A method for preparing a bending-resistant ceramic plate

Through the combination of specific ceramic components and additives, a spatial network structure is formed and the process is optimized during the sintering process, the problem of insufficient bending strength of the ceramic plate is solved, and the high bending strength and good toughness of the ceramic plate are achieved, which is suitable for architectural applications.

CN118652109BActive Publication Date: 2024-11-15GUANGDONG XINRUNCHENG CERAMICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411133034.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-15
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The bending strength of existing ceramic plates is less than 150MPa, resulting in insufficient toughness and poor bending resistance in architectural applications.

Method used

Use specific ceramic components (potassium feldspar, sodium feldspar, kaolin, bentonite, illite and zirconia) to combine graphene oxide, carbon nanotubes, fullerene chloride and yttrium oxide to pass through the spatial network structure and uniformity Dispersion improves toughness and bending strength of ceramic plates, and optimizes heating and cooling rates during sintering to improve compatibility and bending strength.

Benefits of technology

The bending strength of the ceramic plate is prepared exceeds 150MPa, such as 153-165MPa, which significantly improves the application performance of the ceramic plate.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of building ceramics, and discloses a method for preparing a bending-resistant ceramic plate. The method for preparing the bending-resistant ceramic plate comprises the following steps: by weight, 20 parts of potassium feldspar, 12-20 parts of sodium feldspar, 3-8 parts of kaolin, 6-12 parts of bentonite, 15-30 parts of illite, 0.1-1 parts of zirconium oxide, and 30-70 parts of solvent are mixed, 0.5-3 parts of additives are added, stirred and dispersed, slurry is obtained, and then spray granulation is performed to obtain a blank, and then compression molding is performed to obtain a green body, sintering, and a ceramic plate is obtained; the additive includes graphene oxide, carbon nanotubes, fullerene chloride and yttrium oxide, and at least two of calcium chloride, yttrium chloride, and vanadium pentoxide. The ceramic plate of the present invention has good toughness, and its corresponding bending strength exceeds 150MPa, for example, 153-165MPa, which is very beneficial to the application of the ceramic plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building ceramics, and in particular relates to a method for preparing a bending-resistant ceramic plate. Background Art

[0002] Ceramic panels are widely used in the construction industry. However, due to their large area and thin thickness, ceramic panels are prone to problems such as insufficient toughness and poor bending resistance during use. In order to increase the bending strength, ceramic panels in the prior art often mix a large amount of reinforcing particles with ceramic raw materials during the preparation of the ceramic panels. However, the addition of a large amount of reinforcing particles easily leads to poor uniformity in the dispersion of the raw materials, resulting in unstable bending strength of the final ceramic panels. Moreover, with the increase in market requirements, the bending strength of ceramic panels prepared by existing methods is often lower than 150MPa, which limits the application of ceramic panels to a certain extent.

[0003] Therefore, there is an urgent need to provide a new ceramic plate with good bending resistance. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a method for preparing a bending-resistant ceramic plate. The ceramic plate of the present invention has good toughness, and its corresponding bending strength exceeds 150MPa, for example, 153-165MPa, which is very beneficial to the application of the ceramic plate.

[0005] The inventive concept of the present invention is as follows: the ceramic plate of the present invention is introduced with additives by combining specific ceramic components (20 parts of potassium feldspar, 12-20 parts of sodium feldspar, 3-8 parts of kaolin, 6-12 parts of bentonite, 15-30 parts of illite, and 1-3 parts of zirconium oxide), wherein the additives include graphene oxide, carbon nanotubes, fullerene chloride and yttrium oxide, and at least two of calcium chloride, yttrium chloride, and vanadium pentoxide, wherein the graphene oxide, carbon nanotubes, and fullerene chloride are mutually dispersed to form a spatial network structure, and yttrium oxide is uniformly dispersed in the network structure, and further, with the combination of at least two of calcium chloride, yttrium chloride, and vanadium pentoxide, it is helpful to improve the dispersion uniformity of the additives and the specific ceramic components, and improve the toughness of the finally obtained ceramic plate, thereby also improving the bending strength of the ceramic plate.

[0006] Furthermore, through the temperature increase process during the sintering process of the present invention, the compatibility of the additive of the present invention with the specific ceramic component is further improved, which is beneficial to the improvement of the bending strength of the ceramic plate.

[0007] The present invention provides a method for preparing a bending-resistant ceramic plate, comprising the following steps:

[0008] By weight ratio, 20 parts of potassium feldspar, 12-20 parts of sodium feldspar, 3-8 parts of kaolin, 6-12 parts of bentonite, 15-30 parts of illite, 0.1-1 part of zirconium oxide, and 30-70 parts of solvent are mixed, 0.5-3 parts of additives are added, and the mixture is stirred and dispersed to obtain a slurry, and then spray granulation is performed to obtain a blank, and then press molding is performed to obtain a green body, and sintering is performed to obtain the ceramic plate;

[0009] The additives include graphene oxide, carbon nanotubes, fullerene chloride and yttrium oxide, and at least two of calcium chloride, yttrium chloride and vanadium pentoxide.

[0010] Preferably, by weight, 20 parts of potassium feldspar, 12-16 parts of sodium feldspar, 5-8 parts of kaolin, 7-12 parts of bentonite, 15-25 parts of illite, 0.5-0.8 parts of zirconium oxide, and 40-60 parts of solvent are mixed, 1-2 parts of additives are added, and the mixture is stirred and dispersed to obtain a slurry.

[0011] Preferably, the additives, by weight, include 0.2-0.8 parts of graphene oxide, 0.1-0.5 parts of carbon nanotubes, 0.1-0.3 parts of fullerene chloride and 0.3-0.8 parts of yttrium oxide, and at least two of 1-5 parts of calcium chloride, 1-3 parts of yttrium chloride and 0.5-2 parts of vanadium pentoxide; further preferably, the additives, by weight, include 0.2-0.6 parts of graphene oxide, 0.2-0.5 parts of carbon nanotubes, 0.1-0.3 parts of fullerene chloride and 0.3-0.6 parts of yttrium oxide, and at least two of 2-5 parts of calcium chloride, 2-3 parts of yttrium chloride and 1-2 parts of vanadium pentoxide. According to the additive composition of this component, when added in a small amount, the ceramic plate prepared from the above ceramic components (20 parts of potassium feldspar, 12-20 parts of sodium feldspar, 3-8 parts of kaolin, 6-12 parts of bentonite, 15-30 parts of illite, and 1-3 parts of zirconium oxide) can have good bending strength. This also reduces the amount of additives added. If the amount of additives added is too much, it is not conducive to improving the dispersion uniformity, and thus is not conducive to improving the bending strength of the ceramic plate.

[0012] Preferably, the solvent includes water, glycerol and chloroform. The solvent composed of these components helps to better disperse the additive and other components.

[0013] Preferably, in the solvent, the volume ratio of water, glycerol and chloroform is 10:(0.1-2):(0.1-0.8), and more preferably 10:(0.5-1.5):(0.1-0.5).

[0014] Preferably, the fullerene chloride is selected from C 60 Cl6、C 60 Cl 12 , C60 Cl 18 At least one of .

[0015] Preferably, the sintering process is: heating to 800-950°C at a rate of 15-20°C / min, keeping the temperature for 20-40 minutes, then heating to 1150-1250°C at a rate of 5-10°C / min, keeping the temperature for 20-40 minutes.

[0016] Preferably, when the additive is added, 0.1-0.3 parts of ytterbium oxide is also added. Ytterbium oxide, combined with the above components, has the effect of improving the bending strength of the ceramic plate.

[0017] Preferably, before the sintering, the process further includes applying a glaze, a decorative pattern and a protective glaze on the surface of the green body.

[0018] Preferably, the sintering further includes a cooling process.

[0019] Preferably, during the cooling process, the temperature is first cooled to 600-700°C at a rate of 6-12°C / min, and then cooled to room temperature at a rate of 3-5°C / min. At this specific staged cooling rate, the internal stress of the ceramic plate is released, which helps to improve the bending strength of the ceramic plate.

[0020] Preferably, a method for preparing a bending-resistant ceramic plate comprises the following steps:

[0021] By weight ratio, 20 parts of potassium feldspar, 12-20 parts of sodium feldspar, 3-8 parts of kaolin, 6-12 parts of bentonite, 15-30 parts of illite, 0.1-1 part of zirconium oxide, and 30-70 parts of solvent are mixed, 0.5-3 parts of additives are added, and the mixture is stirred and dispersed to obtain a slurry, and then spray granulation is performed to obtain a blank, and then press molding is performed to obtain a green body, and sintering is performed to obtain the ceramic plate;

[0022] The additives include, by weight, 0.2-0.8 parts of graphene oxide, 0.1-0.5 parts of carbon nanotubes, 0.1-0.3 parts of fullerene chloride, 0.3-0.8 parts of yttrium oxide, and at least two of 1-5 parts of calcium chloride, 1-3 parts of yttrium chloride, and 0.5-2 parts of vanadium pentoxide;

[0023] The solvent includes water, glycerol and chloroform, and in the solvent, the volume ratio of water, glycerol and chloroform is 10: (0.1-2): (0.1-0.8).

[0024] Preferably, the bending strength of the ceramic plate of the present invention exceeds 150 MPa, for example, 153-165 MPa.

[0025] Preferably, the thickness of the ceramic plate of the present invention is 5-15 mm, for example, 8-15 mm.

[0026] Preferably, the ceramic plate of the present invention has a length of 800-3000 mm and a width of 400-1000 mm.

[0027] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0028] (1) The ceramic plate of the present invention is introduced with additives by combining specific ceramic components (20 parts of potassium feldspar, 12-20 parts of sodium feldspar, 3-8 parts of kaolin, 6-12 parts of bentonite, 15-30 parts of illite, and 1-3 parts of zirconium oxide), wherein the additives include graphene oxide, carbon nanotubes, fullerene chloride and yttrium oxide, and at least two of calcium chloride, yttrium chloride, and vanadium pentoxide, wherein graphene oxide, carbon nanotubes, and fullerene chloride are mutually dispersed to form a spatial network structure, and yttrium oxide is uniformly dispersed in the network structure. Further, in the combination of at least two of calcium chloride, yttrium chloride, and vanadium pentoxide, it is helpful to improve the dispersion uniformity of the additives and the specific ceramic components, and improve the toughness of the ceramic plate finally obtained, thereby also improving the bending strength of the ceramic plate. The ceramic plate of the present invention has good toughness, and its corresponding bending strength exceeds 150MPa, for example, 153-165MPa, which is very beneficial to the application of the ceramic plate.

[0029] (2) When adding the additives, 0.1-0.3 parts of ytterbium oxide are also added. Ytterbium oxide, combined with the above components, has the effect of improving the bending strength of the ceramic plate.

[0030] (3) Through the temperature increase process during the sintering process of the present invention, the compatibility of the additive of the present invention with the specific ceramic component is further improved, which is beneficial to the improvement of the bending strength of the ceramic plate. During the cooling process, it is first cooled to 600-700°C at a rate of 6-12°C / minute, and then cooled to room temperature at a rate of 3-5°C / minute. At this specific staged cooling rate, it is helpful to release the internal stress of the ceramic plate and help improve the bending strength of the ceramic plate. DETAILED DESCRIPTION

[0031] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.

[0032] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0033] The particles of potassium feldspar, sodium feldspar, kaolin, bentonite, illite, zirconium oxide, yttrium oxide, yttrium chloride and vanadium pentoxide used below can all pass through a 150-200 mesh sieve.

[0034] Example 1

[0035] A method for preparing a bending-resistant ceramic plate comprises the following steps:

[0036] According to the weight ratio, 20 parts of potassium feldspar, 15 parts of sodium feldspar, 6 parts of kaolin, 10 parts of bentonite, 20 parts of illite, 0.4 parts of zirconium oxide, and 50 parts of solvent (the solvent is composed of water, glycerol and chloroform in a volume ratio of 10:1:0.5) are mixed, 1 part of additive is added, and the mixture is stirred and dispersed at 900 rpm for 40 minutes to obtain a slurry, and then spray granulation is performed to obtain a blank, and then press molding is performed (spray granulation and press molding belong to conventional processes in the field) to obtain a green body, sintering, and then cooling to obtain a ceramic plate;

[0037] The additives are composed of the following components by weight: 0.3 parts of graphene oxide, 0.2 parts of carbon nanotubes, and fullerene chloride (C 60 Cl6) 0.1 part and yttrium oxide 0.4 part, as well as yttrium chloride 1 part, vanadium pentoxide 0.7 part;

[0038] The sintering process is as follows: heating to 900°C at a rate of 15°C / min and keeping the temperature for 30 minutes, then heating to 1150°C at a rate of 5°C / min and keeping the temperature for 40 minutes.

[0039] During the cooling process, the temperature was first cooled to 700° C. at a rate of 10° C. / min, and then cooled to room temperature at a rate of 5° C. / min.

[0040] Example 2

[0041] A method for preparing a bending-resistant ceramic plate comprises the following steps:

[0042] By weight, 20 parts of potassium feldspar, 18 parts of sodium feldspar, 8 parts of kaolin, 12 parts of bentonite, 18 parts of illite, 0.3 parts of zirconium oxide, and 55 parts of solvent (the solvent is composed of water, glycerol and chloroform in a volume ratio of 10:1.5:0.5) are mixed, 1.5 parts of additives are added, and the mixture is stirred and dispersed at 1000 rpm for 30 minutes to obtain a slurry, and then spray granulation is performed to obtain a blank, and then press molding is performed (spray granulation and press molding belong to conventional processes in the field) to obtain a green body, sintering, and then cooling to obtain a ceramic plate;

[0043] The additives are composed of the following components by weight: 0.4 parts of graphene oxide, 0.3 parts of carbon nanotubes, and fullerene chloride (C 60 Cl12 ) 0.15 parts and yttrium oxide 0.5 parts, as well as calcium chloride 2 parts, vanadium pentoxide 0.6 parts;

[0044] The sintering process is as follows: heating to 950°C at a rate of 16°C / min and keeping the temperature for 30 minutes, then heating to 1180°C at a rate of 6°C / min and keeping the temperature for 40 minutes.

[0045] During the cooling process, the temperature was first cooled to 600° C. at a rate of 8° C. / min, and then cooled to room temperature at a rate of 4° C. / min.

[0046] Example 3

[0047] A method for preparing a bending-resistant ceramic plate comprises the following steps:

[0048] According to the weight ratio, 20 parts of potassium feldspar, 15 parts of sodium feldspar, 6 parts of kaolin, 10 parts of bentonite, 20 parts of illite, 0.4 parts of zirconium oxide, and 50 parts of solvent (the solvent is composed of water, glycerol and chloroform in a volume ratio of 10:1:0.5) are mixed, 1 part of additive and 0.2 parts of ytterbium oxide are added, and the mixture is stirred and dispersed at 900 rpm for 40 minutes to obtain a slurry, and then spray granulation is performed to obtain a blank, and then press molding is performed (spray granulation and press molding belong to conventional processes in the field) to obtain a green body, sintering, and then cooling to obtain a ceramic plate;

[0049] The additives are composed of the following components by weight: 0.3 parts of graphene oxide, 0.2 parts of carbon nanotubes, and fullerene chloride (C 60 Cl6) 0.1 part and yttrium oxide 0.4 part, as well as yttrium chloride 1 part, vanadium pentoxide 0.7 part;

[0050] The sintering process is as follows: heating to 900°C at a rate of 15°C / min and keeping the temperature for 30 minutes, then heating to 1150°C at a rate of 5°C / min and keeping the temperature for 40 minutes.

[0051] During the cooling process, the temperature was first cooled to 700° C. at a rate of 10° C. / min, and then cooled to room temperature at a rate of 5° C. / min.

[0052] Example 4

[0053] A method for preparing a bending-resistant ceramic plate comprises the following steps:

[0054] According to the weight ratio, 20 parts of potassium feldspar, 15 parts of sodium feldspar, 6 parts of kaolin, 10 parts of bentonite, 20 parts of illite, 0.4 parts of zirconium oxide, and 50 parts of solvent (the solvent is composed of water and glycerol in a volume ratio of 10:1) are mixed, 1 part of additive is added, and the mixture is stirred and dispersed at 900 rpm for 40 minutes to obtain a slurry, and then spray granulation is performed to obtain a blank, and then press molding is performed (spray granulation and press molding belong to conventional processes in the field) to obtain a green body, sintering, and then cooling to obtain a ceramic plate;

[0055] The additives are composed of the following components by weight: 0.3 parts of graphene oxide, 0.2 parts of carbon nanotubes, and fullerene chloride (C 60 Cl6) 0.1 part and yttrium oxide 0.4 part, as well as yttrium chloride 1 part, vanadium pentoxide 0.7 part;

[0056] The sintering process is as follows: heating to 1150°C at a rate of 15°C / min and keeping the temperature for 70 minutes.

[0057] The cooling process is to cool naturally to room temperature.

[0058] Comparative Example 1

[0059] Compared with Example 1, the difference of Comparative Example 1 is that an equal amount of C 60 Replace fullerene chloride (C 60 C16), the rest of the process is the same as in Example 1, and the specific contents of Comparative Example 1 are as follows:

[0060] A method for preparing a bending-resistant ceramic plate comprises the following steps:

[0061] According to the weight ratio, 20 parts of potassium feldspar, 15 parts of sodium feldspar, 6 parts of kaolin, 10 parts of bentonite, 20 parts of illite, 0.4 parts of zirconium oxide, and 50 parts of solvent (the solvent is composed of water, glycerol and chloroform in a volume ratio of 10:1:0.5) are mixed, 1 part of additive is added, and the mixture is stirred and dispersed at 900 rpm for 40 minutes to obtain a slurry, and then spray granulation is performed to obtain a blank, and then press molding is performed (spray granulation and press molding belong to conventional processes in the field) to obtain a green body, sintering, and then cooling to obtain a ceramic plate;

[0062] The additives are composed of the following components by weight: 0.3 parts of graphene oxide, 0.2 parts of carbon nanotubes, and 0.5 parts of fullerene (C 60 ) 0.1 part and yttrium oxide 0.4 part, and yttrium chloride 1 part, vanadium pentoxide 0.7 part;

[0063] The sintering process is as follows: heating to 900°C at a rate of 15°C / min and keeping the temperature for 30 minutes, then heating to 1150°C at a rate of 5°C / min and keeping the temperature for 40 minutes.

[0064] During the cooling process, the temperature was first cooled to 700° C. at a rate of 10° C. / min, and then cooled to room temperature at a rate of 5° C. / min.

[0065] Comparative Example 2

[0066] Compared with Example 1, the difference of Comparative Example 2 is that an equal amount of yttrium oxide is used instead of vanadium pentoxide, and the rest of the process is the same as that of Example 1. The specific contents of Comparative Example 2 are as follows:

[0067] A method for preparing a bending-resistant ceramic plate comprises the following steps:

[0068] According to the weight ratio, 20 parts of potassium feldspar, 15 parts of sodium feldspar, 6 parts of kaolin, 10 parts of bentonite, 20 parts of illite, 0.4 parts of zirconium oxide, and 50 parts of solvent (the solvent is composed of water, glycerol and chloroform in a volume ratio of 10:1:0.5) are mixed, 1 part of additive is added, and the mixture is stirred and dispersed at 900 rpm for 40 minutes to obtain a slurry, and then spray granulation is performed to obtain a blank, and then press molding is performed (spray granulation and press molding belong to conventional processes in the field) to obtain a green body, sintering, and then cooling to obtain a ceramic plate;

[0069] The additives are composed of the following components by weight: 0.3 parts of graphene oxide, 0.2 parts of carbon nanotubes, and fullerene chloride (C 60 Cl6) 0.1 parts and yttrium oxide 1.1 parts, and yttrium chloride 1 part;

[0070] The sintering process is as follows: heating to 900°C at a rate of 15°C / min and keeping the temperature for 30 minutes, then heating to 1150°C at a rate of 5°C / min and keeping the temperature for 40 minutes.

[0071] During the cooling process, the temperature was first cooled to 700° C. at a rate of 10° C. / min, and then cooled to room temperature at a rate of 5° C. / min.

[0072] Comparative Example 3

[0073] Compared with Example 1, the difference of Comparative Example 3 is that an equal amount of bentonite is used instead of illite, and the rest of the process is the same as that of Example 1. The specific contents of Comparative Example 3 are as follows:

[0074] A method for preparing a bending-resistant ceramic plate comprises the following steps:

[0075] According to the weight ratio, 20 parts of potassium feldspar, 15 parts of sodium feldspar, 6 parts of kaolin, 30 parts of bentonite, 0.4 parts of zirconium oxide, and 50 parts of solvent (the solvent is composed of water, glycerol and chloroform in a volume ratio of 10:1:0.5) are mixed, 1 part of additive is added, and the mixture is stirred and dispersed at 900 rpm for 40 minutes to obtain a slurry, and then spray granulation is performed to obtain a blank, and then press molding is performed (spray granulation and press molding belong to conventional processes in the field) to obtain a green body, sintering, and then cooling to obtain a ceramic plate;

[0076] The additives are composed of the following components by weight: 0.3 parts of graphene oxide, 0.2 parts of carbon nanotubes, and fullerene chloride (C 60 Cl6) 0.1 part and yttrium oxide 0.4 part, as well as yttrium chloride 1 part, vanadium pentoxide 0.7 part;

[0077] The sintering process is as follows: heating to 900°C at a rate of 15°C / min and keeping the temperature for 30 minutes, then heating to 1150°C at a rate of 5°C / min and keeping the temperature for 40 minutes.

[0078] During the cooling process, the temperature was first cooled to 700° C. at a rate of 10° C. / min, and then cooled to room temperature at a rate of 5° C. / min.

[0079] Product effect testing

[0080] The ceramic plates prepared in Examples 1-4 and Comparative Examples 1-3 were taken and the bending strength of the ceramic plates was tested using GBT 6569-2006 “Test method for bending strength of fine ceramics”. The results are shown in Table 1.

[0081] Table 1

[0082] Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Bending strength (MPa) 153.1 153.7 162.0 151.4 149.8 148.3 148.9

[0083] It can be seen from Table 1 that the bending strength of the ceramic plate prepared in the embodiment of the present invention is significantly better than the bending strength of the ceramic plates of Comparative Examples 1-3.

Claims

1. A method for preparing a bending-resistant ceramic plate, It is characterized in that The following steps are involved: Mix 20 parts of potassium feldspar, 12-20 parts of sodium feldspar, 3-8 parts of kaolin, 6-12 parts of bentonite, 15-30 parts of illite, 0.1-1 part of zirconium oxide, and 30-70 parts of solvent by weight, add 0.5-3 parts of additives, stir and disperse to obtain slurry, then spray granulate to obtain blank, then press and shape to obtain green body, sinter to obtain the ceramic plate; The additives include graphene oxide, carbon nanotubes, fullerene chloride and yttrium oxide, and at least two of calcium chloride, yttrium chloride and vanadium pentoxide; When adding the additive, 0.1-0.3 parts of ytterbium oxide are also added; The sintering process is: heating to 800-950°C at a rate of 15-20°C / min, keeping warm for 20-40 minutes, then heating to 1150-1250°C at a rate of 5-10°C / min, keeping warm for 20-40 minutes; The sintering process also includes a cooling process. In the cooling process, the material is first cooled to 600-700° C. at a rate of 6-12° C. / minute, and then cooled to room temperature at a rate of 3-5° C. / minute.

2. The preparation method according to claim 1, It is characterized in that By weight, 20 parts of potassium feldspar, 12-16 parts of sodium feldspar, 5-8 parts of kaolin, 7-12 parts of bentonite, 15-25 parts of illite, 0.5-0.8 parts of zirconium oxide, and 40-60 parts of solvent are mixed, and 1-2 parts of additives and 0.1-0.3 parts of ytterbium oxide are added, and the mixture is stirred and dispersed to obtain a slurry.

3. The preparation method according to claim 1, It is characterized in that The additives include, by weight, 0.2-0.8 parts of graphene oxide, 0.1-0.5 parts of carbon nanotubes, 0.1-0.3 parts of fullerene chloride, 0.3-0.8 parts of yttrium oxide, and at least two of 1-5 parts of calcium chloride, 1-3 parts of yttrium chloride, and 0.5-2 parts of vanadium pentoxide.

4. The preparation method according to claim 1, It is characterized in that The solvents include water, glycerol and chloroform.

5. The preparation method according to claim 1, It is characterized in that The fullerene chloride is selected from C 60 Cl 6 , C 60 Cl 12 , C 60 Cl 18 At least one of .

6. The preparation method according to any one of claims 1 to 5, It is characterized in that The bending strength of the ceramic plate exceeds 150 MPa.