A kind of ultra-high thermal conductivity graphene composite film and its preparation method and application
By introducing graphene oxide and graphene film prepared by CVD method into the graphene thermal conductive film, a nested structure is formed and graphitized, which solves the problems of low thermal conductivity and high preparation cost, and achieves efficient thermal conductivity and simplicity. preparation process.
Patent Information
- Application Number
- CN202411142982.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-08-20
AI Technical Summary
In the existing technology, graphene thermal conductivity films have low thermal conductivity and high preparation costs, and are difficult to meet the needs of high-frequency and high-power equipment applications. Moreover, the single-layer graphene film transfer process is cumbersome and easy to be damaged, resulting in limited thermal conductivity.
An RGO carbonized film is prepared using an aqueous slurry containing graphene oxide, and the first array and the second array RGO carbonized film layer are formed by drilling. Combined with the graphene film prepared by the CVD method, a nested matching sandwich structure film is formed. After static cold pressing and graphitization treatment, an ultra-high thermal conductivity graphene composite film was produced.
A graphene composite film with large thickness, ultra-high thermal conductivity and high heat flux has been achieved, which simplifies the preparation process, reduces costs, and improves thermal conductivity through covalent bonds, making it suitable for industrial production.
Smart Images

Figure CN118650939B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of thermal conductive films, and in particular relates to an ultra-high thermal conductive graphene composite film and a preparation method and application thereof. Background Art
[0002] With the advancement of modern science and technology, especially in the fields of microelectronics, semiconductors and new energy, the problem of high heat flux density has become increasingly prominent. In order to effectively solve the heat dissipation problem in these fields, high-flux graphite-based thermal conductive films are widely used due to their excellent thermal conductivity. Especially in the fields of 5G communications, high-performance computing, electric vehicles, etc., its market demand has exploded. In addition to the traditional field of electronic heat dissipation, graphite-based thermal conductive films have also been used in aerospace, medical devices, new energy and other fields. Especially in the field of new energy vehicles, as a key material for battery thermal management systems, it plays a key role in improving the safety and performance of batteries. However, in practical applications, the thermal flux of low-thickness graphite films has been difficult to meet the application requirements of high-frequency and high-power devices. Although preparation technology has made significant progress, how to further improve the thermal conductivity of graphite films, reduce their preparation costs and improve their stability remains a technical challenge currently faced.
[0003] In the prior art, chemical vapor deposition (CVD) is a mass-producible method for preparing large-sized, high-quality single-layer graphene. The graphene prepared by this method has a complete crystal structure, few defects, and extremely high thermal conductivity. However, the transfer process of the single-layer graphene film prepared by this method is cumbersome and complicated, and may also cause damage to the film. It is difficult to ensure the integrity of the film, and the heat flux of the single-layer graphene film is low. In addition, the large-sized graphene prepared by chemical vapor deposition is a single-layer graphene film grown on a metal film as a substrate. In order to apply graphene to the application end, the graphene film needs to be transferred down, usually by wet transfer, using solvents such as ionized water and PMMA to peel off, transfer and dissolve the protective film on the surface of the graphene film on various substrates to prepare the graphene film. This method has cumbersome procedures and is prone to damage to the graphene film. In addition, if the treatment is not clean, it will also cause PMMA glue residue, thereby affecting the performance of the graphene film. The wrinkles and stacking of graphene sheets will lead to low orientation of sheets, discontinuous sheets, low density and affect the thermal conductivity of graphene thermal conductive film. These greatly limit its material performance advantage of high thermal conductivity and affect its practical application. The method of preparing graphene thermal conductive film on a large scale in the prior art is to use graphene oxide slurry as raw material, and realize the preparation of high-thickness graphene thermal conductive film through coating, drying, carbonization, graphitization, calendering and other processes. The thickness of the prepared graphene is between 1 and 500 μm. Although it can ensure that it has a high heat flux, there is a problem that the graphene surface is inert and cannot be self-assembled into a film. Graphene oxide has high-density defects, and the discontinuous sheet structure blocks the propagation path of phonons, resulting in low thermal conductivity. Therefore, it is an urgent problem to provide a graphene composite film with simple process, low cost, ultra-high thermal conductivity and high heat flux and a preparation method thereof. Summary of the invention
[0004] The main purpose of the present invention is to provide an ultra-high thermal conductivity graphene composite film and a preparation method and application thereof, so as to overcome the deficiencies of the prior art.
[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:
[0006] An embodiment of the present invention provides a method for preparing an ultra-high thermal conductive graphene composite film, which comprises:
[0007] Providing a graphene film with a substrate; wherein graphene films are grown on both sides of the substrate;
[0008] The RGO carbonized film is prepared by using an aqueous slurry containing graphene oxide;
[0009] Punching two RGO carbonized films respectively to obtain a first array RGO carbonized film layer and a second array RGO carbonized film layer; wherein the first array RGO carbonized film layer has a first array structure, the second array RGO carbonized film layer has a second array structure, and the first array RGO carbonized film layer and the second array RGO carbonized film layer can be nested and matched through the first array structure and the second array structure;
[0010] The graphene film with substrate is assembled with the first array RGO carbonized film layer and the second array RGO carbonized film layer respectively to form a first sandwich structure film and a second sandwich structure film; wherein the first sandwich structure film includes the first array RGO carbonized film layer and the graphene film with substrate on both sides; the second sandwich structure film includes the second array RGO carbonized film layer and the graphene film with copper foil substrate on both sides;
[0011] Furthermore, the first sandwich structure film and the second sandwich structure film are assembled in a nested matching manner using a first array structure and a second array structure, and then subjected to a first static cold pressing treatment, a graphitization heat treatment, and a second static cold pressing treatment to obtain an ultra-high thermal conductivity graphene composite film.
[0012] The embodiment of the present invention also provides an ultra-high thermal conductivity graphene composite film prepared by the aforementioned preparation method.
[0013] An embodiment of the present invention also provides an ultra-high thermal conductivity graphene composite film, comprising: a first graphene film layer, a first array RGO carbonized film layer, a second array RGO carbonized film layer and a second graphene film layer arranged in sequence along a direction perpendicular to the film surface, wherein the first array RGO carbonized film layer has a first array structure, the second array RGO carbonized film layer has a second array structure, and the first array RGO carbonized film layer and the second array RGO carbonized film layer can be overlapped and matched through the first array structure and the second array structure, and a third graphene film layer is distributed in the first array structure and the second array structure, and the third graphene film layer is in contact with the first graphene film layer and the second graphene film layer and has covalent bonds.
[0014] The embodiments of the present invention also provide uses of the aforementioned ultra-high thermal conductivity graphene composite film in the fields of electronic heat dissipation, aerospace, medical equipment or new energy.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] (1) The present invention combines a graphene thermal conductive film prepared by a CVD method with a multilayer graphene thermal conductive film obtained by coating graphene oxide and then thermally reducing it in a special way to produce an ultra-high thermal conductive graphene composite film with large thickness, ultra-high thermal conductivity and high heat flux;
[0017] (2) The preparation process of the ultra-high thermal conductivity graphene composite film provided by the present invention is simple and greatly reduces the cost, making it suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0019] Figure 1 Schematic diagram of a RGO carbonized film array punching model 1 in a typical embodiment of the present invention;
[0020] Figure 2 A schematic diagram of a stacking mode 1 of a sandwich structure film in a typical embodiment of the present invention;
[0021] Figure 3 is a schematic diagram of a RGO carbonized film array punching model 2 in a typical embodiment of the present invention;
[0022] Figure 4 is a schematic diagram of a stacking mode 2 of a sandwich structure film in a typical embodiment of the present invention;
[0023] Figure 5 is a schematic diagram of a stack assembly of two sandwich structure films in a typical embodiment of the present invention;
[0024] Figure 6 It is a schematic diagram of the structure of an ultra-high thermal conductive graphene composite film in a typical embodiment of the present invention. DETAILED DESCRIPTION
[0025] In view of the defects of the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The present invention proposes an ultra-high thermal conductivity graphene composite film and a method for preparing the same; the ultra-high thermal conductivity graphene composite film comprises a graphene film (RGO film) after thermal reduction by coating graphene oxide and a large-area single-layer or few-layer graphene film prepared by chemical vapor deposition (CVD), and the two achieve ultra-high thermal conductivity of the thermal conductive film through a special structural design. The ultra-high thermal conductivity graphene composite film is a single-layer or few-layer (<5 layers) graphene film prepared by CVD method, which is interwoven in the RGO film, while ensuring the structural integrity of the CVD graphene film, and maintaining the overall thickness of the entire composite structure graphene film. The ultra-high thermal conductivity graphene composite film first opens regular, uniformly sized, and distributed holes with a fixed spacing on the RGO carbonized film, and then the upper and lower parts of the open RGO carbonized film are respectively clamped by CVD graphene films with metal substrates such as copper foil. In addition, a three-layer sandwich composite structure membrane of the same size is prepared in the same way. The difference is that the array arrangement of the holes in the RGO carbonized membrane forms a mutually nested structure with the previous one to compensate for the uneven film thickness caused by the holes. The two sandwich-structured composite membranes are stacked together, compacted by equipment, and then graphitized. During the graphitization process, the high temperature will vaporize and remove the metal substrate. At the same time, the metal gas also has the effect of promoting the increase of the graphitization degree of the graphene thermal conductive film. The graphitized composite structure membrane is then compacted by membrane pressing, and finally an ultra-high thermal conductivity graphene composite film with CVD graphene membrane as the mesh and RGO graphene as the filler is obtained.
[0026] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] Specifically, as one aspect of the technical solution of the present invention, a method for preparing an ultra-high thermal conductive graphene composite film includes:
[0028] Providing a graphene film with a substrate; wherein graphene films are grown on both sides of the substrate;
[0029] The RGO carbonized film is prepared by using an aqueous slurry containing graphene oxide;
[0030] Punching two RGO carbonized films respectively to obtain a first array RGO carbonized film layer and a second array RGO carbonized film layer; wherein the first array RGO carbonized film layer has a first array structure, the second array RGO carbonized film layer has a second array structure, and the first array RGO carbonized film layer and the second array RGO carbonized film layer can be nested and matched through the first array structure and the second array structure;
[0031] The graphene film with substrate is assembled with the first array RGO carbonized film layer and the second array RGO carbonized film layer respectively to form a first sandwich structure film and a second sandwich structure film; wherein the first sandwich structure film includes the first array RGO carbonized film layer and the graphene film with substrate on both sides; the second sandwich structure film includes the second array RGO carbonized film layer and the graphene film with copper foil substrate on both sides;
[0032] Furthermore, the first sandwich structure film and the second sandwich structure film are assembled in a nested matching manner using a first array structure and a second array structure, and then subjected to a first static cold pressing treatment, a graphitization heat treatment, and a second static cold pressing treatment to obtain an ultra-high thermal conductivity graphene composite film.
[0033] In some preferred embodiments, the substrate includes any one of a copper foil substrate, a nickel foil substrate, a silver foil substrate, a platinum foil substrate, and an alloy foil substrate, but is not limited thereto.
[0034] In some preferred embodiments, the thickness of the substrate is 5-20 μm.
[0035] In some preferred embodiments, the size of the graphene film with substrate is ≥25 cm 2 .
[0036] In some preferred embodiments, the preparation method specifically comprises:
[0037] Mixing graphene oxide with water and adjusting the pH value to 6-7 with aqueous ammonia to form an aqueous slurry containing graphene oxide;
[0038] And, the aqueous slurry is coated and dried, and then heat-treated at 200°C-400°C for more than 2h in a protective atmosphere, and then carbonized at 900°C-1200°C for 0.5h-3h to obtain an RGO carbonized film.
[0039] In some preferred embodiments, the punching process at least makes the first array RGO carbonized film layer and the second array RGO carbonized film layer have a structure that penetrates the film layer;
[0040] In some preferred embodiments, the first array structure at least allows the graphene films on both sides of the first sandwich structure film to contact and form graphene covalent bonds during graphitization heat treatment;
[0041] In some preferred embodiments, the second array structure at least allows the graphene films on both sides of the second sandwich structure film to contact each other during graphitization heat treatment to form graphene covalent bonds.
[0042] In some preferred embodiments, the preparation method specifically comprises:
[0043] The first sandwich structure film and the second sandwich structure film are assembled by using a first array structure and a second array structure to achieve nested matching, and a first static cold pressing treatment is performed for 300s to 600s under a pressure of 50kN to 1000kN;
[0044] The film obtained by the first static cold pressing treatment is placed in a graphite mold to maintain pressure and placed in a protective atmosphere, and subjected to graphitization heat treatment at 2800° C. to 3100° C. for 1 to 5 hours to obtain a graphitized composite film;
[0045] And, the graphitized composite film is subjected to a second static cold pressing treatment under a pressure of 2000-3000 kN, so as to obtain an ultra-high thermal conductive graphene composite film.
[0046] Furthermore, the pressure increase rate used in the second static cold pressing treatment is 10 kN / s~60 kN / s.
[0047] Furthermore, the time of the second static cold pressing treatment is 1s~5s.
[0048] Furthermore, the number of membrane pressing times in the second static cold pressing treatment is 40 to 80 times.
[0049] Furthermore, the second static cold pressing treatment at least makes the density of the ultra-high thermal conductive graphene composite film greater than 2.1 g / cm 3 .
[0050] In some more specific embodiments, the method for preparing the ultra-high thermal conductive graphene composite film comprises the following steps:
[0051] (1) Purchase or make a double-sided single-layer graphene film grown on a high-purity rolled copper foil with a substrate thickness of 5-20 microns, and the size of the substrate and graphene film should be ≥ 25 cm 2 .
[0052] (2) Purchase or make your own graphene oxide. Use 300 mesh high-purity (carbon content > 99.9%) natural graphite raw material to prepare graphene oxide through the modified Hummer method, and then purify it by filtration and water washing to obtain graphene oxide filter cake. The relevant indicators of graphene oxide are as follows: filter cake solid content ≥40%, graphene oxide oxygen content ≥40%, carbon content ≥40%, sulfur content ≤2%, chlorine content <1.5%, and sheet diameter D50 is 10-50μm. Graphene oxide is a raw material with high oxidation degree and low impurities. Highly oxidized GO has rich oxygen-containing functional groups. During the heat treatment process, it can ensure the formation of strong covalent bonds between each graphene oxide sheet, and also ensure the formation of strong covalent bonds between graphene oxide and CVD graphene membrane network.
[0053] (3) The graphene oxide is prepared into a 0.5-5% aqueous slurry, the pH value of the slurry is adjusted to between 6 and 7 with ammonia water, the slurry is dispersed by a homogenizer to ensure uniformity, coated by a coater, dried in an oven at 60°C, heat treated at 400°C under a protective gas atmosphere, and carbonized at 900°C under a protective gas atmosphere to obtain an RGO carbonized film.
[0054] (4) RGO carbonized film according to Figure 1 The array pattern is punched, and the hole diameter is 0.5cm 2 -10cm 2 Within the range, the size of the holes should ensure that the graphene on the upper and lower copper foil substrates can fully contact each other and form covalent bonds in the subsequent graphitization process, so as to form a network structure of high-quality graphene film.
[0055] (5) Cut the double-sided single-layer graphene film with copper foil substrate and RGO carbonized film into the same size and press Figure 2 way to stack.
[0056] (6) RGO carbonized film according to Figure 3 The array pattern is punched, and the hole diameter is 0.5cm 2 -10cm 2 within the range.
[0057] (7) Cut the double-sided single-layer graphene film with copper foil substrate and RGO carbonized film into the same size and press Figure 4 The double-sided single-layer graphene film with a copper foil substrate is stacked with the RGO carbonized film in steps (6) and (7) respectively.
[0058] (8) The two stacked composite films are pressed Figure 5 The stacking method of nesting each other can ensure that the entire membrane structure has a relatively uniform thickness, and at the same time can form a structure in which the CVD graphene membrane is a high thermal conductivity network channel.
[0059] (9) The stacked membranes are compacted by static cold pressing to remove the air in the composite membrane. The pressure is between 50 kN and 1000 kN. Static cold pressing can ensure close contact between the layers of the membranes so that a covalent bond network can be formed during the subsequent graphitization process.
[0060] (10) The composite film is clamped with a graphite mold and placed vertically in a graphitization furnace for heat treatment at 2800℃~3100℃ for 1-5h. During this period, inert gas is used as a protective gas. The vertical placement is conducive to the dispersion of copper vapor from the metal substrate. Copper vapor also has a catalytic cracking effect on carbon materials and can repair the structural defects of the graphene film under high temperature conditions.
[0061] (11) The graphitized composite film is subjected to static cold pressing on a molding press with a pressure range of 2000-3000 kN, which increases the density of the graphene composite structure thermal conductive film to > 2.1 g / cm 3 , and obtain an ultra-high thermal conductive graphene composite film.
[0062] The ultra-high thermal conductivity graphene composite film prepared in the present invention has the following advantages:
[0063] (1) The graphene thermal conductive film prepared by the CVD method has the characteristics of high structural integrity and low defect density. It exhibits high thermal conductivity in terms of thermal conductivity, but its thickness is too thin, resulting in too low heat flux, which limits its practical application. The multilayer graphene thermal conductive film obtained by coating graphene oxide and then thermally reducing it can be made very thick. Although it can ensure that it has a high heat flux, it has problems such as the inertness of the graphene surface, the inability to self-assemble into a film, the high-density defects of graphene oxide, and the discontinuous lamellar structure that blocks the propagation path of phonons, resulting in low thermal conductivity. The present invention uses a special structural design to form a composite structure thermal conductive film with a CVD graphene film as a network and an RGO film as a filler by using the thin films prepared by the two methods. It can effectively solve the shortcomings of the above two materials and greatly improve the thermal conductivity and heat flux of the graphene thermal conductive film;
[0064] (2) In general, large-scale graphene prepared by chemical vapor deposition is a single-layer graphene film grown on a metal film as a substrate. In order to apply graphene to the application end, the graphene film needs to be transferred down. Usually, the graphene film is prepared by wet transfer, using solvents such as ionized water and PMMA to remove, transfer and dissolve the protective film on the surface of the graphene film on various substrates. This method is cumbersome and easy to cause damage to the graphene film. In addition, if it is not handled cleanly, it will also cause PMMA glue to remain, thereby affecting the performance of the graphene film. In order to ensure the integrity of the CVD graphene film structure and the operability of the structural design of the composite film, the metal substrate is attached for stacking operation. This method is simple to operate and has high controllable structure precision. In addition, the metal substrate can be gasified and removed under the subsequent high-temperature graphitization of 2800℃~3100℃, which not only ensures the integrity of the graphene structure, but also completely removes impurities in the graphene film.
[0065] (3) The copper foil substrate in the composite structure thermal conductive film precursor of the present invention also plays a role in catalyzing graphitization in the graphite chemical industry at 3000°C. Copper vapor can catalytically crack the surrounding solid carbon source under high temperature conditions, and the carbon source is cracked into active carbon atoms, which can re-epitaxially grow along the original single-layer graphene, thereby improving the graphitization degree of the overall composite film. In addition, the high-temperature graphitization process can effectively repair the structural defects caused by the film stacking and compaction process, greatly improving the thermal conductivity of the graphene composite structure thermal conductive film.
[0066] (4) The CVD single-layer graphene thermal conductive film of the present invention acts as a high-speed channel for phonon propagation in the composite structure. During the high-temperature graphitization process, the CVD single-layer graphene can form a good covalent bond with the RGO graphene, which is beneficial to the propagation and diffusion of phonons and greatly improves the thermal diffusion coefficient of the overall thermal conductive film.
[0067] (5) The RGO carbonized film in the present invention is perforated in an array and then stacked so that the CVD single-layer graphene film is completely distributed in the composite film. The thickness of the perforated part is missing and is complemented by stacking another RGO carbonized film with complementary array perforations, thereby ensuring the uniformity of the overall composite film thickness and high heat flux stability. This method is simple to operate and easy to implement.
[0068] Another aspect of the embodiments of the present invention further provides an ultra-high thermal conductivity graphene composite film obtained by the aforementioned preparation method.
[0069] Another aspect of an embodiment of the present invention also provides an ultra-high thermal conductivity graphene composite film, comprising: a first graphene film layer, a first array RGO carbonized film layer, a second array RGO carbonized film layer and a second graphene film layer arranged in sequence along the direction perpendicular to the film surface, wherein the first array RGO carbonized film layer has a first array structure, the second array RGO carbonized film layer has a second array structure, and the first array RGO carbonized film layer and the second array RGO carbonized film layer can be overlapped and matched through the first array structure and the second array structure, and the first array structure and the second array structure are distributed with a third graphene film layer, and the third graphene film layer is in contact with the first graphene film layer and the second graphene film layer and has a covalent bond.
[0070] In some preferred embodiments, the ultrahigh thermal conductive graphene composite film has a thickness of 20 μm to 80 μm.
[0071] In some preferred embodiments, the density of the ultra-high thermal conductive graphene composite film is greater than 2.1 g / cm 3 .
[0072] In some preferred embodiments, the thermal diffusion coefficient of the ultrahigh thermal conductive graphene composite film is 900-1100 mm / s.
[0073] In some preferred embodiments, the thermal conductivity of the ultrahigh thermal conductive graphene composite film is 1600~2050W / mk.
[0074] Another aspect of the embodiments of the present invention further provides the use of the aforementioned ultra-high thermal conductivity graphene composite film in the fields of electronic heat dissipation, aerospace, medical equipment or new energy.
[0075] For example: the use of the ultra-high thermal conductivity graphene composite film as a key material for battery thermal management systems in the field of energy vehicles.
[0076] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments and drawings. This embodiment is implemented on the premise of the technical solution of the invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.
[0077] Unless otherwise specified, the experimental materials used in the following examples can be purchased from conventional biochemical reagent companies.
[0078] Example 1
[0079] (1) Purchase or make a double-sided single-layer graphene film grown on a high-purity rolled copper foil with a substrate thickness of 20 μm, and cut the substrate and graphene film into four films of 10 cm × 10 cm in size.
[0080] (2) Purchase or make your own graphene oxide, use 300 mesh high-purity (carbon content 99.93%) natural graphite raw material to prepare graphene oxide through the modified Hummer method, and then purify it by filtration and water washing to obtain graphene oxide filter cake. The relevant indicators of graphene oxide are as follows: filter cake solid content 40.5%, graphene oxide oxygen content 42.5%, carbon content 42.7%, sulfur content 1.95%, chlorine content 1.05%, and flake diameter D50 is 32μm.
[0081] (3) Take 296.3g of graphene oxide filter cake, 3673.7g of pure water and 30g of ammonia water, place them in a planetary agitator for stirring and slurrying, and prepare a 3% aqueous graphene oxide slurry. The slurry pH is measured to be 6.5. The slurry is dispersed by a homogenizer to ensure uniformity, and homogenized twice, with homogenization pressures of 750 bar and 850 bar respectively; the coating is applied by a coater with a coating thickness of 3mm, and the coated original film is placed in a 60°C forced air drying oven for 8h. The dried film is then placed in a muffle furnace for heat treatment at a temperature of 400°C under a protective gas N2 atmosphere for 2 hours. The heat-treated film is then placed in a carbonization furnace and carbonized at 900°C under a protective gas N2 atmosphere for 3h to obtain an RGO carbonized film.
[0082] (4) Cut the RGO carbonized original film into 10 cm × 10 cm size and use a mold to punch holes in an array. The size of the holes is 1 cm × 1 cm. Prepare two arrays: punching model 1 (such as Figure 1 ) and punch model 2 (such as Figure 3 ).
[0083] (5) Two 10 cm × 10 cm double-sided single-layer graphene films with copper foil substrates and a 10 cm × 10 cm perforated RGO carbonized film of model 1 were placed on the Figure 2 The stacking method is as follows: from top to bottom, there is a sandwich structure of a graphene film with a copper foil substrate, an RGO carbonized film of perforated model 1, and a graphene film with a copper foil substrate.
[0084] (6) Two 10 cm × 10 cm double-sided single-layer graphene films with copper foil substrates and a 10 cm × 10 cm perforated model 2 RGO carbonized film were placed on the Figure 4 The stacking method is as follows: from top to bottom, there is a sandwich structure of a graphene film with a copper foil substrate, an RGO carbonized film of perforated model 2, and a graphene film with a copper foil substrate.
[0085] (7) The two sandwich structure membranes prepared in step (5) and step (6) are pressed Figure 5The stacking is performed in a manner to form a stacked composite structure comprising, from top to bottom, a graphene film with a copper foil substrate, an RGO carbonized film of perforated model 1, a graphene film with a copper foil substrate, a graphene film with a copper foil substrate, an RGO carbonized film of perforated model 2, and a graphene film with a copper foil substrate.
[0086] (8) The film obtained in step (7) is subjected to static cold pressing by a film press with a pressing pressure of 500 kN and a pressing time of 500 s.
[0087] (9) The composite film of step (8) is clamped with a graphite mold and placed vertically in a graphitization furnace for heat treatment at 3000° C. in a protective gas N 2 atmosphere for 1 h.
[0088] (10) The graphitized composite film was taken out and subjected to static cold pressing on a molding machine. A 7075 aviation aluminum plate was used as a fixture for film pressing. The pressure increase rate was 60 kN / s, the target pressure was 3000 kN, the pressure was maintained for 1 s, and the film pressing times were 60 times. An ultra-high thermal conductive graphene composite film was obtained. The density of the film was measured to be 2.19 g / cm 3 , thermal diffusion coefficient is 1100 mm / s, thermal conductivity is 2050W / mk, and thickness is 40μm.
[0089] Comparative Example 1
[0090] (1) Purchase or make your own graphene oxide, use 300 mesh high-purity (carbon content 99.93%) natural graphite raw material to prepare graphene oxide through the modified Hummer method, and purify it by filtration and water washing to obtain graphene oxide filter cake. The relevant indicators of graphene oxide are as follows: filter cake solid content 40.5%, oxygen content 42.5%, carbon content 42.7%, sulfur content 1.95%, chlorine content 1.05%, and flake diameter D50 is 32μm.
[0091] (2) Take 296.3g of graphene oxide filter cake, 3673.7g of pure water and 30g of ammonia water, place them in a planetary stirrer for stirring and slurrying, and prepare a 3% aqueous graphene oxide slurry. The slurry pH is measured to be 6.5. The slurry is dispersed by a homogenizer to ensure uniformity, and homogenized twice, with homogenization pressures of 750 bar and 850 bar respectively; the coating is applied by a coater with a coating thickness of 3mm, and the coated original film is placed in a 60°C forced air drying oven for 8h. The dried film is then placed in a muffle furnace for heat treatment at a temperature of 400°C under a protective gas N2 atmosphere for 2h. The heat-treated film is then placed in a carbonization furnace for carbonization at 900°C under a protective gas N2 atmosphere. The carbonized film is then placed vertically in a graphitization furnace for heat treatment at 3000°C under a protective gas N2 atmosphere for 1h.
[0092] (3) Take out the graphitized RGO film and perform static cold pressing on the molding machine. Use 7075 aviation aluminum plate as a fixture for film pressing. The pressure increase rate is 60 kN / s, the target pressure is 3000 kN, the pressure is maintained for 1 second, and the film pressing times are 60 times. The RGO thermal conductive film is obtained, and the density of the film is measured to be 2.18 g / cm 3 , thermal diffusion coefficient is 796mm / s, thermal conductivity is 1475W / mk, and thickness is 40μm.
[0093] Example 2
[0094] (1) Purchase or make a double-sided single-layer graphene film grown on a high-purity rolled copper foil with a substrate thickness of 5 μm, and cut the substrate and graphene film into four films of 5 cm × 5 cm in size.
[0095] (2) Purchase or make your own graphene oxide, use 1000 mesh high-purity (carbon content 99.93%) natural graphite raw material to prepare graphene oxide through the modified Hummer method, and then purify it by filtration and water washing to obtain graphene oxide filter cake. The relevant indicators of graphene oxide are as follows: filter cake solid content 40%, oxygen content 41%, carbon content 40%, sulfur content 1.53%, chlorine content 1.03%, and flake diameter D50 is 10μm.
[0096] (3) Take 300g of graphene oxide filter cake, 3670g of pure water and 30g of ammonia water, place them in a planetary agitator for stirring and slurrying, and prepare a 3% aqueous graphene oxide slurry. The slurry pH is measured to be 6.0. The slurry is dispersed by a homogenizer to ensure uniformity, and homogenized twice, with homogenization pressures of 750 bar and 850 bar respectively; the coating is applied by a coater with a coating thickness of 1.5mm. The coated original film is placed in a 60°C forced air drying oven for 8h of drying. The dried film is then placed in a muffle furnace for heat treatment at a temperature of 200°C under a protective gas N2 atmosphere for 3 hours. The heat-treated film is then placed in a carbonization furnace and carbonized at 1200°C under a protective gas N2 atmosphere for 0.5h to obtain an RGO carbonized film.
[0097] (4) Cut the RGO carbonized original film into 5 cm × 5 cm size and use a mold to punch holes in an array. The hole size is 1 cm × 1 cm. Prepare two arrays: punching model 1 (such as Figure 1 ) and punch model 2 (such as Figure 3 ).
[0098] (5) Two 5cm×5cm double-sided single-layer graphene films with copper foil substrates and a 5cm×5cm perforated RGO carbonized film of model 1 were placed on the Figure 2The stacking method is as follows: from top to bottom, there is a sandwich structure of a graphene film with a copper foil substrate, an RGO carbonized film of perforated model 1, and a graphene film with a copper foil substrate.
[0099] (6) Two 5cm×5cm double-sided single-layer graphene films with copper foil substrates and a 5cm×5cm perforated model 2 RGO carbonized film were placed on the surface of the film. Figure 4 The stacking method is as follows: from top to bottom, there is a sandwich structure of a graphene film with a copper foil substrate, an RGO carbonized film of perforated model 2, and a graphene film with a copper foil substrate.
[0100] (7) The two sandwich structure membranes prepared in step (5) and step (6) are pressed Figure 5 The stacking is performed in a manner to form a stacked composite structure comprising, from top to bottom, a graphene film with a copper foil substrate, an RGO carbonized film of perforated model 1, a graphene film with a copper foil substrate, a graphene film with a copper foil substrate, an RGO carbonized film of perforated model 2, and a graphene film with a copper foil substrate.
[0101] (8) The film obtained in step (7) is subjected to static cold pressing by a film press, with a pressing pressure of 1000 kN and a pressing time of 300 s.
[0102] (9) The composite film of step (8) was clamped with a graphite mold and placed vertically in a graphitization furnace for heat treatment at 3100°C under a protective gas N2 atmosphere for 5 hours.
[0103] (10) The graphitized composite film was taken out and subjected to static cold pressing on a molding machine. A 7075 aviation aluminum plate was used as a fixture for film pressing. The pressure increase rate was 10 kN / s, the target pressure was 2000 kN, the pressure was maintained for 5 s, and the film pressing times were 40 times. An ultra-high thermal conductive graphene composite film was obtained. The density of the film was measured to be 2.21 g / cm 3 , thermal diffusion coefficient is 1003 mm / s, thermal conductivity is 1884W / mk, and thickness is 20μm.
[0104] Example 3
[0105] (1) Purchase or make a double-sided single-layer graphene film grown on a high-purity rolled copper foil with a substrate thickness of 15 μm, and cut the substrate and graphene film into four films of 20 cm × 20 cm in size.
[0106] (2) Purchase or make your own graphene oxide, use 150 mesh high-purity (carbon content 99.93%) natural graphite raw material to prepare graphene oxide through the modified Hummer method, and purify it by filtration and water washing to obtain graphene oxide filter cake. The relevant indicators of graphene oxide are as follows: filter cake solid content 44.8%, oxygen content 43.7%, carbon content 44.5%, sulfur content 2%, chlorine content 1.5%, and flake diameter D50 is 50μm.
[0107] (3) Take 267.8g of graphene oxide filter cake, 370.22g of pure water and 30g of ammonia water, place them in a planetary agitator for stirring and slurrying, and prepare a 3% aqueous graphene oxide slurry. The slurry pH is measured to be 7.0. The slurry is dispersed by a homogenizer to ensure uniformity, and homogenized twice, with homogenization pressures of 750 bar and 850 bar respectively; the coating is applied by a coater with a coating thickness of 6mm. The coated original film is placed in a 60°C forced air drying oven for 8h. The dried film is then placed in a muffle furnace for heat treatment at a temperature of 200°C under a protective gas N2 atmosphere for 4 hours. The heat-treated film is then placed in a carbonization furnace and carbonized at 1200°C under a protective gas N2 atmosphere for 1.5h to obtain an RGO carbonized film.
[0108] (4) Cut the RGO carbonized original film into 20 cm × 20 cm size and use a mold to punch holes in an array. The hole size is 1 cm × 1 cm. Prepare two arrays: punching model 1 (such as Figure 1 ) and punch model 2 (such as Figure 3 ).
[0109] (5) Two 20 cm × 20 cm double-sided single-layer graphene films with copper foil substrates and a 20 cm × 20 cm perforated model 1 RGO carbonized film were placed on the Figure 2 The stacking method is as follows: from top to bottom, there is a sandwich structure of a graphene film with a copper foil substrate, an RGO carbonized film of perforated model 1, and a graphene film with a copper foil substrate.
[0110] (6) Two 20 cm × 20 cm double-sided single-layer graphene films with copper foil substrates and a 20 cm × 20 cm perforated model 2 RGO carbonized film were placed on the Figure 4 The stacking method is as follows: from top to bottom, there is a sandwich structure of a graphene film with a copper foil substrate, an RGO carbonized film of perforated model 2, and a graphene film with a copper foil substrate.
[0111] (7) The two sandwich structure membranes prepared in step (5) and step (6) are pressed Figure 5The stacking is performed in a manner to form a stacked composite structure comprising, from top to bottom, a graphene film with a copper foil substrate, an RGO carbonized film of perforated model 1, a graphene film with a copper foil substrate, a graphene film with a copper foil substrate, an RGO carbonized film of perforated model 2, and a graphene film with a copper foil substrate.
[0112] (8) The film obtained in step (7) was subjected to static cold pressing by a film press, with a pressing pressure of 525 kN and a pressing time of 150 s.
[0113] (9) The composite film of step (8) is clamped with a graphite mold and placed vertically in a graphitization furnace for heat treatment at 2800°C under a protective gas N2 atmosphere for 3 hours.
[0114] (10) The graphitized composite film was taken out and subjected to static cold pressing on a molding machine. A 7075 aviation aluminum plate was used as a fixture for film pressing. The pressure increase rate was 40 kN / s, the target pressure was 2500 kN, the pressure was maintained for 3 s, and the number of film pressings was 80 times. An ultra-high thermal conductive graphene composite film was obtained. The density of the film was measured to be 2.18 g / cm 3 , thermal diffusion coefficient is 900 mm / s, thermal conductivity is 1668 W / mk, and thickness is 80μm.
[0115] Example 4
[0116] (1) Purchase or make a double-sided single-layer graphene film grown on a high-purity rolled copper foil with a substrate thickness of 10 μm, and cut the substrate and graphene film into four films of 15 cm × 15 cm in size.
[0117] (2) Purchase or make your own graphene oxide, use 600 mesh high-purity (carbon content 99.93%) natural graphite raw material to prepare graphene oxide through the modified Hummer method, and purify it by filtration and water washing to obtain graphene oxide filter cake. The relevant indicators of graphene oxide are as follows: filter cake solid content 40.5%, oxygen content 42.5%, carbon content 42.7%, sulfur content 1.06%, chlorine content 1.25%, and flake diameter D50 is 20.5μm.
[0118] (3) Take 296.3g of graphene oxide filter cake, 3673.7g of pure water and 30g of ammonia water, place them in a planetary agitator for stirring and slurrying, and prepare a 3% aqueous graphene oxide slurry. The slurry pH is measured to be 6.8. The slurry is dispersed by a homogenizer to ensure uniformity, and homogenized twice, with homogenization pressures of 750 bar and 850 bar respectively; the coating is applied by a coater with a coating thickness of 6mm. The coated original film is placed in a 60°C forced air drying oven for 8h. The dried film is then placed in a muffle furnace for heat treatment at a temperature of 300°C under a protective gas N2 atmosphere for 2.5 hours. The heat-treated film is then placed in a carbonization furnace and carbonized at 1100°C under a protective gas N2 atmosphere for 2.5h to obtain an RGO carbonized film.
[0119] (4) Cut the RGO carbonized original film into a size of 15 cm × 15 cm, and use a mold to punch holes in an array shape. The hole size is 1 cm × 1 cm. Prepare two arrays: punching model 1 (such as Figure 1 ) and punch model 2 (such as Figure 3 ).
[0120] (5) Place two 15 cm × 15 cm double-sided single-layer graphene films with copper foil substrates and a 15 cm × 15 cm perforated model 1 RGO carbonized film on a plate. Figure 2 The stacking method is as follows: from top to bottom, there is a sandwich structure of a graphene film with a copper foil substrate, an RGO carbonized film of perforated model 1, and a graphene film with a copper foil substrate.
[0121] (6) Two 15 cm × 15 cm double-sided single-layer graphene films with copper foil substrates and a 15 cm × 15 cm perforated model 2 RGO carbonized film were placed on the Figure 4 The stacking method is as follows: from top to bottom, there is a sandwich structure of a graphene film with a copper foil substrate, an RGO carbonized film of perforated model 2, and a graphene film with a copper foil substrate.
[0122] (7) The two sandwich structure membranes prepared in step (5) and step (6) are pressed Figure 5 The stacking is performed in a manner to form a stacked composite structure comprising, from top to bottom, a graphene film with a copper foil substrate, an RGO carbonized film of perforated model 1, a graphene film with a copper foil substrate, a graphene film with a copper foil substrate, an RGO carbonized film of perforated model 2, and a graphene film with a copper foil substrate.
[0123] (8) The film obtained in step (7) is subjected to static cold pressing by a film press, with a pressing pressure of 50 kN and a pressing time of 400 s.
[0124] (9) The composite film of step (8) is clamped with a graphite mold and placed vertically in a graphitization furnace for heat treatment at 2900°C under a protective gas N2 atmosphere for 1 hour.
[0125] (10) The graphitized composite film was taken out and subjected to static cold pressing on a molding machine. A 7075 aviation aluminum plate was used as a fixture for film pressing. The pressure increase rate was 50 kN / s, the target pressure was 2800 kN, the pressure was maintained for 2 s, and the film pressing times were 50 times. An ultra-high thermal conductive graphene composite film was obtained. The density of the film was measured to be 2.22 g / cm 3 , thermal diffusion coefficient is 1005 mm / s, thermal conductivity is 1896W / mk, and thickness is 60μm.
[0126] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0127] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.
Claims
1. A method for preparing an ultra-high thermal conductive graphene composite film, characterized in that: include: Providing a graphene film with a substrate; wherein graphene films are grown on both sides of the substrate; A RGO carbonized film is prepared by using a water-based slurry containing graphene oxide; wherein the RGO carbonized film is a graphene film that is thermally reduced by coating graphene oxide; Punching two RGO carbonized films respectively to obtain a first array RGO carbonized film layer and a second array RGO carbonized film layer; wherein the first array RGO carbonized film layer has a first array structure, the second array RGO carbonized film layer has a second array structure, and the first array RGO carbonized film layer and the second array RGO carbonized film layer can be nested and matched through the first array structure and the second array structure; The graphene film with substrate is assembled with the first array RGO carbonized film layer and the second array RGO carbonized film layer respectively to form a first sandwich structure film and a second sandwich structure film; wherein the first sandwich structure film includes the first array RGO carbonized film layer and the graphene film with substrate on both sides; the second sandwich structure film includes the second array RGO carbonized film layer and the graphene film with copper foil substrate on both sides; In addition, the first sandwich structure film and the second sandwich structure film are assembled in a nested matching manner using a first array structure and a second array structure, and a first static cold pressing treatment is performed for 300 to 600 seconds under a pressure condition of 50 kN to 1000 kN; then, a graphite mold is used to place the film obtained by the first static cold pressing treatment in a graphite mold to maintain pressure and placed in a protective atmosphere, and a graphitization heat treatment is performed at 2800°C to 3100°C for 1 to 5 hours to obtain a graphitized composite film; finally, the graphitized composite film is subjected to a second static cold pressing treatment under a pressure condition of 2000 to 3000 kN to obtain an ultra-high thermal conductivity graphene composite film.
2. The preparation method according to claim 1, characterized in that: The substrate includes any one of a copper foil substrate, a nickel foil substrate, a silver foil substrate, a platinum foil substrate, and an alloy foil substrate; And / or, the thickness of the substrate is 5-20 μm; And / or, the size of the graphene film with substrate is ≥25 cm 2 .
3. The preparation method according to claim 1, characterized in that: Specifically include: Mixing graphene oxide with water and adjusting the pH value to 6-7 with aqueous ammonia to form an aqueous slurry containing graphene oxide; And, the aqueous slurry is coated and dried, and then heat-treated at 200°C-400°C for more than 2h in a protective atmosphere, and then carbonized at 900°C-1200°C for 0.5h-3h to obtain an RGO carbonized film.
4. The preparation method according to claim 1, characterized in that: The punching process at least makes the first array RGO carbonized film layer and the second array RGO carbonized film layer have a structure that penetrates the film layer; And / or, the first array structure at least allows the graphene films on both sides of the first sandwich structure film to contact each other during graphitization heat treatment to form graphene covalent bonds; And / or, the second array structure at least enables the graphene films on both sides of the second sandwich structure film to contact each other during the graphitization heat treatment to form graphene covalent bonds.
5. The preparation method according to claim 1, characterized in that: The second static cold pressing process uses a pressure increase rate of 10 kN / s to 60 kN / s; And / or, the second static cold pressing treatment time is 1s to 5s; And / or, the number of membrane pressing times of the second static cold pressing treatment is 40 to 80 times; And / or, the second static cold pressing treatment at least makes the density of the ultra-high thermal conductive graphene composite film greater than 2.1 g / cm 3 .
6. An ultra-high thermal conductive graphene composite film prepared by the preparation method according to any one of claims 1 to 5.
7. An ultra-high thermal conductivity graphene composite film, characterized in that: include: A first graphene film layer, a first array RGO carbonized film layer, a second array RGO carbonized film layer and a second graphene film layer are arranged in sequence in a direction perpendicular to the film surface, wherein the first array RGO carbonized film layer has a first array structure, the second array RGO carbonized film layer has a second array structure, and the first array RGO carbonized film layer and the second array RGO carbonized film layer can be nested and matched through the first array structure and the second array structure, a third graphene film layer is distributed between the first array structure and the second array structure, and the third graphene film layer is in contact with the first graphene film layer and the second graphene film layer and has a covalent bond, and the first array structure and the second array structure are independently holes with a fixed spacing, regularity, uniform size and display distribution.
8. The ultra-high thermal conductivity graphene composite film according to claim 7, characterized in that: The thickness of the ultra-high thermal conductive graphene composite film is 20 μm to 80 μm; And / or, the density of the ultra-high thermal conductive graphene composite film is greater than 2.1 g / cm 3 ; And / or, the thermal diffusion coefficient of the ultra-high thermal conductive graphene composite film is 900-1100 mm / s; And / or, the thermal conductivity of the ultra-high thermal conductivity graphene composite film is 1600~2050W / mk.
9. Use of the ultra-high thermal conductive graphene composite film according to any one of claims 6 to 8 in the fields of electronic heat dissipation, aerospace, medical equipment or new energy.