A highly weather-resistant colored aluminum pigment, preparation method thereof, and application in powder coatings

By forming a multi-layered cladding structure of silica, metal oxide and polymer resin on the surface of aluminum powder, the lack of performance of aluminum pigments in high acid and alkali resistance environments is solved, and the improvement of high weather resistance and colorful performance is achieved. .

CN118685056BActive Publication Date: 2024-12-06HEFEI SUNRISE PIGMENTS
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411157613.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-12-06
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The existing aluminum pigments lack performance when facing high acid and alkali resistance and weather resistance requirements, especially during high-speed mixing, the polymer layer is easily damaged, affecting the weather resistance and appearance effect of the coating film.

Method used

By sequentially covering the silica layer, metal oxide layer and polymer resin layer on the surface of the aluminum powder from the inside to the outside, the inorganic envelope improves corrosion resistance and color diversity, and forms a dense polymer resin through polymerization reaction. layer to improve adhesion and hiding.

Benefits of technology

It significantly improves the acid and alkali corrosion resistance and colorful properties of aluminum pigments, ensures the weather resistance and adhesion of aluminum powder, and meets customers' needs for weather resistance and colorfulness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118685056B_ABST
    Figure CN118685056B_ABST
Patent Text Reader

Abstract

The present invention discloses a highly weather-resistant colored aluminum pigment, a preparation method thereof, and an application thereof in a powder coating. The aluminum pigment comprises a flaky aluminum powder and a silicon dioxide layer, a metal oxide layer, and a polymer resin layer which sequentially coat the flaky aluminum powder from the inside to the outside. The present invention provides a highly weather-resistant colored aluminum pigment, a preparation method thereof, and an application thereof in a powder coating. After being coated with multiple layers, the aluminum pigment not only has excellent acid and alkali resistance and weather resistance, but also has diversified colors and high color concentration, thereby satisfying customers' simultaneous demands for weather resistance and multi-colorization of aluminum pigments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aluminum pigments, and in particular relates to a highly weather-resistant colored aluminum pigment, a preparation method thereof, and application in powder coatings. Background Art

[0002] At present, powder coatings have become the "4E" (high efficiency, energy saving, environmental protection, and economic) coatings that are generally recognized by everyone. Under the background of domestic environmental protection production, powder coatings have become the new favorite of the market. In recent years, the output and market scale of powder coatings in my country have continued to expand. They are widely used in building materials, household appliances, furniture, 3C, automobiles and other fields.

[0003] Aluminum pigment, also known as flake aluminum powder, has a special two-dimensional structure and excellent physical and chemical properties. It is one of the common metal pigments. It has excellent metallic effect, so it is widely used in the powder coating industry. However, in recent years, as outdoor building materials powder coating has higher requirements for acid and alkali resistance and weather resistance, the performance of ordinary aluminum pigments can no longer meet customer needs. Summary of the invention

[0004] Based on the above technical problems, the present invention provides a highly weather-resistant colored aluminum pigment, a preparation method and an application in powder coatings. After multi-layer coating, the aluminum pigment not only has excellent acid and alkali resistance and weather resistance, but also has diversified colors and high color concentration, meeting customers' simultaneous demands for weather resistance and colorfulness of aluminum pigments.

[0005] The invention provides a highly weather-resistant colored aluminum pigment, which comprises flaky aluminum powder and a silicon dioxide layer, a metal oxide layer and a polymer resin layer which sequentially cover the flaky aluminum powder from the inside to the outside.

[0006] For those skilled in the art, after the surface treatment of flaky aluminum powder is performed simply by organic polymer coating or inorganic sol coating, the polymer layer on the surface of the aluminum powder is easily destroyed during the high-speed mixing process, which reduces the protective effect of the aluminum powder and the weather resistance of the coating film is poor; while the aluminum powder simply coated by inorganic sol has the problem that the aluminum powder has poor compatibility with the powder coating resin and is prone to agglomeration, which affects the mechanical properties and appearance of the coating film;

[0007] Therefore, in the present invention, a silicon dioxide layer, a metal oxide layer and a polymer resin layer are sequentially coated on the surface of the aluminum powder from the inside to the outside. On the one hand, the inorganic coating layer of silicon dioxide and metal oxide solves the shortcomings of poor corrosion resistance and single color of the aluminum powder; on the other hand, the organic coating layer of the polymer resin enables the aluminum powder to be evenly dispersed in the organic matrix, which can effectively improve the adhesion of the aluminum pigment and well maintain the covering power of the aluminum pigment, thereby further ensuring the acid and alkali corrosion resistance.

[0008] Preferably, the aspect ratio of the flaky aluminum powder is 40-200, and the particle size is 10-50 μm.

[0009] Preferably, the metal oxide layer is at least one of an iron oxide layer, an iron oxide layer, a ferrous oxide layer, a titanium dioxide layer, a tin dioxide layer, a nickel oxide layer, an aluminum oxide layer, a chromium oxide layer, a zirconium dioxide layer, a manganese dioxide layer, a cobalt oxide layer or a cobalt oxide layer.

[0010] Preferably, the polymer resin layer is a polyacrylic resin layer.

[0011] The present invention also provides a method for preparing the above-mentioned highly weather-resistant colored aluminum pigment, comprising the following steps:

[0012] S1, dispersing flaky aluminum powder in an alcohol solvent, adding a silicon source for hydrolysis reaction, and coating the surface of the flaky aluminum powder to form a silicon dioxide layer;

[0013] S2, dispersing flaky aluminum powder with a silicon dioxide coating layer in water, adding a metal salt to carry out a deposition reaction, and coating the surface of the silicon dioxide layer to form a metal oxide layer;

[0014] S3, dispersing the flaky aluminum powder having the metal oxide layer and the silicon dioxide layer in an organic solvent, adding acrylic monomer, styrene monomer and initiator to carry out polymerization reaction, and coating the surface of the metal oxide layer to form a polymer resin layer, thereby obtaining the colored aluminum pigment.

[0015] In the present invention, an inorganic-organic multilayer coated aluminum pigment is prepared on the surface of flaky aluminum powder by a sol-gel method combined with an in-situ polymerization method. The surface of the inorganic-organic multilayer coated aluminum pigment has, from the inside to the outside, a dense, ultra-thin, transparent inorganic silicon dioxide layer, a colorful metal oxide layer, and a polymer resin layer that more effectively protects the flaky aluminum powder, thereby greatly improving the acid and alkali corrosion resistance and colorful performance of the aluminum pigment.

[0016] Preferably, in step S1, the silicon source is at least one of methyl orthosilicate, ethyl orthosilicate, propyl orthosilicate, butyl orthosilicate orthosilicate, or pentyl orthosilicate;

[0017] Preferably, the silicon source further comprises an aminosilane coupling agent, and the aminosilane coupling agent is at least one of 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane or 3-aminopropylmethyltriethoxysilane;

[0018] Preferably, the amount of the silicon source added is 20-50wt% of the mass of the flaky aluminum powder;

[0019] Preferably, the catalyst for the hydrolysis reaction is ammonia water or ethylenediamine, the temperature is 40-60° C., and the time is 4-8 hours.

[0020] Preferably, in step S2, the metal salt is at least one of ferric chloride, titanium chloride, tin chloride, nickel chloride, aluminum chloride, chromium chloride, zirconium chloride, manganese chloride or cobalt chloride;

[0021] Preferably, the amount of the metal salt added is 30-60wt% of the mass of the flaky aluminum powder;

[0022] Preferably, the pH value of the deposition reaction is 3-5, the temperature is 80-90° C., and the time is 10-30 min.

[0023] Preferably, in step S3, the acrylic monomer is at least one of methyl methacrylate, methyl acrylate, hydroxyethyl methacrylate, hydroxyethyl acrylate, hydroxypropyl methacrylate, hydroxypropyl acrylate, butyl methacrylate or butyl acrylate, and the initiator is azobisisobutyronitrile or azobisisoheptylnitrile;

[0024] Preferably, the amount of the acrylic acid monomer added is 20-80wt% of the mass of the flaky aluminum powder;

[0025] Preferably, the polymerization reaction temperature is 80-90° C. and the time is 2-4 hours.

[0026] Preferably, in step S3, before adding acrylic monomer, styrene monomer and initiator for polymerization reaction, the step further includes subjecting the flaky aluminum powder having the metal oxide layer and the silicon dioxide coating layer to a pre-condensation reaction with allyl chloroformate.

[0027] In the present invention, after the flaky aluminum powder is coated by hydrolysis of silicon source and metal salt, the surface of the flaky aluminum powder is grafted with amino groups and hydroxyl groups existing on the surface of the metal oxide layer. Since the amino groups or hydroxyl groups can undergo amidation or esterification condensation reaction with allyl chloroformate, acrylate can be chemically grafted on the surface of the aluminum powder. Afterwards, when acrylate monomer and styrene monomer are added for polymerization reaction, the acrylate group can form copolymers with the acrylate monomer and styrene monomer, so that it can be ensured that the obtained polymer resin layer can be tightly coated on the surface of the aluminum powder, and the obtained polymer resin layer is also more dense and not easily destroyed by pulverization, thereby further improving the adhesion, weather resistance and acid and alkali resistance of the obtained aluminum pigment.

[0028] The present invention also provides an application of the colored aluminum pigment or the colored aluminum pigment prepared by the above preparation method in powder coatings.

[0029] Beneficial effects of the present invention:

[0030] The present invention pre-coats a dense silicon dioxide protective layer on flaky aluminum powder to improve the corrosion resistance of the aluminum powder, and then utilizes metal salt hydrolysis to deposit a metal oxide layer, wherein the metal oxide layer with a high refractive index has color development and high heat resistance, and then forms a polymer resin layer on the surface of the metal oxide layer through polymerization reaction, thereby further increasing the coating density of the aluminum powder surface and improving the corrosion resistance of the coated aluminum powder. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 Schematic diagram of the appearance of spray products of commercially available aluminum pigment (left), the aluminum pigment described in Example 1 (right), and the aluminum pigment described in Example 2 (middle). DETAILED DESCRIPTION

[0032] Hereinafter, the present invention will describe the technical solution in detail through specific embodiments, but it should be clearly stated that these embodiments are for illustration only and are not to be construed as limiting the scope of the present invention.

[0033] Example 1

[0034] This embodiment provides a highly weather-resistant red aluminum pigment, which is prepared by the following method:

[0035] (1) 100 g of commercially available aluminum pigment (flaky aluminum powder having a solid content of 70 wt%, an aspect ratio of 120, and a D50 particle size of 30 μm) was added to 300 g of ethanol and stirred to mix evenly. After stirring at 40° C. for 3 h, the solvent oil, additives and other substances on the surface of the aluminum pigment were washed off, and the solid and liquid were separated to obtain a deoiled flaky aluminum powder;

[0036] (2) Add 50 g of the degreased flaky aluminum powder to 300 g of isopropanol and disperse it evenly by ultrasonication, then add 6 g of ammonia water (concentration of 15 wt%), stir and mix to obtain an aluminum powder suspension; heat the aluminum powder suspension to 50°C, and add 60 g of an isopropanol solution containing ethyl orthosilicate and 3-aminopropyltrimethoxysilane (ethyl orthosilicate concentration of 25 wt%, 3-aminopropyltrimethoxysilane concentration of 5 wt%) dropwise under rapid stirring conditions, stir and react for 6 h, age, wash, filter, and form a silicon dioxide coating layer on the surface of the flaky aluminum powder to obtain a flaky aluminum powder with a silicon dioxide coating layer;

[0037] (3) 30 g of flaky aluminum powder with a silicon dioxide coating layer was dispersed in deionized water, heated to 90°C and stirred to disperse evenly, hydrochloric acid (concentration of 30 wt%) was added to adjust the pH to 3.5, and then 100 g of ferric chloride solution (concentration of 10 wt%) was added, and sodium hydroxide solution (concentration of 15 wt%) was added dropwise to maintain a constant pH, and the mixture was kept warm and stirred for 20 min. After washing, filtering and drying, the mixture was calcined at 450°C for 30 min to form an iron oxide coating layer on the surface of the silicon dioxide coating layer, thereby obtaining a flaky aluminum powder with iron oxide and silicon dioxide coating layers;

[0038] (4) Add 20 g of flaky aluminum powder with a coating layer of ferric oxide and silicon dioxide into 100 mL of hydrocarbon solvent S-150 and stir to mix evenly. Then add 5 g of butyl acrylate and 4 g of hydroxyethyl acrylate and stir for 30 min. Then add 0.5 g of azobisisobutyronitrile dissolved in hydrocarbon solvent S-150 solution (concentration is 2 wt%). After stirring for 30 min, heat to 70 ° C under nitrogen protection, slowly add 1 g of styrene dropwise, and then heat to 80 ° C and continue to react for 3 h. Cool, wash, and filter. A polymer resin coating layer is formed on the surface of the ferric oxide coating layer to obtain the red aluminum pigment.

[0039] Example 2

[0040] This embodiment provides a highly weather-resistant golden aluminum pigment, which is prepared by the following method:

[0041] (1) 100 g of commercially available aluminum pigment (flaky aluminum powder having a solid content of 70 wt%, an aspect ratio of 120, and a D50 particle size of 30 μm) was added to 300 g of ethanol and stirred to mix evenly. After stirring at 40° C. for 3 h, the solvent oil, additives and other substances on the surface of the aluminum pigment were washed off, and the solid and liquid were separated to obtain a deoiled flaky aluminum powder;

[0042] (2) adding 50 g of the degreased flaky aluminum powder to 300 g of isopropanol and uniformly dispersing the powder by ultrasonication, then adding 5 g of ethylenediamine and stirring to obtain an aluminum powder suspension; heating the aluminum powder suspension to 40°C, and dropping 40 g of an isopropanol solution containing ethyl orthosilicate and 3-aminopropyltriethoxysilane (the concentration of ethyl orthosilicate is 25 wt %, and the concentration of 3-aminopropyltriethoxysilane is 5 wt %) under rapid stirring, stirring for 8 h, aging, washing, filtering, and forming a silicon dioxide coating layer on the surface of the flaky aluminum powder to obtain a flaky aluminum powder having a silicon dioxide coating layer;

[0043] (3) 30 g of flaky aluminum powder with a silicon dioxide coating layer was dispersed in deionized water, heated to 80° C. and stirred to disperse evenly, hydrochloric acid (concentration of 30 wt%) was added to adjust the pH to 3, and then 60 g of titanium tetrachloride solution (concentration of 20 wt%) was added, and sodium hydroxide solution (concentration of 15 wt%) was added dropwise to maintain a constant pH, and the mixture was kept warm and stirred for 30 min. After washing, filtering, and drying, the mixture was calcined at 450° C. for 30 min to form a titanium dioxide coating layer on the surface of the silicon dioxide coating layer, thereby obtaining a flaky aluminum powder with titanium dioxide and silicon dioxide coating layers;

[0044] (4) Add 20 g of flaky aluminum powder having a titanium dioxide layer and a silicon dioxide coating layer into 100 mL of hydrocarbon solvent S-150 and stir to mix evenly. Then add 10 g of methyl methacrylate and stir for 30 min. Then add 0.5 g of hydrocarbon solvent S-150 solution containing azobisisobutyronitrile (concentration is 2 wt%). After stirring for 30 min, heat to 70 °C under nitrogen protection, slowly add 2 g of styrene dropwise, and after completion, heat to 90 °C and continue to react for 2 h. Cool, wash, and filter. A polymer resin coating layer is formed on the surface of the titanium dioxide coating layer to obtain the gold aluminum pigment.

[0045] Example 3

[0046] This embodiment provides a highly weather-resistant green aluminum pigment, which is prepared by the following method:

[0047] (1) 100 g of commercially available aluminum pigment (flaky aluminum powder having a solid content of 70 wt%, an aspect ratio of 120, and a D50 particle size of 30 μm) was added to 300 g of ethanol and stirred to mix evenly. After stirring at 40° C. for 3 h, the solvent oil, additives and other substances on the surface of the aluminum pigment were washed off, and the solid and liquid were separated to obtain a deoiled flaky aluminum powder;

[0048] (2) Add 50 g of the degreased flaky aluminum powder to 300 g of isopropanol and disperse it evenly by ultrasonication, then add 6 g of ammonia water (concentration of 15 wt%), stir and mix to obtain an aluminum powder suspension; heat the aluminum powder suspension to 60°C, and add 80 g of an isopropanol solution containing ethyl orthosilicate and 3-aminopropyltrimethoxysilane (ethyl orthosilicate concentration of 25 wt%, 3-aminopropyltrimethoxysilane concentration of 5 wt%) dropwise under rapid stirring conditions, stir and react for 4 h, age, wash, filter, and form a silicon dioxide coating layer on the surface of the flaky aluminum powder to obtain a flaky aluminum powder with a silicon dioxide coating layer;

[0049] (3) 30 g of flaky aluminum powder with a silica coating layer was dispersed in deionized water, heated to 90° C. and stirred to disperse evenly, hydrochloric acid (concentration of 30 wt%) was added to adjust the pH to 5, and then 60 g of chromium trichloride solution (concentration of 15 wt%) was added, and sodium hydroxide solution (concentration of 15 wt%) was added dropwise to maintain a constant pH, and the mixture was kept warm and stirred for 10 min. After washing, filtering, and drying, the mixture was calcined at 300° C. for 30 min to form a chromium oxide coating layer on the surface of the silica coating layer, thereby obtaining a flaky aluminum powder with a chromium oxide and silica coating layer;

[0050] (4) Add 20 g of flaky aluminum powder with chromium oxide and silicon dioxide coating layers into 100 mL of hydrocarbon solvent S-150 and stir to mix evenly. Then add 3 g of methyl acrylate and 2 g of hydroxypropyl methacrylate and stir for 30 min. Then add 0.5 g of hydrocarbon solvent S-150 solution containing azobisisobutyronitrile (concentration is 2 wt%). After stirring for 30 min, heat to 70 ° C under nitrogen protection, slowly add 1 g of styrene dropwise, and then heat to 80 ° C and continue to react for 4 h. Cool, wash, and filter. A polymer resin coating layer is formed on the surface of the chromium oxide coating layer to obtain the green aluminum pigment.

[0051] Example 4

[0052] This embodiment provides a highly weather-resistant golden red aluminum pigment, which is prepared by the following method:

[0053] (1) 100 g of commercially available aluminum pigment (flaky aluminum powder having a solid content of 70 wt%, an aspect ratio of 120, and a D50 particle size of 30 μm) was added to 300 g of ethanol and stirred to mix evenly. After stirring at 40° C. for 3 h, the solvent oil, additives and other substances on the surface of the aluminum pigment were washed off, and the solid and liquid were separated to obtain a deoiled flaky aluminum powder;

[0054] (2) Add 50 g of the degreased flaky aluminum powder to 300 g of isopropanol and disperse it evenly by ultrasonication, then add 6 g of ammonia water (concentration of 15 wt%), stir and mix to obtain an aluminum powder suspension; heat the aluminum powder suspension to 50°C, and add 60 g of an isopropanol solution containing ethyl orthosilicate and 3-aminopropyltrimethoxysilane (ethyl orthosilicate concentration of 25 wt%, 3-aminopropyltrimethoxysilane concentration of 5 wt%) dropwise under rapid stirring conditions, stir and react for 6 h, age, wash, filter, and form a silicon dioxide coating layer on the surface of the flaky aluminum powder to obtain a flaky aluminum powder with a silicon dioxide coating layer;

[0055] (3) 30 g of flaky aluminum powder with a silicon dioxide coating layer was dispersed in deionized water, heated to 90°C and stirred to disperse evenly, hydrochloric acid (concentration of 30 wt%) was added to adjust the pH to 3.5, and then 100 g of ferric chloride solution (concentration of 10 wt%) was added, and sodium hydroxide solution (concentration of 15 wt%) was added dropwise to maintain a constant pH, and the mixture was kept warm and stirred for 20 min. After washing, filtering and drying, the mixture was calcined at 450°C for 30 min to form an iron oxide coating layer on the surface of the silicon dioxide coating layer, thereby obtaining a flaky aluminum powder with iron oxide and silicon dioxide coating layers;

[0056] (4) Add 20 g of flaky aluminum powder with a coating layer of ferric oxide and silicon dioxide into 50 mL of toluene and disperse it evenly by ultrasonication, then add 0.1 g of triethylamine, stir and mix, then add 2 g of a toluene solution of allyl chloroformate (concentration of 45 wt%), heat to 80 ° C and react for 2 h, filter and dry to obtain the pretreated flaky aluminum powder with a coating layer of ferric oxide and silicon dioxide;

[0057] The pretreated flaky aluminum powder having an iron oxide and silicon dioxide coating layer is added to 100 mL of hydrocarbon solvent S-150 and stirred to mix evenly. Then, 5 g of butyl acrylate and 4 g of hydroxyethyl acrylate are added and stirred for 30 min. Then, 0.5 g of azobisisobutyronitrile-dissolved hydrocarbon solvent S-150 solution (concentration is 2 wt%) is added. After stirring for 30 min, the temperature is raised to 70° C. under nitrogen protection, and 1 g of styrene is slowly added dropwise. After completion, the temperature is raised to 80° C. and the reaction is continued for 3 h. The reaction is cooled, washed, and filtered. A polymer resin coating layer is formed on the surface of the iron oxide coating layer to obtain the golden red aluminum pigment.

[0058] Comparative Example 1

[0059] This comparative example proposes a highly weather-resistant red aluminum pigment, which is prepared by the following method:

[0060] (1) 100 g of commercially available aluminum pigment (flaky aluminum powder having a solid content of 70 wt%, an aspect ratio of 120, and a D50 particle size of 30 μm) was added to 300 g of ethanol and stirred to mix evenly. After stirring at 40° C. for 3 h, the solvent oil, additives and other substances on the surface of the aluminum pigment were washed off, and the solid and liquid were separated to obtain a deoiled flaky aluminum powder;

[0061] (2) Add 50 g of the degreased flaky aluminum powder to 300 g of isopropanol and disperse it evenly by ultrasonication, then add 6 g of ammonia water (concentration of 15 wt%), stir and mix to obtain an aluminum powder suspension; heat the aluminum powder suspension to 50°C, and add 60 g of an isopropanol solution containing ethyl orthosilicate and 3-aminopropyltrimethoxysilane (ethyl orthosilicate concentration of 25 wt%, 3-aminopropyltrimethoxysilane concentration of 5 wt%) dropwise under rapid stirring conditions, stir and react for 6 h, age, wash, filter, and form a silicon dioxide coating layer on the surface of the flaky aluminum powder to obtain a flaky aluminum powder with a silicon dioxide coating layer;

[0062] (3) 30 g of flaky aluminum powder with a silicon dioxide coating layer is dispersed in deionized water, heated to 90° C. and stirred to disperse evenly, hydrochloric acid (concentration of 30 wt%) is added to adjust the pH to 3.5, and then 100 g of ferric chloride solution (concentration of 10 wt%) is added, and sodium hydroxide solution (concentration of 15 wt%) is added dropwise to maintain a constant pH, and the mixture is kept warm and stirred for 20 min. After washing, filtering, and drying, the mixture is calcined at 450° C. for 30 min. A ferric oxide coating layer is formed on the surface of the silicon dioxide coating layer, thereby obtaining the red aluminum pigment.

[0063] The aluminum pigments described in the examples and comparative examples were subjected to the following performance tests, and the results are shown in Table 1 below:

[0064] Hydrogen evolution test: add 1g aluminum pigment to 200mL of 0.01mol / L hydrochloric acid solution (or 0.01mol / L sodium hydroxide solution), place in a 250mL ground-mouth flask, and collect the released hydrogen with a graduated glass tube. The test time is 1 week.

[0065] Glossiness test: add 1g aluminum pigment to 1g ethylene glycol monobutyl ether, then add 10g acrylic resin, stir evenly, add appropriate amount of ethylene glycol monobutyl ether to adjust the viscosity, spray on a special iron plate, and after drying, use a gloss meter to test the glossiness of the coating at 60°;

[0066] Adhesion test: add 1g aluminum pigment to 1g ethylene glycol monobutyl ether, then add 10g acrylic resin, stir evenly, add appropriate amount of ethylene glycol monobutyl ether to adjust the viscosity, spray on a special iron plate, and after drying, perform a paint film adhesion test according to the national standard GB / T9286-1998 "Paint and varnish, cross-cut test of paint film". The test results are divided into 0-5 levels, with 0 being the best and 5 being the worst;

[0067] Artificial weathering: Add 1g aluminum pigment to 1g ethylene glycol monobutyl ether, then add 10g acrylic resin, stir evenly, add appropriate amount of ethylene glycol monobutyl ether to adjust the viscosity, spray on a special iron plate, and after drying, perform artificial weathering test according to method 1 cycle A in national standard GB / T1865-2009.

[0068] Table 1 Test properties of the aluminum pigments described in the examples and comparative examples

[0069] Acid corrosion hydrogen evolution amount (mL) Alkali corrosion hydrogen evolution amount (mL) 60° glossiness Adhesion (grade) Artificial weathering Example 1 2 5 96 1 1000h paint film discoloration level 0, differentiation level 0, no cracking Example 2 3 7 95 1 1000h paint film discoloration level 0, differentiation level 0, no cracking Example 3 3 6 95 1 1000h paint film discoloration level 0, differentiation level 0, no cracking Example 4 1 1 96 0 1000h paint film discoloration level 0, differentiation level 0, no cracking Comparative Example 1 23 46 91 2 1000h paint film discoloration level 1, differentiation level 0, no cracking Commercially available aluminum pigments 156 275 99 3 1000h paint film discoloration level 2, differentiation level 1, many cracks

[0070] As shown in Table 1 above, it can be seen that compared with commercially available aluminum pigments, the amount of hydrogen evolution of the pure inorganic silica and ferric oxide coated red aluminum pigment (Comparative Example 1) in acidic and alkaline corrosion solutions is significantly reduced, but the amount of hydrogen evolution of the inorganic silica, ferric oxide and organic polymer resin layer coated red aluminum pigment (Example 1) is even less, and if the flaky aluminum powder with ferric oxide and silica coating layer is pretreated, a more compact organic polymer resin layer coated color aluminum pigment (Example 4) can be obtained, so its hydrogen evolution amount is more excellent, especially under alkaline conditions. In addition, the adhesion evaluation result of the aluminum pigment (Example 4) is also excellent.

[0071] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A highly weather-resistant colored aluminum pigment, characterized in that: The aluminum pigment comprises flaky aluminum powder and a silicon dioxide layer, a metal oxide layer and a polymer resin layer which sequentially cover the flaky aluminum powder from the inside to the outside; The polymer resin layer is a polyacrylic resin layer; The highly weather-resistant colored aluminum pigment is prepared by the following preparation method: S1, dispersing flaky aluminum powder in an alcohol solvent, adding a silicon source for hydrolysis reaction, and coating the surface of the flaky aluminum powder to form a silicon dioxide layer; S2, dispersing flaky aluminum powder with a silicon dioxide coating layer in water, adding a metal salt to carry out a deposition reaction, and coating the surface of the silicon dioxide layer to form a metal oxide layer; S3, dispersing the flaky aluminum powder having the metal oxide layer and the silicon dioxide layer in an organic solvent, adding acrylic monomer, styrene monomer and initiator to carry out polymerization reaction, and coating the surface of the metal oxide layer to form a polymer resin layer, so as to obtain the colored aluminum pigment; In step S1, the silicon source is at least one of methyl orthosilicate, ethyl orthosilicate, propyl orthosilicate, butyl orthosilicate orthosilicate, or pentyl orthosilicate; The silicon source further includes an aminosilane coupling agent, wherein the aminosilane coupling agent is at least one of 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane or 3-aminopropylmethyltriethoxysilane; In step S3, before adding acrylic monomer, styrene monomer and initiator for polymerization reaction, the step further includes subjecting the flaky aluminum powder having the metal oxide layer and the silicon dioxide layer to a pre-condensation reaction with allyl chloroformate.

2. The highly weather-resistant colored aluminum pigment according to claim 1, characterized in that: The aspect ratio of the flaky aluminum powder is 40-200, and the particle size is 10-50 μm.

3. The highly weather-resistant colored aluminum pigment according to claim 1 or 2, characterized in that: The metal oxide layer is at least one of a ferric oxide layer, a ferrous oxide layer, a titanium dioxide layer, a tin dioxide layer, a nickel oxide layer, an aluminum oxide layer, a chromium oxide layer, a zirconium dioxide layer, a manganese dioxide layer, a cobalt oxide layer or a cobalt oxide layer.

4. A method for preparing the highly weather-resistant colored aluminum pigment according to any one of claims 1 to 3, characterized in that: The steps include: S1, dispersing flaky aluminum powder in an alcohol solvent, adding a silicon source for hydrolysis reaction, and coating the surface of the flaky aluminum powder to form a silicon dioxide layer; S2, dispersing flaky aluminum powder with a silicon dioxide coating layer in water, adding a metal salt to carry out a deposition reaction, and coating the surface of the silicon dioxide layer to form a metal oxide layer; S3, dispersing the flaky aluminum powder having the metal oxide layer and the silicon dioxide layer in an organic solvent, adding acrylic monomer, styrene monomer and initiator to carry out polymerization reaction, and coating the surface of the metal oxide layer to form a polymer resin layer, so as to obtain the colored aluminum pigment; In step S1, the silicon source is at least one of methyl orthosilicate, ethyl orthosilicate, propyl orthosilicate, butyl orthosilicate orthosilicate, or pentyl orthosilicate; The silicon source further includes an aminosilane coupling agent, wherein the aminosilane coupling agent is at least one of 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane or 3-aminopropylmethyltriethoxysilane; In step S3, before adding acrylic monomer, styrene monomer and initiator for polymerization reaction, the step further includes subjecting the flaky aluminum powder having the metal oxide layer and the silicon dioxide layer to a pre-condensation reaction with allyl chloroformate.

5. The method for preparing the highly weather-resistant colored aluminum pigment according to claim 4, characterized in that: In step S1, the amount of silicon source added is 20-50wt% of the mass of the flaky aluminum powder; The catalyst for the hydrolysis reaction is ammonia water or ethylenediamine, the temperature is 40-60° C., and the time is 4-8 hours.

6. The method for preparing the highly weather-resistant colored aluminum pigment according to claim 4 or 5, characterized in that: In step S2, the metal salt is at least one of ferric chloride, titanium chloride, tin chloride, nickel chloride, aluminum chloride, chromium chloride, zirconium chloride, manganese chloride or cobalt chloride; The amount of the metal salt added is 30-60wt% of the mass of the flaky aluminum powder; The pH value of the deposition reaction is 3-5, the temperature is 80-90° C., and the time is 10-30 minutes.

7. The method for preparing the highly weather-resistant colored aluminum pigment according to claim 4 or 5, characterized in that: In step S3, the acrylic monomer is at least one of methyl methacrylate, methyl acrylate, hydroxyethyl methacrylate, hydroxyethyl acrylate, hydroxypropyl methacrylate, hydroxypropyl acrylate, butyl methacrylate or butyl acrylate, and the initiator is azobisisobutyronitrile or azobisisoheptylnitrile; The amount of the acrylic acid monomer added is 20-80wt% of the mass of the flaky aluminum powder; The polymerization reaction temperature is 80-90° C. and the reaction time is 2-4 hours.

8. Use of the colored aluminum pigment according to any one of claims 1 to 3 or the colored aluminum pigment prepared by the preparation method according to any one of claims 4 to 7 in powder coatings.

Citation Information

Patent Citations

  • Pearlescent iridescent aluminum powder pigment and its preparation method

    CN102260421A

  • Waterproof anti-bacterial polyurethane composite material

    CN105778475A

  • Aluminum pigment and preparation method thereof

    CN109575646A

  • Metal pigment composition

    US20070051272A1

  • Vinylchloroformate-free synthesis of vinyl and allyl(THIO)carbamates

    WO2005073181A1