A method for preparing a high specific capacity lithium ion battery electrode material
By combining the single layer MXene with cobalt salt and iron-containing organic ligand and vulcanized, an electrode material with a porous structure was prepared, which solved the problem of reduced porosity and structural collapse of the lithium-ion battery electrode material during charging and discharging. , improves the cycle stability and specific capacity of the battery.
Patent Information
- Application Number
- CN202411067717.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-06
AI Technical Summary
Existing lithium-ion battery electrode materials are prone to problems such as decreased porosity, structural collapse and volume expansion during charging and discharging, resulting in poor specific capacity and cycle stability.
A single layer of MXene is used to combine with cobalt salt and iron-containing organic ligand, and CFM is formed by sonication and solvothermal reaction, followed by vulcanization treatment to prepare an electrode material with a porous structure and a high specific surface area, combining the high conductivity of MXene and MOF's rugged construction.
It improves the discharge performance and cycle stability of lithium-ion batteries, enhances the conductivity and specific capacity, solves the problems of low conductivity and structural collapse of MOF materials, and suppresses the accumulation of MXene sheets.
Smart Images

Figure CN118588932B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of electrochemical technology, and in particular to a method for preparing an electrode material for a lithium-ion battery with high specific capacity. Background Art
[0002] Lithium-ion batteries have the advantages of long life, high energy density, and high discharge potential, and have developed from traditional small portable devices to the power source of automobiles. However, traditional graphite electrodes have gradually failed to meet the requirements, so the development of new electrode materials with higher energy density, higher safety and improved cycle performance has become an important research field.
[0003] In order to improve this problem, currently commonly used electrode materials include carbon materials, metal organic frameworks, silicon-based materials, etc., among which carbon materials mainly include carbon nanotubes, graphene, etc.
[0004] However, the above solutions also have problems with the materials themselves. Although graphene has high porosity and high conductivity, the stacking problem of the two-dimensional material itself seriously limits its development. Carbon nanotubes and carbon nanofibers tend to agglomerate during the charging and discharging process, which leads to a decrease in porosity and a decrease in specific capacity. A single metal organic framework has a high porosity and rich functional groups, but low conductivity and structural collapse will cause the battery capacity to drop sharply. Although silicon-based materials have a high specific capacity and good cycle stability, they will undergo huge volume expansion, leading to damage and short circuits inside the battery. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a high specific capacity lithium ion battery electrode material to solve the problems existing in the above-mentioned prior art.
[0006] To achieve the above object, the present invention provides the following solutions:
[0007] One of the technical solutions of the present invention is to provide a method for preparing an electrode material for a high specific capacity lithium-ion battery, the steps comprising:
[0008] Dissolving a monolayer of MXene and a cobalt salt in water to obtain a Co-MXene solution;
[0009] dissolving an iron-containing organic ligand in an organic solvent to prepare an iron source solution;
[0010] The iron source solution and the Co-MXene solution are uniformly mixed and ultrasonically treated, and after a solvothermal reaction, a precipitated product is separated to obtain CFM;
[0011] The electrode material is obtained by sulfurizing CFM.
[0012] Furthermore, the single-layer MXene is a single-layer Ti3C2T x 、Ti3N2T x 、V3N2T x or Nb3N2T x .
[0013] Furthermore, the cobalt salt is Co(NO3)2·6H2O, CoCl2 or CoSO4.
[0014] Furthermore, the iron-containing organic ligand is 1,1'-dicarboxyferrocene.
[0015] Furthermore, the organic solvent is N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO) or dichloromethane (DCM).
[0016] Furthermore, the mass ratio of the monolayer MXene, the cobalt salt and the water is 0.1-0.2:0.2-0.4:20-25, preferably 0.1-0.2:0.22-0.33:20-25.
[0017] Furthermore, the usage ratio of the iron-containing organic ligand to the organic solvent is 0.2~0.4 g:30~35 mL, preferably 0.214~0.34 g:30~35 mL.
[0018] Furthermore, the ultrasonic treatment time is 1 to 2 hours.
[0019] Ultrasonic treatment can make the metal cations in the solution fully adsorbed on the negatively charged monolayer MXene surface.
[0020] Furthermore, the solvent thermal reaction is carried out at 120-180° C. for 9-15 hours.
[0021] Furthermore, the sulfurization treatment uses CFM and sulfur as raw materials, uses an inert gas as a carrier gas, and reacts at 600-650° C. for 2-3 hours.
[0022] Preferably, the mass ratio of CFM to sulfur is not higher than 1:10.
[0023] Preferably, the inert gas comprises argon.
[0024] In the sulfurization treatment, sulfur powder is placed upstream and CFM is placed downstream, and the sublimated sulfur is transported downstream by carrier gas to react with CFM.
[0025] The second technical solution of the present invention is to provide an electrode material for a high specific capacity lithium-ion battery prepared by the above preparation method.
[0026] The third technical solution of the present invention is to provide an application of the above-mentioned electrode material for high specific capacity lithium-ion batteries in battery preparation.
[0027] The fourth technical solution of the present invention is to provide a lithium-ion battery electrode, the raw materials of which include the above-mentioned electrode material for high specific capacity lithium-ion batteries.
[0028] Furthermore, the lithium-ion battery electrode raw materials also include: carbon black, polyvinylidene fluoride (PVDF) and copper foil.
[0029] The fifth technical solution of the present invention: provides a lithium-ion battery, comprising the above-mentioned lithium-ion battery electrode.
[0030] Furthermore, the lithium-ion battery also includes: a lithium secondary battery electrolyte, a lithium sheet and a separator.
[0031] The present invention discloses the following technical effects:
[0032] The present invention improves the discharge performance of lithium-ion batteries by combining porous MOF materials with MXene materials. The MOF material itself has a large specific surface area and a high porosity. The large specific surface area enables the electrode material to fully contact the electrolyte, while the high porosity can accelerate the transmission of lithium ions. Its solid 3D structure not only does not change its porosity but also effectively reduces the volume expansion of lithium ions. The introduction of two-dimensional MXene sheets can not only solve the problem of low conductivity of MOF materials but also inhibit the structural collapse of Fe-based MOF during the charge and discharge process. In addition, this 2D-3D inhibition structure also solves the stacking problem of two-dimensional MXene sheets. The subsequent sulfurization can prevent the structural collapse of MOF materials during the charge and discharge process, enhance its cycle stability, and improve the conductivity and specific capacity of the material.
[0033] According to the negatively charged property of the monolayer MXene itself, the present invention adsorbs cobalt on its surface, and then anchors the bimetallic organic framework on the monolayer MXene sheet by a solvothermal method using two carboxyl groups in 1,1'-dicarboxyferrocene as bridges, and then enhances the structural stability and the specific capacity of the battery by sulfurization. This solves the problems of structural collapse of MOF materials during circulation and accumulation of MXene sheets, and enhances the conductivity and cycle stability of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0035] Figure 1 Ti3C2T x Microscopic morphology of
[0036] Figure 2 The SEM images of CF and the TEM images of CFM, where a is the SEM image of CF and b is the TEM image of CFM;
[0037] Figure 3 The microscopic morphology of CFM@S, where a is the SEM image of CFM@S and b is the TEM image of CFM@S;
[0038] Figure 4 XRD of CFM, Co(NO3)2·6H2O and 1,1'-dicarboxyferrocene, and Ti3C2T x Standard card;
[0039] Figure 5 It is the XRD of CFM@S and the standard card of FeS2 and CoS2;
[0040] Figure 6 For CFM, CF and Ti3C2T x The cyclic specific capacity of the material at a current density of 0.5A / g;
[0041] Figure 7 is the cyclic specific capacity of CFM and CFM@S at a current density of 0.5 A / g;
[0042] Figure 8 is the cyclic specific capacity of CFM and CFM@S at a current density of 2A / g;
[0043] Fig. 9 The rate performance of CFM and CFM@S;
[0044] Fig.10 For AC impedance test of CFM and CFM@S;
[0045] Fig.11 are the first three charge-discharge curves of CFM and CFM@S, where a is the first three charge-discharge curves of CFM, and b is the first three charge-discharge curves of CFM@S. DETAILED DESCRIPTION
[0046] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0047] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0048] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0049] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0050] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0051] In a specific embodiment of the present invention, a single layer Ti3C2T x As an example, a single-layer MXene material has a microscopic morphology as shown in Figure 1 As shown, the preparation steps are:
[0052] At 35 ° C, 3.2 g LiF (AR) was added to 40 mL HCl (9 M, AR) and stirred for 10 min to fully dissolve it. Then, 2 g Ti3AlC2 (200 mesh, AR) was slowly added and stirred at a constant temperature of 400 rpm for 24 h for etching. After the etching was completed, the obtained mixture was centrifuged at 5000 rpm for 1 min. After the supernatant was poured out, deionized water was added and the above steps were repeated until the supernatant was black (at this time, the supernatant had an obvious Tyndall effect). Then, the solution was shaken and placed in an ultrasonic cleaner for ice water ultrasound for 1 h. After the ultrasound was completed, it was centrifuged at 3500 rpm for 10-15 min. After the centrifugation was completed, the obtained black supernatant was freeze-dried to obtain a single layer of Ti3C2T x .
[0053] Example 1
[0054] The preparation steps for high specific capacity lithium ion battery electrode materials are as follows:
[0055] S1. Weigh 0.1 g of Ti3C2T prepared above. x and 0.33 g Co(NO3)2·6H2O were dissolved in 20 mL of deionized water to obtain Co-MXene solution;
[0056] S2, weigh 0.34 g of 1,1'-dicarboxyferrocene and dissolve it in 30 mL of DMF to obtain an iron source solution;
[0057] S3, the Co-MXene solution and the iron source solution were mixed and ultrasonicated for 1 hour, and then the mixed solution was placed in a high-pressure reactor to react at 150°C for 12 hours, and then centrifuged at 5000 rpm for 5 minutes to separate the precipitated product, and vacuum dried at 60°C for 8 hours to obtain CFM;
[0058] S4. Weigh 0.1 g of CFM and 2 g of sulfur powder, put them into two crucibles respectively, put the sulfur powder upstream of the tube furnace and the CFM downstream of the tube furnace, pass argon for 10 minutes to ensure that the entire tube is filled with argon, and then increase the temperature to 600°C at a heating rate of 5°C / min without stopping the ventilation. After reacting for 2 hours, cool to room temperature to obtain the electrode material product, recorded as CFM@S.
[0059] Example 2
[0060] The preparation steps of lithium-ion battery electrodes are:
[0061] The CFM@S, carbon black and PVDF prepared in Example 1 were mixed and ground in a mass ratio of 8:1:1. After grinding, N,N-methylpyrrolidone (NMP) was slowly added dropwise, stirred into a paste, and then evenly coated on a copper foil with a coater, followed by vacuum drying at 80°C for 6 hours to obtain a lithium-ion battery electrode.
[0062] Example 3
[0063] The preparation steps of lithium-ion battery (CR2025) are:
[0064] The lithium ion battery electrode prepared in Example 2 was used as the positive electrode (14×14 mm) and placed in a CR2025 battery shell, and then a PP separator (18×18 mm) was placed, and 30 μL of lithium secondary battery electrolyte (LB-002) was slowly dripped. After the electrode was completely soaked, a lithium sheet (14×14 mm) and nickel foam (18×18 mm) and a CR2025 battery shell cover were placed in sequence, and then a tablet press was used to press the tablet at a pressure of 50 MPa for 5 s to obtain a CR2025 lithium ion battery.
[0065] Comparative Example 1
[0066] Compared with Example 1, the only difference is that no Ti3C2T x , the specific steps are as follows:
[0067] S1. Weigh 0.33 g Co(NO3)2·6H2O and dissolve it in 20 mL deionized water to obtain a Co solution.
[0068] S2, weigh 0.34 g of 1,1'-dicarboxyferrocene and dissolve it in 30 mL of DMF to obtain an iron source solution;
[0069] S3, the Co solution and the iron source solution were mixed and ultrasonicated for 1 hour, and then the mixed solution was placed in a high-pressure reactor and reacted at 150°C for 12 hours, and then centrifuged at 5000 rpm for 5 minutes to separate the precipitated product, and vacuum dried at 60°C for 8 hours to obtain CF;
[0070] S4. Weigh 0.1 g of CF and 2 g of sulfur powder, put them into two crucibles respectively, put the sulfur powder in the upstream of the tube furnace and the CF in the downstream of the tube furnace, pass argon for 10 minutes to ensure that the entire tube is filled with argon, and then increase the temperature to 600°C at a heating rate of 5°C / min without stopping the ventilation. After reacting for 2 hours, cool to room temperature to obtain the electrode material product, which is recorded as CF@S.
[0071] Comparative Example 2
[0072] The preparation steps of lithium-ion battery electrodes are:
[0073] The CF@S, carbon black and PVDF prepared in Comparative Example 1 were mixed and ground in a mass ratio of 8:1:1, and N,N-methylpyrrolidone (NMP) was slowly added dropwise after grinding. After stirring into a paste, it was evenly coated on a copper foil with a coater, and then vacuum dried at 80°C for 6 hours to obtain a lithium-ion battery electrode.
[0074] Comparative Example 3
[0075] The preparation steps of lithium-ion battery (CR2025) are:
[0076] The lithium ion battery electrode prepared in Comparative Example 2 was used as the positive electrode (14×14 mm) and placed in a CR2025 battery shell, and then a PP separator (18×18 mm) was placed, and 30 μL of lithium secondary battery electrolyte (LB-002) was slowly dripped. After the electrode was completely soaked, a lithium sheet (14×14 mm) and nickel foam (18×18 mm) and a CR2025 battery shell cover were placed in turn, and then a tablet press was used to press the tablet at a pressure of 50 MPa for 5 s to obtain a CR2025 lithium ion battery.
[0077] Comparative Example 4
[0078] The preparation steps of lithium-ion battery electrodes are:
[0079] The single layer Ti3C2T x , carbon black and PVDF are mixed evenly in a mass ratio of 8:1:1 and ground. After grinding, N,N-methylpyrrolidone (NMP) is slowly added dropwise. After stirring into a paste, it is evenly coated on a copper foil with a coater, and then vacuum dried at 80°C for 6 hours to obtain a lithium-ion battery electrode.
[0080] Comparative Example 5
[0081] The preparation steps of lithium-ion battery (CR2025) are:
[0082] The lithium ion battery electrode prepared in Comparative Example 4 was used as the positive electrode (14×14 mm) and placed in a CR2025 battery shell, and then a PP separator (18×18 mm) was placed, and 30 μL of lithium secondary battery electrolyte (LB-002) was slowly dripped. After the electrode was completely soaked, a lithium sheet (14×14 mm) and nickel foam (18×18 mm) and a CR2025 battery shell cover were placed in turn, and then a tablet press was used to press the tablet at a pressure of 50 MPa for 5 s to obtain a CR2025 lithium ion battery.
[0083] Comparative Example 6
[0084] The preparation steps of lithium-ion battery electrodes are:
[0085] The CFM, carbon black and PVDF in Example 1 were mixed and ground in a mass ratio of 8:1:1, and N,N-methylpyrrolidone (NMP) was slowly added dropwise after grinding. After stirring into a paste, it was evenly coated on a copper foil with a coater, and then vacuum dried at 80°C for 6 hours to obtain a lithium-ion battery electrode.
[0086] Comparative Example 7
[0087] The lithium ion battery electrode prepared in Comparative Example 6 was used as the positive electrode (14×14 mm) and placed in a CR2025 battery shell, and then a PP separator (18×18 mm) was placed, and 30 µL of lithium secondary battery electrolyte (LB-002) was slowly dripped. After the electrode was completely soaked, a lithium sheet (14×14 mm) and nickel foam (18×18 mm) and a CR2025 battery shell cover were placed in turn, and then a tablet press was used to press the tablet at a pressure of 50 MPa for 5 s to obtain a CR2025 lithium ion battery.
[0088] Test example
[0089] Figure 1 Ti3C2T x The microscopic morphology of Figure 1It can be seen that Ti3C2T x The microscopic morphology under a transmission electron microscope shows a perfect lamellar structure.
[0090] Figure 2 The SEM image of CF and the TEM image of CFM, where a is the SEM image of CF and b is the TEM image of CFM. Figure 2 As can be seen from a, CF presents an obvious flower-like structure composed of nanosheets. Figure 2 In b, we can see that CF grows evenly on the small Ti3C2T x On the film.
[0091] Figure 3 The microscopic morphology of CFM@S, where a is the SEM image of CFM@S and b is the TEM image of CFM@S. Figure 3 It can be seen that Figure 2 The difference between the TEM images of CFM and CFM@S is that point-like substances appear on the nanoflower-like structure, the density of the petals is reduced, and the specific surface area is increased.
[0092] Figure 4 XRD of CFM, Co(NO3)2·6H2O and 1,1'-dicarboxyferrocene, and Ti3C2T x Standard card. Figure 4 It can be seen that the characteristic peaks of CFM raw materials can all be found in CFM, among which the characteristic peaks of Ti3C2Tx shift to low angles. This is because after the MXene sheet is compounded with the MOF material, its interlayer spacing is supported by MOF, which leads to a larger lattice parameter.
[0093] Figure 5 The XRD of CFM@S and the standard card of FeS2 and CoS2 are Figure 5 It can be seen that the XRD of CFM@S is highly consistent with that of FeS2 and CoS2. In addition, compared with FeS2, the peak of CFM@S generally shifts to a small angle, while compared with CoS2, CFM@S shifts to a large angle, indicating that CFM@S is an independent material between the two.
[0094] Figure 6 For CFM, CF and Ti3C2T x The material has a cycling capacity at a current density of 0.5A / g. Figure 6 It can be seen that the relative specific capacity of CF decreases rapidly first and then reaches the highest value at the 160th cycle, and then begins to gradually decrease. x After that, the CFM specific capacity is relatively stable. This is because Ti3C2T x The strong two-dimensional structure of the sheets inhibits the collapse of the CF structure.
[0095] Figure 7 is the cycle specific capacity of CFM and CFM@S at a current density of 0.5 A / g, given by Figure 7 It can be seen that the sulfurized material has maintained a specific capacity higher than CFM throughout 240 cycles. After 240 cycles, its specific capacity is still as high as a relative specific capacity of 1137.4 mAh / g.
[0096] Figure 8 is the cycling specific capacity of CFM and CFM@S at a current density of 2A / g, and Figure 7 In comparison, the specific capacity of CFM decreased significantly, while the relative specific capacity of CFM@S decreased less, and maintained a higher specific capacity than CFM during 400 cycles. After 400 cycles, its specific capacity was still as high as 926 mAh / g.
[0097] Fig. 9 is the rate performance of CFM and CFM@S, Fig. 9 It can be seen that when the current density increases from small to large and then from large to small, the specific capacities of the two materials are relatively well preserved. By comparison, no matter at which current density, CFM@S exhibits a higher specific capacity than CFM.
[0098] Fig.10 For the AC impedance test of CFM and CFM@S, Fig.10 It can be seen that the capacitive arc radius of CFM@S is smaller than that of CFM, indicating that the vulcanized material has a lower internal resistance. At the same time, the linear slope of CFM@ in the high frequency region is significantly smaller than that of CFM, indicating that CFM@S has a higher ion diffusion rate.
[0099] Fig.11 The first three charge-discharge curves of CFM and CFM@S, where a is the first three charge-discharge curves of CFM and b is the first three charge-discharge curves of CFM@S. Fig.11 It can be seen that CFM@S has an obvious charging and discharging platform, while CFM does not. At the same time, the overlap between the second and third charging and discharging curves of CFM@S is significantly higher than that of CFM, indicating that CFM@S has better cycle stability.
[0100] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing an electrode material for a high specific capacity lithium-ion battery, characterized in that the steps include: Dissolving a monolayer of MXene and a cobalt salt in water to obtain a Co-MXene solution; dissolving an iron-containing organic ligand in an organic solvent to prepare an iron source solution; The iron source solution and the Co-MXene solution are uniformly mixed and ultrasonically treated, and after a solvothermal reaction, a precipitated product is separated to obtain CFM; The electrode material is obtained by subjecting CFM to a sulfurization treatment; The sulfurization treatment is to use CFM and sulfur as raw materials, inert gas as carrier gas, and react for 2 to 3 hours at 600 to 650° C., wherein sulfur powder is upstream and CFM is downstream; The monolayer MXene is a monolayer Ti3C2T x 、Ti3N2T x 、V3C2T x or Nb3C2T x ; The cobalt salt is CoCl2 or CoSO4; the iron-containing organic ligand is 1,1'-dicarboxyferrocene; the organic solvent is DMF, DMSO or DCM; The mass ratio of the monolayer MXene, cobalt salt and water is 0.1-0.2:0.2-0.4:20-25; the dosage ratio of the iron-containing organic ligand to the organic solvent is 0.2-0.4 g:30-35 mL; the volume ratio of the Co-MXene solution to the iron source solution is 20-25:30-35; The ultrasonic treatment time is 1-2 hours; the solvent thermal reaction is carried out at 120-180° C. for 9-15 hours; The mass ratio of CFM to sulfur is no higher than 1:10; and the inert gas includes argon.
2. An electrode material for a high specific capacity lithium-ion battery obtained by the preparation method as claimed in claim 1.
3. Use of the electrode material for high specific capacity lithium-ion battery as claimed in claim 2 in battery preparation.
4. A lithium ion battery electrode, characterized in that: The invention comprises the electrode material for a high specific capacity lithium-ion battery as described in claim 2.
5. A lithium ion battery, characterized in that: The lithium-ion battery electrode comprises the lithium-ion battery electrode as claimed in claim 4.
Citation Information
Patent Citations
Carbon-assembled zinc sulfide and cobalt sulfide hollow nano polyhedral framework material as well as preparation and application thereof
CN112366298A
A Fe-Co MOF-derived material and its application in lithium-sulfur batteries
CN114276556B
Cyano group modified Zr-Fe MOF, preparation method thereof and zinc negative electrode material of zinc-based flow battery
CN115172774A
Preparation method of transition metal phosphide / C / MXene composite material
CN116040595A
Preparation of cobalt-cobalt disulfide heterojunction embedded nitrogen-sulfur co-doped carbon nanocage positive electrode material and application of cobalt-cobalt disulfide heterojunction embedded nitrogen-sulfur co-doped carbon nanocage positive electrode material in lithium-sulfur battery
CN116504951A