An armored butterfly optical cable

Through the combination of modified carbon fiber cloth and reinforced fiber, the armored butterfly optical cable armored layer is solved, and the armored layer with high mechanical strength and low attenuation rate is achieved, which improves the armored layer with high mechanical strength and low attenuation rate. Overall performance of optical cables.

CN118671903BActive Publication Date: 2024-11-08ZHEJIANG DONGTONG OPTICAL NETWORK & IOT TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411173679.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-08
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

The armored layer of the existing armored butterfly optical cable is easily damaged by lightning strikes due to the conductive material and is prone to metal fatigue, which affects the normal communication of the optical cable and is insufficient in bending resistance.

Method used

Using modified carbon fiber cloth as the armor layer, through the combination of carbon fiber surface modification and MXene material, combined with epoxy resin and polyethylene glycol and other materials, an armor layer with excellent mechanical strength and bending resistance is prepared, and the armor layer with protection is provided. Reinforcement fibers are added to the sleeve to improve the overall performance of the optical cable.

Benefits of technology

The high mechanical strength and low attenuation rate of the armored layer are achieved, which reduces the risk of lightning strike damage, and improves the bending resistance of the optical cable, which is better than that of the metal armored layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118671903B_ABST
    Figure CN118671903B_ABST
Patent Text Reader

Abstract

The present invention provides an armored butterfly optical cable, comprising a protective sleeve, wherein an optical fiber and a reinforcing member are arranged in the protective sleeve, wherein the optical fiber is arranged in the middle of the protective sleeve, and the reinforcing member is arranged on both wings of the protective sleeve, and an armor layer is arranged on the surface of the optical fiber, wherein the armor layer is composited by modified carbon fiber cloth and polyimide film and is wound and wrapped on the surface of the optical fiber; reinforcing fibers are added in the protective sleeve, and the optical cable has excellent mechanical strength and bending resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of communication optical cable manufacturing, and in particular relates to an armored butterfly optical cable. Background Art

[0002] With the rapid development of optical communication networks and the continuous increase in broadband services, people's requirements for information transmission are getting higher and higher. Operators' demand for network transmission capacity is constantly increasing. Optical cables have good protection performance. The armored layer of armored butterfly optical cables is generally composed of steel structures, so the armored layer is conductive. In the event of lightning strikes, the current can easily damage the cable and easily cause metal fatigue, affecting the normal communication of the optical cable. Summary of the invention

[0003] The present invention provides an armored butterfly optical cable, wherein the armor layer is composited by modified carbon fiber cloth and polyimide film, has excellent insulation performance, and has good bending resistance, and reinforcing fiber is added in the protective sheath, and the optical cable has excellent mechanical strength and low-attenuation bending resistance.

[0004] The present invention provides an armored butterfly optical cable, comprising a protective sleeve 1, wherein an optical fiber 2 and a reinforcing member 4 are arranged in the protective sleeve 1, an armor layer 3 is arranged on the surface of the optical fiber 2, the optical fiber 2 is arranged in the middle of the protective sleeve 1, and reinforcing members 4 are arranged on both sides of the optical fiber 2, the armor layer 3 is composited by modified carbon fiber cloth and polyimide film, and is wound and wrapped on the surface of the optical fiber 2; reinforcing fibers are added in the protective sleeve 1, and the optical cable has excellent mechanical strength and bending resistance.

[0005] The specific plan is as follows:

[0006] An armored butterfly optical cable comprises a protective sleeve, an optical fiber, an armor layer and a reinforcing member. The optical fiber and the reinforcing member are arranged in the protective sleeve, the optical fiber is arranged in the middle of the protective sleeve, the reinforcing member is on the two wings of the protective sleeve, and the armor layer is arranged on the surface of the optical fiber. The armor layer is prepared by the following method:

[0007] (1) Immersing the carbon fiber in a potassium permanganate solution, performing a closed hydrothermal reaction to deposit manganese dioxide on the surface of the carbon fiber, washing with water, drying, placing in N-methylpyrrolidone, adding polyetherimide (PEI), mixing evenly, impregnating, and then transferring to an ice water bath for standing, washing with water, and drying to obtain a pretreated carbon fiber;

[0008] (2) dispersing the MXene material in N,N-dimethylformamide, adding 3-aminopropyltrimethoxysilane, and mixing uniformly to obtain a MXene solution; immersing the pretreated carbon fiber obtained in step (1) in the MXene solution, heating for a predetermined time, washing with water, and drying to obtain the modified carbon fiber;

[0009] (3) preparing a plurality of the modified carbon fibers into rovings and then weaving the rovings into carbon fiber cloth;

[0010] (4) adding epoxy resin, polyethylene glycol, 3-aminopropyltrimethoxysilane, 1-allylhydantoin, 2-azobisisoheptanenitrile, and sodium dodecylsulfonate to N,N-dimethylformamide, adjusting the Ph value to be neutral, obtaining an impregnation solution, immersing the carbon fiber cloth in the impregnation solution, washing with water, and drying to obtain a pretreated carbon fiber cloth;

[0011] (5) The polyimide film and the carbon fiber cloth are stacked and hot pressed to obtain the polyimide composite carbon fiber cloth, which is then wound on the surface of the optical fiber to obtain the armor layer.

[0012] Furthermore, the MXene material is prepared by the following method:

[0013] (1) Add Ti3AlC2 to a hydrofluoric acid solution and stir at 40-50°C, use hydrofluoric acid to etch away the Al layer, centrifuge, and wash with water;

[0014] (2) adding anhydrous ethanol, ultrasonicating for 1-2 hours, centrifuging, and washing with water to obtain the MXene material.

[0015] Further, the step 1 is to immerse the carbon fiber in a potassium permanganate solution with a mass fraction of 0.4-0.8%, heat it to 90-100°C for a closed hydrothermal reaction for 1-2h, wash it with water, dry it, put it in N-methylpyrrolidone and heat it to 70-80°C, add polyetherimide (PEI), the mass fraction of the polyetherimide in N-methylpyrrolidone is 0.1-0.4%, immerse it for 1-2h, then transfer it to an ice water bath and let it stand for 12-48h, wash it with water, and dry it to obtain a pretreated carbon fiber;

[0016] Furthermore, the step 2 is to disperse the MXene material in N,N-dimethylformamide, add 3-aminopropyltrimethoxysilane, and mix them evenly to obtain a MXene solution, wherein the mass fraction of the MXene material is 2-4%, and the mass fraction of 3-aminopropyltrimethoxysilane is 0.5-2%; the pretreated carbon fiber obtained in step (1) is placed in the MXene solution, stirred at 70-80° C. for 1-2 h, washed with water, and dried to obtain the modified carbon fiber;

[0017] Further, the step 4 is to add 40-50 parts of epoxy resin, 10-15 parts of polyethylene glycol, 5-8 parts of 3-aminopropyltrimethoxysilane, 4-6 parts of 1-allylhydantoin, 0.1-0.5 parts of 2-azobisisoheptanenitrile, and 0.1-0.3 parts of sodium dodecylsulfonate to 1000 parts of N,N-dimethylformamide, adjust the Ph value to neutral, obtain an impregnation solution, immerse the carbon fiber cloth in the impregnation solution for 1-2 hours, wash with water, and dry to obtain a pretreated carbon fiber cloth;

[0018] Furthermore, the protective sleeve comprises the following components by weight: 70-80 parts of polyethylene, 30-40 parts of EPDM rubber, 20-30 parts of polyamide, 20-25 parts of ethylene-vinyl acetate copolymer, 20-25 parts of reinforcing fiber, 2-5 parts of antioxidant, 4-6 parts of plasticizer, 2-4 parts of maleic anhydride grafted polyethylene, 3-6 parts of stearic acid, and 1-2 parts of polymethylvinylsiloxane; the reinforcing fiber is prepared by the following method:

[0019] The carbon nanofibers are added to a nitric acid aqueous solution, subjected to a hydrothermal reaction, filtered, washed, and dried to obtain activated carbon nanofibers; the activated carbon nanofibers are added to an ethanol solution of butyl titanate, acetic acid is added, subjected to a hydrothermal reaction, filtered, washed, dried, and heated for calcination; the calcined product is added to an N,N-dimethylformamide solvent with 1-butyl-3-methylimidazole bromide and polyethylene glycol, mixed evenly, azobisisobutyronitrile and stannous isooctanoate are added, stirred evenly, allowed to stand, subjected to a hydrothermal reaction, filtered, washed, and dried to obtain the method.

[0020] Furthermore, the reinforcing fiber is prepared by the following method:

[0021] 20g of carbon nanofibers with a diameter of 30-60 microns are added to 500ml of nitric acid aqueous solution with a concentration of 2-3mol / L, and after hydrothermal reaction at 70-80℃ for 6-10h, filtered, washed, and dried to obtain activated carbon nanofibers; 20g of activated carbon nanofibers are added to 500ml of ethanol solution of butyl titanate with a concentration of 2-4wt%, 10g of acetic acid is added, and hydrothermal reaction is carried out at 70-80℃ for 5-10h, filtered, washed, dried, and heated to 650-700℃ for calcination for 3-5h; 10g of the calcined product is taken, and added to 100ml with 5-10g of 1-butyl-3-methylimidazole bromide and 4-6g of polyethylene glycol. Mix evenly in N, N-dimethylformamide, add 1-2g of azobisisobutyronitrile and 1-2g of stannous isooctanoate, stir evenly and let stand for 10-60min, then carry out hydrothermal reaction at 70-90℃ for 3-6h, filter, wash and dry to obtain the product.

[0022] Furthermore, the plasticizer is selected from one or a combination of dioctyl phthalate, butyl benzyl phthalate, dicyclohexyl phthalate, dibutyl phthalate, diisobutyl phthalate, dimethyl phthalate, and diethyl phthalate.

[0023] Furthermore, the antioxidant is selected from one or more of antioxidant 1010, antioxidant 1790, antioxidant 245, antioxidant 168, antioxidant CA, antioxidant 264, and antioxidant 1076.

[0024] The present invention has the following beneficial effects:

[0025] Compared with the prior art, the beneficial effects of the present invention are:

[0026] 1) The surface of the carbon fiber is modified with manganese dioxide to increase the surface roughness of the carbon fiber, which can be more firmly combined with the MXene material. In addition, polyetherimide is added during the modification process, which can greatly improve the tensile, twisting and bending deformation performance of the carbon fiber, and is beneficial to the later plying and weaving when preparing the carbon fiber cloth. At the same time, after adding 3-aminopropyltrimethoxysilane, 1-allylhydantoin, 2-azobisisoheptanenitrile and sodium dodecylsulfonate to the sizing agent, the epoxy resin and polyethylene glycol are uniformly dispersed in the pores of the carbon fiber cloth. At the same time, the presence of 1-allylhydantoin and 2-azobisisoheptanenitrile components provides good bonding performance with the polyimide film, so that the polyimide film can enter the pores of the carbon fiber cloth during the hot pressing process, thereby improving the mechanical strength and bending resistance of the armor layer. Compared with the metal armor layer, the armor layer prepared by the present invention has a lower attenuation rate.

[0027] 2) The titanium dioxide particles on the surface of the carbon fiber form protrusions on the fiber surface, which can anchor the carbon fiber in the sheath and slow down the slippage of the carbon fiber in the sheath layer. The modified carbon fiber filler increases the mechanical strength of the sheath layer. After the titanium dioxide particles are deposited, a coating layer is formed on the surface of the carbon fiber by polyionic liquid 1-butyl-3-methylimidazole bromide and polyethylene glycol, thereby solidifying the titanium dioxide on the surface of the carbon fiber. The coating layer has a cross-linked structure and is firmly coated on the carbon surface and is not easy to fall off. The carbon nanofibers and titanium dioxide particles are fully coated by copolymerization and cross-linking of 1-butyl-3-methylimidazole bromide and polyethylene glycol, and the coating is relatively uniform. The imidazole group of the ionic liquid can improve the dispersion of the filler in the sheath, and the coating of polyethylene glycol can also improve the bending resistance of the sheath. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is a cross-sectional view of the optical cable of the present invention. DETAILED DESCRIPTION

[0029] The present invention is further described below in conjunction with specific implementation methods, but the protection scope of the present invention is not limited to the following embodiments. Any non-essential adjustments and modifications made to the present invention based on the above invention content still fall within the protection scope of the present invention.

[0030] The MXene material of the present invention is prepared by the following method:

[0031] Add Ti3AlC2 to a 2.5 mol / L hydrofluoric acid solution and stir at 50°C. Use hydrofluoric acid to etch away the Al layer, centrifuge, and wash with water. Add anhydrous ethanol, ultrasonicate for 2 hours, centrifuge, and wash with water to obtain a few-layer MXene material.

[0032] Example 1

[0033] The carbon fiber was immersed in a potassium permanganate solution with a mass fraction of 0.4%, heated to 100°C for a closed hydrothermal reaction for 2 hours, washed with water, dried, placed in N-methylpyrrolidone and heated to 70°C, polyetherimide (PEI) was added, the mass fraction of the polyetherimide in N-methylpyrrolidone was 0.1%, immersed for 2 hours, then transferred to an ice water bath and allowed to stand for 24 hours, washed with water, and dried to obtain pretreated carbon fiber; MXene material was dispersed in N,N-dimethylformamide, 3-aminopropyltrimethoxysilane was added, and mixed evenly to obtain a MXene solution, wherein the mass fraction of the MXene material was 2%, and the mass fraction of 3-aminopropyltrimethoxysilane was 0.5%; the pretreated carbon fiber was placed in the MXene solution, stirred at 70°C for 2 hours, washed with water, and dried to obtain modified carbon fiber; a plurality of the modified carbon fibers were made into rovings and woven into carbon fiber cloth, wherein the linear density of the coarse sand was 4000tex, and the gram weight of the fiber cloth was 400g•m -2 ; Add 40 parts of epoxy resin, 10 parts of polyethylene glycol, 5 parts of 3-aminopropyltrimethoxysilane, 4 parts of 1-allylhydantoin, 0.1 parts of 2-azobisisoheptanenitrile, and 0.1 parts of sodium dodecylsulfonate to 1000 parts of N,N-dimethylformamide, adjust the Ph value to neutral, and obtain an impregnation solution. Immerse the carbon fiber cloth in the impregnation solution for 1 hour, wash with water, and dry to obtain a pretreated carbon fiber cloth; sandwich the pretreated carbon fiber cloth between two polyimide films, heat to 130°C, and pressurize to 8Mpa at the same time, and maintain the pressure for 0.5 hours; obtain a polyimide composite carbon fiber cloth;

[0034] 20g of carbon nanofibers with a diameter of 40 microns were added to 500ml of 2mol / L nitric acid aqueous solution, and after hydrothermal reaction at 70°C for 10h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers; 20g of activated carbon nanofibers were added to 500ml of 2wt% butyl titanate ethanol solution, 10g of acetic acid was added, hydrothermal reaction was carried out at 70°C for 5h, filtered, washed with deionized water, dried at 80°C, and placed in a tube furnace and heated to 650°C for calcination for 3h; 10g of the product was taken, and 5g of 1-butyl-3-methylimidazole bromide and 4g of polyethylene glycol were added to 100ml of N, N-dimethylformamide and mixed evenly, 1g of azobisisobutyronitrile and 1g of stannous isooctanoate were added, stirred evenly and allowed to stand for 10min, followed by hydrothermal reaction at 70°C for 6h, filtered, washed with deionized water, and dried at 80°C to obtain reinforced fibers;

[0035] The polyimide composite carbon fiber cloth is wound on the surface of the optical fiber, i.e., the armor layer; 70 parts of polyethylene, 30 parts of EPDM rubber, 20 parts of polyamide, 20 parts of ethylene-vinyl acetate copolymer, 20 parts of reinforcing fiber, 2 parts of antioxidant 1010, 4 parts of plasticizer dioctyl phthalate, 2 parts of maleic anhydride grafted polyethylene, 3 parts of stearic acid, and 1 part of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled, and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber 2 and the reinforcing member 3 coated with the armor layer through a screw extruder, wherein the optical fiber 2 is located at the center of the butterfly sheath 1, and the reinforcing member 3 is on both wings of the butterfly sheath 1, to obtain the butterfly optical cable.

[0036] Example 2

[0037] The carbon fiber was immersed in a potassium permanganate solution with a mass fraction of 0.8%, heated to 100°C for a closed hydrothermal reaction for 1 hour, washed with water, dried, placed in N-methylpyrrolidone and heated to 80°C, polyetherimide (PEI) was added, the mass fraction of the polyetherimide in N-methylpyrrolidone was 0.4%, immersed for 1 hour, then transferred to an ice water bath and allowed to stand for 24 hours, washed with water, and dried to obtain pretreated carbon fiber; MXene material was dispersed in N,N-dimethylformamide, 3-aminopropyltrimethoxysilane was added, and mixed evenly to obtain a MXene solution, wherein the mass fraction of the MXene material was 4%, and the mass fraction of 3-aminopropyltrimethoxysilane was 2%; the pretreated carbon fiber was placed in the MXene solution, stirred at 70°C for 1 hour, washed with water, and dried to obtain modified carbon fiber; a plurality of the modified carbon fibers were made into rovings and then woven into carbon fiber cloth, wherein the linear density of the coarse sand was 4000tex, and the gram weight of the fiber cloth was 400g•m -2; Add 50 parts of epoxy resin, 12 parts of polyethylene glycol, 8 parts of 3-aminopropyltrimethoxysilane, 6 parts of 1-allylhydantoin, 0.5 parts of 2-azobisisoheptanenitrile, and 0.3 parts of sodium dodecylsulfonate to 1000 parts of N,N-dimethylformamide, adjust the Ph value to neutral, and obtain an impregnation solution. Immerse the carbon fiber cloth in the impregnation solution for 2 hours, wash with water, and dry to obtain a pretreated carbon fiber cloth; sandwich the pretreated carbon fiber cloth between two polyimide films, heat to 150°C, and pressurize to 6Mpa at the same time, and maintain the pressure for 1 hour; obtain a polyimide composite carbon fiber cloth;

[0038] 20g of carbon nanofibers with a diameter of 40 microns were added to 500ml of 3mol / L nitric acid aqueous solution, and after hydrothermal reaction at 80°C for 6h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers; 20g of activated carbon nanofibers were added to 500ml of 4wt% butyl titanate ethanol solution, 10g of acetic acid was added, hydrothermal reaction was carried out at 80°C for 5h, filtered, washed with deionized water, dried at 80°C, and placed in a tube furnace and heated to 700°C for calcination for 3h; 10g of the product was taken, added with 10g of 1-butyl-3-methylimidazole bromide and 6g of polyethylene glycol to 100ml of N,N-dimethylformamide and mixed evenly, 2g of azobisisobutyronitrile and 2g of stannous isooctanoate were added, stirred evenly and allowed to stand for 60min, then hydrothermally reacted at 90°C for 3h, filtered, washed with deionized water, and dried at 80°C to obtain reinforced fibers.

[0039] The polyimide composite carbon fiber cloth is wound on the surface of the optical fiber, i.e., the armor layer; 80 parts of polyethylene, 40 parts of EPDM rubber, 30 parts of polyamide, 25 parts of ethylene-vinyl acetate copolymer, 25 parts of reinforcing fiber, 5 parts of antioxidant 1010, 6 parts of plasticizer dioctyl phthalate, 4 parts of maleic anhydride grafted polyethylene, 6 parts of stearic acid, and 2 parts of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled, and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber 2 and the reinforcing member 3 coated with the armor layer through a screw extruder, wherein the optical fiber 2 is located at the center of the butterfly sheath 1, and the reinforcing member 3 is on both wings of the butterfly sheath 1, to obtain the butterfly optical cable.

[0040] Example 3

[0041] The carbon fiber was immersed in a potassium permanganate solution with a mass fraction of 0.5%, heated to 95°C for a closed hydrothermal reaction for 1.5 hours, washed with water, dried, placed in N-methylpyrrolidone and heated to 75°C, polyetherimide (PEI) was added, the mass fraction of the polyetherimide in N-methylpyrrolidone was 0.2%, immersed for 2 hours, then transferred to an ice water bath and allowed to stand for 24 hours, washed with water, and dried to obtain pretreated carbon fiber; MXene material was dispersed in N,N-dimethylformamide, 3-aminopropyltrimethoxysilane was added, and mixed evenly to obtain a MXene solution, wherein the mass fraction of the MXene material was 3%, and the mass fraction of 3-aminopropyltrimethoxysilane was 1%; the pretreated carbon fiber was placed in the MXene solution, stirred at 75°C for 2 hours, washed with water, and dried to obtain modified carbon fiber; a plurality of the modified carbon fibers were made into rovings and woven into carbon fiber cloth, wherein the linear density of the coarse sand was 4000tex, and the gram weight of the fiber cloth was 400g•m -2 ; Add 45 parts of epoxy resin, 12 parts of polyethylene glycol, 6 parts of 3-aminopropyltrimethoxysilane, 5 parts of 1-allylhydantoin, 0.2 parts of 2-azobisisoheptanenitrile, and 0.2 parts of sodium dodecylsulfonate to 1000 parts of N,N-dimethylformamide, adjust the Ph value to neutral, and obtain an impregnation solution. Immerse the carbon fiber cloth in the impregnation solution for 2 hours, wash with water, and dry to obtain a pretreated carbon fiber cloth; sandwich the pretreated carbon fiber cloth between two polyimide films, heat to 140°C, and pressurize to 7Mpa at the same time, and maintain the pressure for 1 hour; obtain a polyimide composite carbon fiber cloth;

[0042] 20g of carbon nanofibers with a diameter of 40 microns were added to 500ml of 2.5mol / L nitric acid aqueous solution, and after hydrothermal reaction at 75°C for 8h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers; 20g of activated carbon nanofibers were added to 500ml of 3wt% butyl titanate ethanol solution, 10g of acetic acid was added, hydrothermal reaction was carried out at 75°C for 6h, filtered, washed with deionized water, dried at 80°C, and placed in a tubular furnace and heated to 670°C for calcination for 4h; 10g of the product was taken, added with 8g of 1-butyl-3-methylimidazole bromide and 5g of polyethylene glycol to 100ml of N,N-dimethylformamide and mixed evenly, 1.5g of azobisisobutyronitrile and 1.5g of stannous isooctanoate were added, stirred evenly and allowed to stand for 30min, then hydrothermally reacted at 80°C for 4h, filtered, washed with deionized water, and dried at 80°C to obtain reinforced fibers.

[0043] The polyimide composite carbon fiber cloth is wound on the surface of the optical fiber, i.e., the armor layer; 75 parts of polyethylene, 35 parts of EPDM rubber, 25 parts of polyamide, 22 parts of ethylene-vinyl acetate copolymer, 25 parts of reinforcing fiber, 3 parts of antioxidant 1010, 5 parts of plasticizer dioctyl phthalate, 3 parts of maleic anhydride grafted polyethylene, 4 parts of stearic acid, and 1 part of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled, and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber 2 and the reinforcing member 3 coated with the armor layer through a screw extruder, wherein the optical fiber 2 is located at the center of the butterfly sheath 1, and the reinforcing member 3 is on both wings of the butterfly sheath 1, to obtain the butterfly optical cable.

[0044] Example 4

[0045] The carbon fiber was immersed in a potassium permanganate solution with a mass fraction of 0.6%, heated to 90°C for a closed hydrothermal reaction for 2 hours, washed with water, dried, placed in N-methylpyrrolidone and heated to 75°C, polyetherimide (PEI) was added, the mass fraction of the polyetherimide in N-methylpyrrolidone was 0.3%, immersed for 1.5 hours, then transferred to an ice water bath for standing for 24 hours, washed with water, and dried to obtain pretreated carbon fiber; MXene material was dispersed in N,N-dimethylformamide, 3-aminopropyltrimethoxysilane was added, and mixed evenly to obtain a MXene solution, wherein the mass fraction of the MXene material was 3%, and the mass fraction of 3-aminopropyltrimethoxysilane was 1%; the pretreated carbon fiber was placed in the MXene solution, stirred at 75°C for 2 hours, washed with water, and dried to obtain modified carbon fiber; a plurality of the modified carbon fibers were made into rovings and woven into carbon fiber cloth, wherein the linear density of the coarse sand was 3000tex, and the gram weight of the fiber cloth was 400g•m -2 ; Add 45 parts of epoxy resin, 13 parts of polyethylene glycol, 7 parts of 3-aminopropyltrimethoxysilane, 5 parts of 1-allylhydantoin, 0.3 parts of 2-azobisisoheptanenitrile, and 0.3 parts of sodium dodecylsulfonate to 1000 parts of N,N-dimethylformamide, adjust the Ph value to neutral, and obtain an impregnation solution. Immerse the carbon fiber cloth in the impregnation solution for 2 hours, wash with water, and dry to obtain a pretreated carbon fiber cloth; sandwich the pretreated carbon fiber cloth between two polyimide films, heat to 140°C, and pressurize to 7Mpa at the same time, and maintain the pressure for 1 hour; obtain a polyimide composite carbon fiber cloth;

[0046] 20g of carbon nanofibers with a diameter of 40 microns were added to 500ml of 2.5mol / L nitric acid aqueous solution, and after hydrothermal reaction at 75°C for 8h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers; 20g of activated carbon nanofibers were added to 500ml of 3wt% butyl titanate ethanol solution, 10g of acetic acid was added, hydrothermal reaction was carried out at 75°C for 6h, filtered, washed with deionized water, dried at 80°C, and placed in a tubular furnace and heated to 670°C for calcination for 4h; 10g of the product was taken, added with 8g of 1-butyl-3-methylimidazole bromide and 5g of polyethylene glycol to 100ml of N,N-dimethylformamide and mixed evenly, 1.5g of azobisisobutyronitrile and 1.5g of stannous isooctanoate were added, stirred evenly and allowed to stand for 30min, then hydrothermally reacted at 80°C for 4h, filtered, washed with deionized water, and dried at 80°C to obtain reinforced fibers.

[0047] The polyimide composite carbon fiber cloth is wound on the surface of the optical fiber, i.e., the armor layer; 76 parts of polyethylene, 74 parts of EPDM rubber, 25 parts of polyamide, 24 parts of ethylene-vinyl acetate copolymer, 24 parts of reinforcing fiber, 4 parts of antioxidant 1010, 5 parts of plasticizer dioctyl phthalate, 3 parts of maleic anhydride grafted polyethylene, 5 parts of stearic acid, and 2 parts of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled, and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber 2 and the reinforcing member 3 coated with the armor layer through a screw extruder, wherein the optical fiber 2 is located at the center of the butterfly sheath 1, and the reinforcing member 3 is on both wings of the butterfly sheath 1, to obtain the butterfly optical cable.

[0048] Example 5

[0049] The carbon fiber was immersed in a potassium permanganate solution with a mass fraction of 0.7%, heated to 95°C for a closed hydrothermal reaction for 2 hours, washed with water, dried, placed in N-methylpyrrolidone and heated to 80°C, polyetherimide (PEI) was added, the mass fraction of the polyetherimide in N-methylpyrrolidone was 0.3%, immersed for 2 hours, then transferred to an ice water bath and allowed to stand for 24 hours, washed with water, and dried to obtain pretreated carbon fiber; MXene material was dispersed in N,N-dimethylformamide, 3-aminopropyltrimethoxysilane was added, and mixed evenly to obtain a MXene solution, wherein the mass fraction of the MXene material was 3%, and the mass fraction of 3-aminopropyltrimethoxysilane was 1.5%; the pretreated carbon fiber was placed in the MXene solution, stirred at 75°C for 2 hours, washed with water, and dried to obtain modified carbon fiber; a plurality of the modified carbon fibers were made into rovings and woven into carbon fiber cloth, wherein the linear density of the coarse sand was 4000tex, and the gram weight of the fiber cloth was 400g•m -2; Add 48 parts of epoxy resin, 14 parts of polyethylene glycol, 7 parts of 3-aminopropyltrimethoxysilane, 5 parts of 1-allylhydantoin, 0.4 parts of 2-azobisisoheptanenitrile, and 0.2 parts of sodium dodecylsulfonate to 1000 parts of N,N-dimethylformamide, adjust the Ph value to neutral, and obtain an impregnation solution. Immerse the carbon fiber cloth in the impregnation solution for 2 hours, wash with water, and dry to obtain a pretreated carbon fiber cloth; sandwich the pretreated carbon fiber cloth between two polyimide films, heat to 150°C, and pressurize to 8Mpa at the same time, and maintain the pressure for 1 hour; obtain a polyimide composite carbon fiber cloth;

[0050] 20g of carbon nanofibers with a diameter of 40 microns were added to 500ml of 2.5mol / L nitric acid aqueous solution, and after hydrothermal reaction at 75°C for 8h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers; 20g of activated carbon nanofibers were added to 500ml of 3wt% butyl titanate ethanol solution, 10g of acetic acid was added, hydrothermal reaction was carried out at 75°C for 6h, filtered, washed with deionized water, dried at 80°C, and placed in a tubular furnace and heated to 670°C for calcination for 4h; 10g of the product was taken, added with 8g of 1-butyl-3-methylimidazole bromide and 5g of polyethylene glycol to 100ml of N,N-dimethylformamide and mixed evenly, 1.5g of azobisisobutyronitrile and 1.5g of stannous isooctanoate were added, stirred evenly and allowed to stand for 30min, then hydrothermally reacted at 80°C for 4h, filtered, washed with deionized water, and dried at 80°C to obtain reinforced fibers.

[0051] The polyimide composite carbon fiber cloth is wound on the surface of the optical fiber, i.e., the armor layer; 75 parts of polyethylene, 38 parts of EPDM rubber, 26 parts of polyamide, 22 parts of ethylene-vinyl acetate copolymer, 25 parts of reinforcing fiber, 4 parts of antioxidant 1010, 5 parts of plasticizer dioctyl phthalate, 3 parts of maleic anhydride grafted polyethylene, 5 parts of stearic acid, and 2 parts of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled, and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber 2 and the reinforcing member 3 coated with the armor layer through a screw extruder, wherein the optical fiber 2 is located at the center of the butterfly sheath 1, and the reinforcing member 3 is on both wings of the butterfly sheath 1, to obtain the butterfly optical cable.

[0052] Comparative Example 1

[0053] A steel tape is wound on the surface of an optical fiber, i.e., an armor layer; 75 parts of polyethylene, 38 parts of EPDM rubber, 26 parts of polyamide, 22 parts of ethylene-vinyl acetate copolymer, 25 parts of the same reinforcing fiber as in Example 5, 4 parts of antioxidant 1010, 5 parts of plasticizer dioctyl phthalate, 3 parts of maleic anhydride grafted polyethylene, 5 parts of stearic acid, and 2 parts of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled, and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber 2 and the reinforcing member 3 coated with the armor layer through a screw extruder, wherein the optical fiber 2 is at the center of the butterfly sheath 1, and the reinforcing member 3 is on both wings of the butterfly sheath 1 to obtain the butterfly optical cable.

[0054] Comparative Example 2

[0055] A plurality of carbon fibers are made into rovings and then woven into carbon fiber cloth, wherein the linear density of the rovings is 4000 tex and the weight of the fiber cloth is 400 g·m -2 ; Two polyimide films are sandwiched around the carbon fiber cloth, heated to 150°C, and pressurized to 8Mpa for 1 hour; polyimide composite carbon fiber cloth is obtained;

[0056] The polyimide composite carbon fiber cloth is wound on the surface of the optical fiber, i.e., the armor layer, and 75 parts of polyethylene, 38 parts of EPDM rubber, 26 parts of polyamide, 22 parts of ethylene-vinyl acetate copolymer, 25 parts of the same reinforcing fiber as in Example 5, 4 parts of antioxidant 1010, 5 parts of plasticizer dioctyl phthalate, 3 parts of maleic anhydride grafted polyethylene, 5 parts of stearic acid, and 2 parts of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled, and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber 2 and the reinforcing member 3 coated with the armor layer through a screw extruder, wherein the optical fiber 2 is located at the center of the butterfly sheath 1, and the reinforcing member 3 is on both wings of the butterfly sheath 1 to obtain the butterfly optical cable.

[0057] Comparative Example 3

[0058] The MXene material is dispersed in N,N-dimethylformamide, 3-aminopropyltrimethoxysilane is added, and the mixture is uniformly mixed to obtain a MXene solution, wherein the mass fraction of the MXene material is 3%, and the mass fraction of the 3-aminopropyltrimethoxysilane is 1.5%; the carbon fiber is placed in the MXene solution, stirred at 75°C for 2 hours, washed with water, and dried to obtain the modified carbon fiber; a plurality of the modified carbon fibers are made into rovings and then woven into carbon fiber cloth, wherein the linear density of the rovings is 4000tex, and the gram weight of the fiber cloth is 400g•m -2; Add 48 parts of epoxy resin, 14 parts of polyethylene glycol, 7 parts of 3-aminopropyltrimethoxysilane, 5 parts of 1-allylhydantoin, 0.4 parts of 2-azobisisoheptanenitrile, and 0.2 parts of sodium dodecylsulfonate to 1000 parts of N,N-dimethylformamide, adjust the Ph value to neutral, and obtain an impregnation solution. Immerse the carbon fiber cloth in the impregnation solution for 2 hours, wash with water, and dry to obtain a pretreated carbon fiber cloth; sandwich the pretreated carbon fiber cloth between two polyimide films, heat to 150°C, and pressurize to 8Mpa at the same time, and maintain the pressure for 1 hour; obtain a polyimide composite carbon fiber cloth;

[0059] The polyimide composite carbon fiber cloth is wound on the surface of the optical fiber, i.e., the armor layer, and 75 parts of polyethylene, 38 parts of EPDM rubber, 26 parts of polyamide, 22 parts of ethylene-vinyl acetate copolymer, 25 parts of the same reinforcing fiber as in Example 5, 4 parts of antioxidant 1010, 5 parts of plasticizer dioctyl phthalate, 3 parts of maleic anhydride grafted polyethylene, 5 parts of stearic acid, and 2 parts of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled, and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber 2 and the reinforcing member 3 coated with the armor layer through a screw extruder, wherein the optical fiber 2 is located at the center of the butterfly sheath 1, and the reinforcing member 3 is on both wings of the butterfly sheath 1 to obtain the butterfly optical cable.

[0060] Comparative Example 4

[0061] The carbon fiber is immersed in a potassium permanganate solution with a mass fraction of 0.7%, heated to 95°C for a closed hydrothermal reaction for 2 hours, washed with water, dried, placed in N-methylpyrrolidone and heated to 80°C, polyetherimide (PEI) is added, and the mass fraction of the polyetherimide in N-methylpyrrolidone is 0.3%, immersed for 2 hours, and then transferred to an ice water bath for standing for 24 hours, washed with water, and dried to obtain a pretreated carbon fiber; a plurality of the pretreated carbon fibers are made into rovings and then woven into carbon fiber cloth, wherein the linear density of the rovings is 4000tex, and the gram weight of the fiber cloth is 400g•m -2 ; Add 48 parts of epoxy resin, 14 parts of polyethylene glycol, 7 parts of 3-aminopropyltrimethoxysilane, 5 parts of 1-allylhydantoin, 0.4 parts of 2-azobisisoheptanenitrile, and 0.2 parts of sodium dodecylsulfonate to 1000 parts of N,N-dimethylformamide, adjust the Ph value to neutral, and obtain an impregnation solution. Immerse the carbon fiber cloth in the impregnation solution for 2 hours, wash with water, and dry to obtain a pretreated carbon fiber cloth; sandwich the pretreated carbon fiber cloth between two polyimide films, heat to 150°C, and pressurize to 8Mpa at the same time, and maintain the pressure for 1 hour; obtain a polyimide composite carbon fiber cloth;

[0062] The polyimide composite carbon fiber cloth is wound on the surface of the optical fiber, i.e., the armor layer, and 75 parts of polyethylene, 38 parts of EPDM rubber, 26 parts of polyamide, 22 parts of ethylene-vinyl acetate copolymer, 25 parts of the same reinforcing fiber as in Example 5, 4 parts of antioxidant 1010, 5 parts of plasticizer dioctyl phthalate, 3 parts of maleic anhydride grafted polyethylene, 5 parts of stearic acid, and 2 parts of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled, and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber 2 and the reinforcing member 3 coated with the armor layer through a screw extruder, wherein the optical fiber 2 is located at the center of the butterfly sheath 1, and the reinforcing member 3 is on both wings of the butterfly sheath 1 to obtain the butterfly optical cable.

[0063] Comparative Example 5

[0064] The carbon fiber was immersed in a potassium permanganate solution with a mass fraction of 0.7%, heated to 95°C for a closed hydrothermal reaction for 2 hours, washed with water, dried, placed in N-methylpyrrolidone and heated to 80°C, polyetherimide (PEI) was added, the mass fraction of the polyetherimide in N-methylpyrrolidone was 0.3%, immersed for 2 hours, then transferred to an ice water bath and allowed to stand for 24 hours, washed with water, and dried to obtain pretreated carbon fiber; MXene material was dispersed in N,N-dimethylformamide, 3-aminopropyltrimethoxysilane was added, and mixed evenly to obtain a MXene solution, wherein the mass fraction of the MXene material was 3%, and the mass fraction of 3-aminopropyltrimethoxysilane was 1.5%; the pretreated carbon fiber was placed in the MXene solution, stirred at 75°C for 2 hours, washed with water, and dried to obtain modified carbon fiber; a plurality of the modified carbon fibers were made into rovings and woven into carbon fiber cloth, wherein the linear density of the coarse sand was 4000tex, and the gram weight of the fiber cloth was 400g•m -2 ; Two polyimide films are sandwiched around the carbon fiber cloth, heated to 150°C, and pressurized to 8Mpa for 1 hour; polyimide composite carbon fiber cloth is obtained;

[0065] The polyimide composite carbon fiber cloth is wound on the surface of the optical fiber, i.e., the armor layer, and 75 parts of polyethylene, 38 parts of EPDM rubber, 26 parts of polyamide, 22 parts of ethylene-vinyl acetate copolymer, 25 parts of the same reinforcing fiber as in Example 5, 4 parts of antioxidant 1010, 5 parts of plasticizer dioctyl phthalate, 3 parts of maleic anhydride grafted polyethylene, 5 parts of stearic acid, and 2 parts of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled, and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber 2 and the reinforcing member 3 coated with the armor layer through a screw extruder, wherein the optical fiber 2 is located at the center of the butterfly sheath 1, and the reinforcing member 3 is on both wings of the butterfly sheath 1 to obtain the butterfly optical cable.

[0066] Comparative Example 6

[0067] Use the same polyimide composite carbon fiber cloth as in Example 5;

[0068] The polyimide composite carbon fiber cloth is wound on the surface of the optical fiber, i.e., the armor layer; 75 parts of polyethylene, 38 parts of EPDM rubber, 26 parts of polyamide, 22 parts of ethylene-vinyl acetate copolymer, 4 parts of antioxidant 1010, 5 parts of plasticizer dioctyl phthalate, 3 parts of maleic anhydride grafted polyethylene, 5 parts of stearic acid, and 2 parts of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled, and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber 2 and the reinforcing member 3 coated with the armor layer through a screw extruder, wherein the optical fiber 2 is located at the center of the butterfly sheath 1, and the reinforcing member 3 is on both wings of the butterfly sheath 1, to obtain the butterfly optical cable.

[0069] Comparative Example 7

[0070] The same polyimide composite carbon fiber cloth as in Example 5 will be used;

[0071] 20 g of carbon nanofibers with a diameter of 40 microns were added to 500 ml of a 2.5 mol / L nitric acid aqueous solution, and the mixture was hydrothermally reacted at 75°C for 8 h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers. 10 g of the product was added to 100 ml of N,N-dimethylformamide with 8 g of 1-butyl-3-methylimidazole bromide and 5 g of polyethylene glycol, and mixed evenly. 1.5 g of azobisisobutyronitrile and 1.5 g of stannous isooctanoate were added, stirred evenly, and allowed to stand for 30 min. The mixture was then hydrothermally reacted at 80°C for 4 h, filtered, washed with deionized water, and dried at 80°C to obtain reinforced fibers.

[0072] The polyimide composite carbon fiber cloth is wound on the surface of the optical fiber, i.e., the armor layer; 75 parts of polyethylene, 38 parts of EPDM rubber, 26 parts of polyamide, 22 parts of ethylene-vinyl acetate copolymer, 25 parts of reinforcing fiber, 4 parts of antioxidant 1010, 5 parts of plasticizer dioctyl phthalate, 3 parts of maleic anhydride grafted polyethylene, 5 parts of stearic acid, and 2 parts of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled, and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber 2 and the reinforcing member 3 coated with the armor layer through a screw extruder, wherein the optical fiber 2 is located at the center of the butterfly sheath 1, and the reinforcing member 3 is on both wings of the butterfly sheath 1, to obtain the butterfly optical cable.

[0073] Comparative Example 8

[0074] Use the same polyimide composite carbon fiber cloth as in Example 5;

[0075] 20 g of carbon nanofibers with a diameter of 40 microns were added to 500 ml of a 2.5 mol / L nitric acid aqueous solution, and subjected to hydrothermal reaction at 75°C for 8 hours. The resultant reaction was filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers. 20 g of activated carbon nanofibers were added to 500 ml of a 3 wt% ethanol solution of butyl titanate, 10 g of acetic acid was added, and the resultant reaction was hydrothermally reacted at 75°C for 6 hours. The resultant reaction was filtered, washed with deionized water, and dried at 80°C. The resultant reaction was heated in a tubular furnace to 670°C and calcined for 4 hours to obtain reinforced fibers.

[0076] The polyimide composite carbon fiber cloth is wound on the surface of the optical fiber, i.e., the armor layer; 75 parts of polyethylene, 38 parts of EPDM rubber, 26 parts of polyamide, 22 parts of ethylene-vinyl acetate copolymer, 25 parts of reinforcing fiber, 4 parts of antioxidant 1010, 5 parts of plasticizer dioctyl phthalate, 3 parts of maleic anhydride grafted polyethylene, 5 parts of stearic acid, and 2 parts of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled, and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber 2 and the reinforcing member 3 coated with the armor layer through a screw extruder, wherein the optical fiber 2 is located at the center of the butterfly sheath 1, and the reinforcing member 3 is on both wings of the butterfly sheath 1, to obtain the butterfly optical cable.

[0077] Comparative Example 9

[0078] Use the same polyimide composite carbon fiber cloth as in Example 5;

[0079] 20g of carbon nanofibers with a diameter of 40 microns were added to 500ml of 2.5mol / L nitric acid aqueous solution, and after hydrothermal reaction at 75°C for 8h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers; 20g of activated carbon nanofibers were added to 500ml of 3wt% butyl titanate ethanol solution, 10g of acetic acid was added, hydrothermal reaction was carried out at 75°C for 6h, filtered, washed with deionized water, dried at 80°C, and heated to 670°C in a tubular furnace and calcined for 4h; 10g of the product was taken, added with 5g of polyethylene glycol to 100ml of N,N-dimethylformamide, mixed evenly, 1.5g of azobisisobutyronitrile and 1.5g of stannous isooctanoate were added, stirred evenly and allowed to stand for 30min, then hydrothermally reacted at 80°C for 4h, filtered, washed with deionized water, and dried at 80°C to obtain reinforced fibers.

[0080] The polyimide composite carbon fiber cloth is wound on the surface of the optical fiber, i.e., the armor layer; 75 parts of polyethylene, 38 parts of EPDM rubber, 26 parts of polyamide, 22 parts of ethylene-vinyl acetate copolymer, 25 parts of reinforcing fiber, 4 parts of antioxidant 1010, 5 parts of plasticizer dioctyl phthalate, 3 parts of maleic anhydride grafted polyethylene, 5 parts of stearic acid, and 2 parts of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled, and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber 2 and the reinforcing member 3 coated with the armor layer through a screw extruder, wherein the optical fiber 2 is located at the center of the butterfly sheath 1, and the reinforcing member 3 is on both wings of the butterfly sheath 1, to obtain the butterfly optical cable.

[0081] Experiments and Data

[0082] The tensile strength of the sheath material is tested according to the national standard GB / T2951.

[0083] According to YD / T1997.1-2022 "Introduction Optical Fiber Cable for Communication Part 1: Butterfly Optical Cable", the optical cable performance was tested and the repeated bending: residual additional attenuation was obtained.

[0084] The results are shown in Table 1.

[0085] Table 1

[0086]

[0087] Tests and Results

[0088] As can be seen from Table 1, Comparative Examples 1-5 use the same sheath material as Example 5, and the only difference is the preparation process of the armor layer. Therefore, the tensile strength is not measured, and only the bending attenuation performance is measured. Compared with Comparative Example 1, it can be seen that the armor layer of the present invention has higher bending resistance than the armor layer prepared by steel strip, and it can be seen from Comparative Example 2 that the untreated carbon fiber and the polyimide film can play a certain bending resistance after being compounded, but compared with the traditional steel strip armor layer, since the carbon fiber has not been pretreated, its attenuation rate is higher, and it can be seen from Comparative Examples 3-4 that different pretreatment processes for carbon fiber have an effect on the bending resistance, and Comparative Example 5 shows the effect of the impregnation liquid on the durability of the carbon fiber cloth; and Comparative Examples 6-9 are studies on the performance of the optical cable for the reinforced fibers in the sheath layer when the armor layer is the same as Example 5. It can be clearly seen from Comparative Example 6 that the addition of reinforced fibers has an effect on the mechanical strength and bending resistance of the sheath, and Comparative Examples 7-9 can show the effect of different reinforcement fiber processing processes on the final performance. Through the examples and comparative examples, it can be seen that in the armor layer, due to The surface of the carbon fiber is modified with manganese dioxide to increase the surface roughness of the carbon fiber, so that it can be more firmly combined with the MXene material. In addition, polyetherimide is added during the modification process, which can greatly improve the tensile, twisting and bending deformation performance of the carbon fiber, and is beneficial to the later plying and weaving when preparing the carbon fiber cloth. At the same time, after adding 3-aminopropyltrimethoxysilane, 1-allylhydantoin, 2-azobisisoheptanenitrile and sodium dodecylsulfonate to the sizing agent, the epoxy resin and polyethylene glycol are uniformly dispersed in the pores of the carbon fiber cloth. At the same time, the presence of 1-allylhydantoin and 2-azobisisoheptanenitrile components provides good bonding performance with the polyimide film, so that the polyimide film can enter the pores of the carbon fiber cloth during the hot pressing process, thereby improving the mechanical strength and bending resistance of the armor layer. Compared with the metal armor layer, the armor layer prepared by the present invention has a lower attenuation rate. In the sheath layer, the titanium dioxide particles on the surface of the carbon fiber used in the reinforced fiber form protrusions on the fiber surface, thereby enabling the carbon fiber to produce an anchoring effect in the sheath, slowing down the slippage of the carbon fiber in the sheath layer, and the modified carbon fiber filler increases the mechanical strength of the sheath layer. After the titanium dioxide particles are deposited, a coating layer is formed on the surface of the carbon fiber by polyionic liquid 1-butyl-3-methylimidazole bromide and polyethylene glycol, thereby solidifying the titanium dioxide on the surface of the carbon fiber, and the coating layer has a cross-linked structure, which is firmly coated on the carbon surface and is not easy to fall off. The carbon nanofibers and titanium dioxide particles are fully coated by copolymerization and cross-linking of 1-butyl-3-methylimidazole bromide and polyethylene glycol, and the coating is relatively uniform. The imidazole group of the ionic liquid can improve the dispersion of the filler in the sheath, and the coating of polyethylene glycol can also improve the bending resistance of the sheath.Although the content of the present invention has been described in detail through the above preferred embodiments, the above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. An armored butterfly optical cable, comprising a protective sleeve, an optical fiber, an armor layer and a reinforcing member, wherein the protective sleeve is provided with an optical fiber and a reinforcing member, wherein the optical fiber is provided in the middle of the protective sleeve, and the reinforcing member is provided on both wings of the protective sleeve, and an armor layer is provided on the surface of the optical fiber, wherein the armor layer is prepared by the following method: (1) Immersing the carbon fiber in a potassium permanganate solution with a mass fraction of 0.4-0.8%, heating to 90-100°C for a closed hydrothermal reaction for 1-2 hours, washing with water, drying, placing in N-methylpyrrolidone and heating to 70-80°C, adding polyetherimide PEI, wherein the mass fraction of the polyetherimide in N-methylpyrrolidone is 0.1-0.4%, immersing for 1-2 hours, then transferring to an ice water bath and standing for 12-48 hours, washing with water, and drying to obtain a pretreated carbon fiber; (2) Dispersing the MXene material in N,N-dimethylformamide, adding 3-aminopropyltrimethoxysilane, and mixing evenly to obtain a MXene solution, wherein the mass fraction of the MXene material is 2-4%, and the mass fraction of 3-aminopropyltrimethoxysilane is 0.5-2%; placing the pretreated carbon fiber obtained in step 1 in the MXene solution, stirring at 70-80°C for 1-2h, washing with water, and drying to obtain the modified carbon fiber; (3) preparing a plurality of the modified carbon fibers into rovings and then weaving the rovings into carbon fiber cloth; (4) Add 40-50 parts of epoxy resin, 10-15 parts of polyethylene glycol, 5-8 parts of 3-aminopropyltrimethoxysilane, 4-6 parts of 1-allylhydantoin, 0.1-0.5 parts of 2-azobisisoheptanenitrile, and 0.1-0.3 parts of sodium dodecylsulfonate to 1000 parts of N,N-dimethylformamide, adjust the Ph value to neutral, and obtain an impregnation solution. Immerse the carbon fiber cloth in the impregnation solution for 1-2 hours, wash with water, and dry to obtain a pretreated carbon fiber cloth. (5) The polyimide film and the carbon fiber cloth are stacked and hot pressed to obtain the polyimide composite carbon fiber cloth, which is then wound on the surface of the optical fiber to obtain the armor layer.

2. The armored butterfly optical cable according to claim 1, characterized in that: The MXene material is prepared by the following method: (1) Add Ti3AlC2 to a hydrofluoric acid solution and stir at 40-50°C, use hydrofluoric acid to etch away the Al layer, centrifuge, and wash with water; (2) adding anhydrous ethanol, ultrasonicating for 1-2 hours, centrifuging, and washing with water to obtain the MXene material.

3. The armored butterfly optical cable according to claim 1, characterized in that: The protective sleeve comprises the following components by weight: 70-80 parts of polyethylene, 30-40 parts of EPDM rubber, 20-30 parts of polyamide, 20-25 parts of ethylene-vinyl acetate copolymer, 20-25 parts of reinforcing fiber, 2-5 parts of antioxidant, 4-6 parts of plasticizer, 2-4 parts of maleic anhydride grafted polyethylene, 3-6 parts of stearic acid, and 1-2 parts of polymethylvinylsiloxane; the reinforcing fiber is prepared by the following method: The carbon nanofibers are added to a nitric acid aqueous solution, subjected to a hydrothermal reaction, filtered, washed, and dried to obtain activated carbon nanofibers; the activated carbon nanofibers are added to an ethanol solution of butyl titanate, acetic acid is added, subjected to a hydrothermal reaction, filtered, washed, dried, and heated for calcination; the calcined product is added to an N,N-dimethylformamide solvent with 1-butyl-3-methylimidazole bromide and polyethylene glycol, mixed evenly, azobisisobutyronitrile and stannous isooctanoate are added, stirred evenly, allowed to stand, subjected to a hydrothermal reaction, filtered, washed, and dried to obtain the method.

4. The armored butterfly optical cable according to claim 3, characterized in that: The plasticizer is selected from one or a combination of dioctyl phthalate, butyl benzyl phthalate, dicyclohexyl phthalate, dibutyl phthalate, diisobutyl phthalate, dimethyl phthalate, and diethyl phthalate.

5. The armored butterfly optical cable according to claim 3, characterized in that: The antioxidant is selected from one or more of antioxidant 1010, antioxidant 1790, antioxidant 245, antioxidant 168, antioxidant CA, antioxidant 264, and antioxidant 1076.

Citation Information

Patent Citations

  • MXene coated carbon fiber and preparation method thereof

    CN113652858A

  • MXene modified carbon fiber non-woven felt with multi-layer structure and preparation method of MXene modified carbon fiber non-woven felt

    CN117947633A

  • PEEK electromagnetic shielding material containing carbon fibers and preparation method of PEEK electromagnetic shielding material

    CN118344701A

  • Butterfly-shaped optical cable and production process thereof

    CN118444446A

  • Bending-insensitive butterfly cable and preparation method thereof

    CN118502046A