Calcium hydroxyapatite microspheres and preparation method thereof

By using a specific proportion of hydroxyapatite calcium raw material and a mixture of cordierite and water in spray granulation technology for vacuum granulation, spray drying and sintering, the density and compactness of hydroxyapatite calcium microspheres in the prior art are solved. Due to the problem of low degree and crystallinity, high-quality microspheres suitable for clinical applications were prepared.

CN118637571BActive Publication Date: 2024-11-08HEFEI BREATH MEDICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411134876.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-08
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The hydroxyapatite calcium microspheres produced by existing spray granulation technology have low density, low density and low crystallinity, which are easy to degrade and cannot meet the needs of clinical applications.

Method used

The specific mass ratio of hydroxyapatite calcium raw material and cordierite to water and Ca/P molar ratio were used to prepare hydroxyapatite calcium microspheres by vacuum grinding, spray drying and sintering. During the sintering process, cordierite formed microspheres. The melting zone reduces the diffusion resistance of substances, vacuum grinding removes bubbles to improve slurry uniformity, and spray drying controls temperature and speed to improve density and crystallinity.

Benefits of technology

The prepared hydroxyapatite calcium microspheres have high density, compactness and crystallinity, low degradation rate and good fluidity, and are suitable as medical fill materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118637571B_ABST
    Figure CN118637571B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of inorganic materials, and specifically relates to a calcium hydroxyapatite microsphere and a preparation method thereof. The preparation method comprises the following steps: mixing calcium hydroxyapatite raw material, cordierite and water to obtain a slurry; vacuum grinding, spray drying and sintering the slurry to obtain calcium hydroxyapatite microspheres; during the sintering process, cordierite forms a micro-melting zone between the calcium hydroxyapatite raw materials, promoting the separation of the surface particles of the calcium hydroxyapatite raw materials from the calcium hydroxyapatite raw materials, reducing the material diffusion resistance and improving the fluidity; and vacuum grinding can remove bubbles while grinding, further improving the uniformity of the slurry, so that the microspheres finally obtained have excellent density, compactness and crystallinity, and are not easy to degrade.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of inorganic materials, and in particular relates to calcium hydroxyapatite microspheres and a preparation method thereof. Background Art

[0002] Hydroxyapatite (Ca 10 (OH)2(PO4)6, also known as calcium hydroxyapatite, basic calcium phosphate, calcium apatite) is an important inorganic component in animal bones and teeth. Because of its good biocompatibility and fluidity, it is widely used as a bone filling material in clinical surgeries such as dentistry, orthopedics, and medical aesthetics.

[0003] Microsphere materials have good properties that other irregularly shaped materials do not have, such as good fluidity, high bulk density, light weight, high strength, not easy to agglomerate, good injection performance and not easy to cause stress concentration when filled into composite materials.

[0004] Therefore, considering the advantages of calcium hydroxyapatite microspheres, calcium hydroxyapatite microspheres are a medical material with good application prospects.

[0005] Micron-sized medical calcium hydroxyapatite microspheres are usually used as structural support materials, for example, for the preparation of injectable filling preparations. If the particle size of the calcium hydroxyapatite microspheres is too small, it is easy for the calcium hydroxyapatite microspheres to transfer from the injection site to other sites or be engulfed by immune cells in the human body. If the particle size is too large, there will be problems such as difficulty in degradation of the calcium hydroxyapatite microspheres injected into the human body.

[0006] At present, the synthesis methods of hydroxyapatite calcium microspheres mainly include direct synthesis method and secondary granulation molding method. There are two main types of direct synthesis methods: one is to use calcium salt and phosphate as raw materials, and directly control the synthesis of hydroxyapatite calcium microspheres by adjusting the parameters in the reaction process, but the particle size distribution of the obtained hydroxyapatite calcium microspheres is wide and the morphology is not regular enough. This method is mainly used to synthesize nano-microspheres; the other is a soft template method using flexible organic molecules with large structural variability as templates and a hard template method using substances with rigid structures as templates. Calcium hydroxyapatite microspheres with the required structure and morphology are synthesized and prepared through ion exchange reactions, but the template needs to be removed, and the operation is cumbersome. The secondary molding method includes plasma melting method and spray drying method. Among them, the plasma melting method has a high operating temperature, and it is difficult to use this method for materials that are easily decomposed at high temperature. The spray drying method can significantly improve the yield and particle size uniformity of hydroxyapatite calcium microspheres, and is easy to mass produce.

[0007] However, the calcium hydroxyapatite microspheres produced by the existing spray granulation technology have low density, low compactness, and low crystallinity. They are easily degraded after being implanted in the human body and cannot meet actual needs. Summary of the invention

[0008] Therefore, the present invention aims to overcome the defects of low density, low compactness, low crystallinity and easy degradation of calcium hydroxyapatite microspheres prepared by existing spray granulation technology, thereby providing calcium hydroxyapatite microspheres and a preparation method thereof.

[0009] The first aspect of the present invention protects a method for preparing calcium hydroxyapatite microspheres, which comprises the following steps:

[0010] Calcium hydroxyapatite raw material, cordierite and water are mixed to obtain slurry; the slurry is vacuum ground, spray dried and sintered to obtain calcium hydroxyapatite microspheres.

[0011] According to the present invention, the mass ratio of the calcium hydroxyapatite raw material to cordierite is 100:0.001-0.005.

[0012] According to the present invention, the mass ratio of the calcium hydroxyapatite raw material to water is (45-60):(40-55).

[0013] According to the present invention, the mass ratio of the calcium hydroxyapatite raw material to water is (50-55):(45-50).

[0014] According to the present invention, the Ca / P molar ratio in the calcium hydroxyapatite raw material is 1.65-1.68:1.

[0015] According to the present invention, the Ca / P molar ratio in the calcium hydroxyapatite raw material is 1.66-1.67:1.

[0016] In the present invention, ICP (inductively coupled plasma spectroscopy) is used to test the Ca / P molar ratio in the calcium hydroxyapatite raw material.

[0017] According to the present invention, the mass ratio of the calcium hydroxyapatite raw material to water is 20-100 nm.

[0018] According to the present invention, the mass ratio of the calcium hydroxyapatite raw material to water is 40-80nm.

[0019] According to the present invention, the average particle size of the cordierite is 5-10 nm.

[0020] According to the present invention, the mixing temperature is 20-40° C., and the mixing time is 30-60 min.

[0021] According to the present invention, the grinding speed of the vacuum grinding is 50-100 rpm, the vacuum degree of the vacuum grinding is 10-100 Pa, and the vacuum grinding time is 1-2 h.

[0022] In the present invention, the temperature of the vacuum grinding is room temperature (25° C.).

[0023] According to the present invention, the inlet temperature of the spray drying is 150-200°C, and the outlet temperature is 80-100°C.

[0024] In the present invention, the rotation speed of the atomizing disk in the spray drying is 10000-12000 rpm, and the slurry flow rate is 2-5 kg / h.

[0025] According to the present invention, the sintering temperature is 1200-1550° C., and the sintering time is 2-4 hours.

[0026] In the present invention, the sintering is carried out in a high-temperature kiln, wherein the high-temperature kiln includes any one of a muffle furnace, a bell kiln, a tunnel kiln, and a roller kiln.

[0027] The second aspect of the present invention protects calcium hydroxyapatite microspheres prepared by the above-mentioned preparation method.

[0028] According to the present invention, the density of the calcium hydroxyapatite microspheres is 3.00-3.20 g / cm 3 The density is 90-100%, the crystallinity is 90-100%, and the degradation rate is 0.1-0.6%.

[0029] The technical solution of the present invention has the following advantages:

[0030] 1. A method for preparing calcium hydroxyapatite microspheres provided by the present invention comprises the following steps: mixing calcium hydroxyapatite raw material, cordierite and water to obtain a slurry; vacuum grinding, spray drying and sintering the slurry to obtain calcium hydroxyapatite microspheres; during the sintering process, cordierite forms a micro-melting zone between the calcium hydroxyapatite raw materials, promoting the separation of particles on the surface of the calcium hydroxyapatite raw materials from the calcium hydroxyapatite raw materials, reducing the material diffusion resistance and improving the fluidity; and vacuum grinding can remove bubbles in the slurry while grinding, further improving the uniformity of the slurry, so that the finally obtained microspheres have excellent density, compactness and crystallinity, and are not easy to degrade.

[0031] 2. The specific mass ratio of calcium hydroxyapatite raw material to water in the present invention can further reduce the proportion of spheres initially formed in the slurry due to drying shrinkage, avoiding deformation of the spheres caused by large shrinkage; at the same time, it can reduce the damage of the spheres caused by the rapid volatilization and expansion of water during spray drying.

[0032] 3. The specific Ca / P molar ratio of the calcium hydroxyapatite raw material of the present invention can improve the high temperature resistance of the calcium hydroxyapatite raw material, so that the calcium hydroxyapatite raw material can be sintered at a specific temperature, further improving the density, compactness and crystallinity of the finally obtained calcium hydroxyapatite microspheres, and is not prone to degradation.

[0033] 4. The specific average particle size of the calcium hydroxyapatite raw material of the present invention makes the calcium hydroxyapatite raw material have a higher surface energy, which can further increase the driving force of sintering densification, improve the density, compactness and crystallinity of the prepared calcium hydroxyapatite microspheres, and further reduce the degradation rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0035] Figure 1 is the XRD pattern of the calcium hydroxyapatite microspheres of Examples 1-8 and Comparative Examples 1-4;

[0036] Figure 2 is an optical microscope image of calcium hydroxyapatite microspheres of Example 1;

[0037] Figure 3 This is an optical microscope image of calcium hydroxyapatite microspheres of Comparative Example 1. DETAILED DESCRIPTION

[0038] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0039] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0040] The machine model used for spray drying is an OMLG-5 laboratory spray dryer.

[0041] ICP (inductively coupled plasma spectroscopy) was used to test the Ca / P molar ratio in calcium hydroxyapatite raw material.

[0042] Sintering is carried out in a muffle furnace.

[0043] Example 1

[0044] This embodiment provides a method for preparing calcium hydroxyapatite microspheres, and the specific steps are as follows:

[0045] Preparation of slurry: adding raw calcium hydroxyapatite with an average particle size of 20 nm and a Ca / P molar ratio of 1.67:1 and water, the mass ratio of raw calcium hydroxyapatite to water is 45:55, and adding cordierite with an average particle size of 5 nm, the mass ratio of raw calcium hydroxyapatite to cordierite is 100:0.001, mixing into a uniform slurry, the mixing temperature is 25° C., the mixing time is 30 min, vacuum grinding, the grinding speed is 50 rpm, the vacuum degree is 10 Pa, and the processing time is 1 h;

[0046] Preparation of calcium hydroxyapatite green microspheres, spray drying of the slurry after grinding, wherein the atomizing disk speed is 10000 rpm, the slurry flow rate is 5 kg / h, the drying tower inlet temperature is 170°C, and the outlet temperature is 100°C;

[0047] Sintering of calcium hydroxyapatite microspheres: placing the dried calcium hydroxyapatite green microspheres in a corundum crucible for sintering at a temperature of 1200° C. for 2 hours to obtain calcium hydroxyapatite microspheres;

[0048] The calcium hydroxyapatite microspheres prepared in Example 1 were subjected to XRD test, and the results are shown in Figure 1 In the figure, it can be seen that the XRD diffraction peak of hydroxyapatite calcium microspheres is consistent with the position of the hydroxyapatite standard spectrum (PDF#09-0432), and the diffraction peak is sharp and narrow, indicating that the crystallinity is high. The prepared hydroxyapatite calcium microspheres were observed using an optical microscope, and the results are shown in Figure 2 , it can be seen from the picture that the surface of the sphere is smooth and opaque, indicating that the sphere has good density.

[0049] Example 2

[0050] This embodiment provides a method for preparing calcium hydroxyapatite microspheres. Compared with Example 1, the only difference is that the mass ratio of calcium hydroxyapatite raw material to cordierite is 100:0.003, and the sintering temperature is 1300°C.

[0051] Example 3

[0052] This embodiment provides a method for preparing calcium hydroxyapatite microspheres. Compared with embodiment 1, the only difference is that the sintering temperature is 1550°C.

[0053] Example 4

[0054] This embodiment provides a method for preparing calcium hydroxyapatite microspheres. Compared with Example 2, the only difference is that the mass ratio of calcium hydroxyapatite raw material to water is 50:50.

[0055] Example 5

[0056] This embodiment provides a method for preparing calcium hydroxyapatite microspheres. Compared with Example 2, the only difference is that the mass ratio of calcium hydroxyapatite raw material to water is 60:40.

[0057] Example 6

[0058] This embodiment provides a method for preparing calcium hydroxyapatite microspheres. Compared with Example 4, the only difference is that the average particle size of the calcium hydroxyapatite raw material is 60 nm.

[0059] Example 7

[0060] This embodiment provides a method for preparing calcium hydroxyapatite microspheres. Compared with Example 1, the only difference is that the Ca / P molar ratio in the calcium hydroxyapatite raw material is 1.65:1.

[0061] Example 8

[0062] This embodiment provides a method for preparing calcium hydroxyapatite microspheres, and the specific steps are as follows:

[0063] Preparation of slurry: adding raw calcium hydroxyapatite with an average particle size of 100 nm and a Ca / P molar ratio of 1.68:1 and water, the mass ratio of raw calcium hydroxyapatite to water is 45:55, and adding cordierite with an average particle size of 5 nm, the mass ratio of raw calcium hydroxyapatite to cordierite is 100:0.005, mixing into a uniform slurry, the mixing temperature is 40° C., the mixing time is 60 min, vacuum grinding, the grinding speed is 50 rpm, the vacuum degree is 10 Pa, and the processing time is 1 h;

[0064] Preparation of calcium hydroxyapatite green microspheres, spray drying of the slurry after grinding, wherein the atomizing disk speed is 10000 rpm, the slurry flow rate is 5 kg / h, the drying tower inlet temperature is 150°C, and the outlet temperature is 80°C;

[0065] Sintering of hydroxyapatite calcium microspheres: The dried hydroxyapatite calcium green microspheres are placed in a corundum crucible and sintered at a temperature of 1200° C. for 4 hours to obtain hydroxyapatite calcium microspheres.

[0066] Comparative Example 1

[0067] This comparative example provides a method for preparing calcium hydroxyapatite microspheres. Compared with Example 1, the only difference is that no cordierite is added and the sintering temperature is 1100°C. The prepared calcium hydroxyapatite microspheres are observed using an optical microscope, and the results are shown in Figure 3 , the surface of the sphere is very rough, and a small amount of light passes through the sphere.

[0068] Comparative Example 2

[0069] This comparative example provides a method for preparing calcium hydroxyapatite microspheres, which is different from Example 1 only in that cordierite is not added.

[0070] Comparative Example 3

[0071] This comparative example provides a method for preparing calcium hydroxyapatite microspheres, and the specific steps are as follows:

[0072] Calcium hydroxyapatite raw material with an average particle size of 20 nm and a Ca / P molar ratio of 1.67:1 and water, the mass ratio of the calcium hydroxyapatite raw material to water is 45:55, and cordierite with an average particle size of 5 nm is added at the same time, the mass ratio of the calcium hydroxyapatite raw material to the cordierite is 100:0.001, and mixed into a uniform slurry, the mixing temperature is 25° C., the mixing time is 30 min, and spray drying is performed, wherein the atomizing disk speed is 10000 rpm, the slurry flow rate is 5 kg / h, the drying tower inlet temperature is 170° C., and the outlet temperature is 100° C.; the dried calcium hydroxyapatite green microspheres are placed in a corundum crucible and sintered at a temperature of 1200° C. for 2 h to obtain calcium hydroxyapatite microspheres.

[0073] Comparative Example 4

[0074] This comparative example provides a method for preparing calcium hydroxyapatite microspheres. Compared with Example 1, the only difference is that "mica" is used to replace "cordierite".

[0075] Test Case

[0076] The density test was carried out using a true density meter. The specific steps were as follows: ① Connect the gas line, and the pressure gauge displays 0.16 MPa; ② Turn on the instrument power; ③ Use an electronic balance to weigh 3 g of hydroxyapatite calcium microspheres in a 1 mL sample chamber using the difference method, put the sample chamber into the chamber, and cover the sealing cover; ④ Set the experimental parameters and click to start the test; ⑤ Display the test results after the test is completed;

[0077] The specific formula is: density = actual density / theoretical density × 100%.

[0078] The crystallinity was tested by XRD and calculated by Jade software;

[0079] The specific formula is: crystallinity = crystalline peak area / (crystalline peak area + amorphous peak area) × 100%.

[0080] The degradation rate test method is as follows: ① prepare a citric acid buffer solution with a pH of 3 at 37°C, ② weigh 5 g of hydroxyapatite calcium microspheres to be degraded and add 100 mL of citric acid buffer into a 250 mL conical flask, ③ place the conical flask containing the sample in an environment controlled at 37°C and shake the conical flask at a frequency of 2 Hz, ④ filter with a Buchner funnel and rinse three times with a citric acid buffer solution with a pH of 3 at 37°C, ⑤ dry the filter residue in a 120°C oven for 12 hours, cool to room temperature, and weigh it;

[0081] The specific formula is: degradation rate = (1-mass after degradation / mass before degradation) × 100%.

[0082] Table 1

[0083]

[0084] The calcium hydroxyapatite microspheres prepared in the embodiment of the present invention have excellent density, compactness and crystallinity, and are not prone to degradation.

[0085] By comparing Example 1 and Example 4, it can be seen that the specific mass ratio of the raw material of calcium hydroxyapatite to water in the present invention can further reduce the proportion of the initial spheres formed in the slurry due to drying shrinkage, and avoid deformation of the spheres caused by large shrinkage; at the same time, it can reduce the breakage of the spheres caused by the rapid volatilization and expansion of water during the spray drying process, improve the density, compactness and crystallinity of the prepared calcium hydroxyapatite microspheres, and further reduce the degradation rate.

[0086] By comparing Example 1 with Example 6, it can be seen that the specific average particle size of the calcium hydroxyapatite raw material of the present invention makes the calcium hydroxyapatite raw material have a higher surface energy, which can further increase the driving force for sintering densification, improve the density, density and crystallinity of the prepared calcium hydroxyapatite microspheres, and further reduce the degradation rate.

[0087] By comparing Example 1 with Example 7, it can be seen that the specific Ca / P molar ratio of the hydroxyapatite calcium raw material can improve the high temperature resistance of the hydroxyapatite calcium raw material, so that the hydroxyapatite calcium raw material is sintered at a specific temperature, and the density, compactness and crystallinity of the finally obtained hydroxyapatite calcium microspheres are further improved, and degradation is not easy to occur.

[0088] Comparison of Example 1, Comparative Example 1 and Comparative Example 2 shows that cordierite forms a micro-melting zone between calcium hydroxyapatite raw materials, promotes the separation of surface particles of calcium hydroxyapatite raw materials from calcium hydroxyapatite raw materials, reduces material diffusion resistance, improves fluidity, and the microspheres of Example 1 with added cordierite have higher density, compactness, crystallinity and lower degradation rate; Comparison of Example 1 and Comparative Example 4 shows that not all materials can play the role of cordierite.

[0089] By comparing Example 1 with Comparative Example 3, it can be seen that Example 1, which has been subjected to vacuum grinding, can remove bubbles in the slurry while grinding, further improving the uniformity of the slurry, so that the microspheres finally obtained have excellent density, compactness and crystallinity, and are not easily degraded.

[0090] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. A method for preparing calcium hydroxyapatite microspheres, characterized in that: The following steps are involved: The calcium hydroxyapatite raw material, cordierite and water are mixed to obtain a slurry; the slurry is vacuum ground, spray dried and sintered to obtain calcium hydroxyapatite microspheres; The mass ratio of the calcium hydroxyapatite raw material to cordierite is 100:0.001-0.003; The sintering temperature is 1200-1550°C.

2. The preparation method according to claim 1, characterized in that: The mass ratio of the calcium hydroxyapatite raw material to water is (45-60):(40-55); and / or, the Ca / P molar ratio in the calcium hydroxyapatite raw material is 1.65-1.68:1; And / or, the average particle size of the calcium hydroxyapatite raw material is 20-100 nm; And / or, the average particle size of the cordierite is 5-10 nm.

3. The preparation method according to claim 2, characterized in that: The mass ratio of the calcium hydroxyapatite raw material to water is (50-55):(45-50); And / or, the Ca / P molar ratio in the calcium hydroxyapatite raw material is 1.66-1.67:

1.

4. The preparation method according to claim 2, characterized in that: The average particle size of the calcium hydroxyapatite raw material is 40-80nm.

5. The preparation method according to claim 1, characterized in that: The mixing temperature is 20-40° C., and the mixing time is 30-60 min.

6. The preparation method according to claim 1, characterized in that: The vacuum grinding has a grinding speed of 50-100 rpm, a vacuum degree of 10-100 Pa, and a vacuum grinding time of 1-2 h.

7. The preparation method according to claim 1, characterized in that: The inlet temperature of the spray drying is 150-200°C, and the outlet temperature is 80-100°C.

8. The preparation method according to claim 1, characterized in that: The sintering time is 2-4h.

9. Calcium hydroxyapatite microspheres prepared by any one of the preparation methods of claims 1 to 8.