree of entanglement of the molecular chains will increase, hindering the diffusion and contact of the coating molecules and the curing agent molecules, thereby affecting the compatibility and viscosity of the colored environmentally friendly paving coating with the ceramic particles, and even affecting the curing time. When the grafting rate of the maleic anhydride grafted polymer is too low, or the usage is too low, the side group content is too low, and the maleic anhydride grafted polymer does not sufficiently improve the compatibility of the colored environmentally friendly paving coating with the ceramic particles. However, by comparing Comparative Example 1 with Comparative Examples 2-7, it can be seen that the use of maleic anhydride grafted polymer still has a certain promoting effect on the compatibility of the colored environmentally friendly paving coating with ceramic particles.

[0152] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A colorful environmentally friendly paving paint, characterized in that: include: Component A and component B, the ratio of component A to component B is 1:1; In parts by weight, the component A includes 30-60 parts of methyl methacrylate monomer, 10-30 parts of functional acrylate monomer, 10-20 parts of pigment, 1-2 parts of leveling agent, 10-20 parts of maleic anhydride grafted polymer with a grafting rate of 12.5-14.5%, 0.5-2 parts of antioxidant, 2-4 parts of dispersant, 3-8 parts of compatibilizer, and 0.5-1.5 parts of accelerator; The B component includes 30-60 parts of methyl methacrylate monomer, 10-30 parts of functional acrylate monomer, 5-15 parts of curing agent, 1-2 parts of leveling agent, 0.5-1 parts of dispersant, and 0.5-2 parts of antioxidant; The functional acrylate monomer is one or more of isotridecyl acrylate, 1,4-cyclohexanedimethanol diacrylate, ethoxyethoxyethyl acrylate, 1,6-hexanediol dimethacrylate, and 2-propoxylated neopentyl glycol diacrylate; The maleic anhydride grafted polymer is one or more of polypropylene grafted maleic anhydride, polyethylene grafted maleic anhydride and polystyrene grafted maleic anhydride.

2. The colorful environmentally friendly paving paint according to claim 1, characterized in that: The antioxidant is one or more of antioxidant 1010 , antioxidant 168 , and antioxidant 1076 .

3. The colorful environmentally friendly paving paint according to claim 1, characterized in that: In component A, the dispersant is a mixture of one or more of polyvinyl alcohol, cellulose, and polyvinyl pyrrolidone and one or more of ethylene bisstearamide and zinc stearate; In component B, the dispersant is one or more of polyvinyl alcohol, cellulose and polyvinyl pyrrolidone.

4. The colorful environmentally friendly paving paint according to claim 1, characterized in that: The compatibilizer is one or more of styrene-maleic anhydride copolymer and methyl methacrylate-butadiene-styrene copolymer.

5. The colorful environmentally friendly paving paint according to claim 1 is characterized by: The curing agent is one or more of dibenzoyl peroxide, dicumyl peroxide, tert-butyl peroxide, cyclohexanone peroxide, and methyl ethyl ketone peroxide.

6. The colorful environmentally friendly paving paint according to claim 1, characterized in that: The accelerator is one or more of N,N-dimethyl-p-methylaniline, cobalt isooctanoate, cobalt naphthenate, and cobalt cyclohexaneate.

7. A process for preparing the colorful environmentally friendly paving coating according to any one of claims 1 to 6, characterized in that: The preparation process of component A is: a1. Add methyl methacrylate monomer, functional acrylate monomer, maleic anhydride grafted polymer, 3 / 4 of compatibilizer, leveling agent and 1 / 2 of dispersant in component A into a high-speed stirring kettle according to the proportion, stir at a speed of 1500 rpm for 15-25 min, heat to 65-70°C, stir for 10-15 min, heat to 80-100°C, stir at a speed of 1500 rpm, and stir for 30-60 min; a2. Add pigment, remaining compatibilizer and dispersant into a high-speed stirring kettle according to the proportion, cool to 65-70°C, stir at 3000rpm, stir for 20-30min and let stand for 50-60min; a3. Add antioxidant and accelerator into the high-speed stirring kettle according to the proportion, stir at a speed of 1500 rpm, stir for 15-20 minutes, cool to below 35°C, and obtain component A of the colored environmentally friendly paving coating; The preparation process of component B is: b1. Add methyl methacrylate monomer, functional acrylate monomer, leveling agent and dispersant in component B into a high-speed stirring kettle according to the proportion, stir at a speed of 3000 rpm, stir for 15-25 minutes, heat to 65-70°C, and stir for 10-15 minutes; b2. Add the curing agent into the high-speed stirring kettle according to the proportion, stirring at a speed of 3000rpm for 15-25min; b3. Add the antioxidant into the high-speed stirring kettle according to the proportion, the stirring speed is 1500rpm, stir for 15-20min, cool to below 35℃, and obtain component B of the colorful environmentally friendly paving coating.

8. The process for preparing a colored environmentally friendly paving coating according to claim 7 is characterized in that: When preparing the maleic anhydride grafted polymer used in step a1, the polymer, the interfacial agent, the initiator, the antioxidant and the maleic anhydride are melt-blended and extruded to form a grafted crude material, and the grafted crude material is circulated in an ultraviolet irradiation device and irradiated by ultraviolet rays for 50-80 minutes, and the grafting rate of the grafted crude material after ultraviolet irradiation is increased as the cross-sectional thickness of the grafted crude material flowing in the ultraviolet irradiation device decreases, and a maleic anhydride grafted polymer with a grafting rate of 12.5-14.5% is prepared; The ultraviolet irradiation device comprises an outer shell (1), a transparent outer cylinder (2), a transparent inner cylinder (3), an outer light-emitting element (4), an end light-emitting element (5) and a central light-emitting element (6); The housing (1) comprises a cylindrical body (11), a sealing end cover (12) and an open end cover (13); the cylindrical body (11) is provided with openings at both ends; the sealing end cover (12) and the open end cover (13) are respectively provided at the openings at both ends of the cylindrical body (11); the sealing end cover (12), the open end cover (13) and the cylindrical body (11) are connected by threaded fasteners; The two ends of the transparent outer cylinder (2) are open, and the middle protrusion of the transparent outer cylinder (2) is provided with two sets of parallel ring parts (21), the ring parts (21) are in sealing contact with the inner wall of the cylindrical body (11), and a feed area (100) and a discharge area (200) separated from each other are formed between the cylindrical body (11) and the transparent outer cylinder (2), the feed area (100) is connected to the feed nozzle (111) on the cylindrical body (11), and the discharge area (200) is connected to the discharge nozzle (112) on the cylindrical body (11); The transparent inner cylinder (3) is coaxially inserted into the interior of the transparent outer cylinder (2), and an annular flow channel (300) is formed between the transparent inner cylinder (3) and the transparent outer cylinder (2), and the feed area (100) and the discharge area (200) are connected via the annular flow channel (300); A plurality of inner protrusions (201) and inner grooves (202) are arranged at intervals on the inner circumferential wall of the transparent outer cylinder (2); a plurality of outer protrusions (301) and outer grooves (302) are arranged at intervals on the outer circumferential wall of the transparent inner cylinder (3); when the inner protrusions (201) and the outer protrusions (301) are in contact with each other, the inner grooves (202) and the outer grooves (302) are correspondingly matched to form an intermittent single annular flow channel (300a); when the transparent inner cylinder (3) is rotated until the inner protrusions (201) and the outer grooves (302) are correspondingly matched, when the outer protrusions (301) and the inner grooves (202) are correspondingly matched, two circles of inner-outer and outer-outer arranged and intermittently arranged double annular flow channels (300b) are formed; The external light-emitting elements (4) are arranged in a circular array around the side wall of the transparent outer cylinder (2), and the inner layer of the grafted coarse material flowing in the feeding area (100) and the discharging area (200) is irradiated with ultraviolet light, and the external light-emitting elements (4) simultaneously irradiate the outer layer of the grafted coarse material flowing in the annular flow channel (300) with ultraviolet light; The end light emitting element (5) is arranged at the feeding area (100), and the end light emitting element (5) is separated from the feeding area (100) by a transparent spherical cover (51); an arc-shaped transparent cover (22) with a central opening is installed on the end of the transparent outer cylinder (2) corresponding to the transparent spherical cover (51); a spherical channel (511) is formed between the arc-shaped transparent cover (22) and the transparent spherical cover (51); the spherical channel (511) connects the feeding area (100) and the annular flow channel (300) through a connecting port (221) on the arc-shaped transparent cover (22); the end light emitting element (5) irradiates the outer layer of the grafted coarse material flowing in the spherical channel (511) with ultraviolet rays; The central light-emitting element (6) is inserted into the transparent inner cylinder (3), and the central light-emitting element (6) irradiates the inner layer of the grafted coarse material flowing in the annular flow channel (300) with ultraviolet rays.

Citation Information

Patent Citations

  • MMA (methyl methacrylate) polymer slow-release anti-freezing colored antiskid paving material as well as preparation method and construction method thereof

    CN115926567A

  • Anti-skid unsaturated MMA resin composition containing synthetic MMA resin, manufacturing method, and road surface construction method using the same

    KR102456746B1

  • Construction method for anti-slip pavement materials for road

    KR102629941B1