Light emitting diode epitaxial wafer and preparation method thereof, LED
By using the C/Mg co-doped nitride layer and the C-doped Ga nitride layer in the GaN-based light emitting diode, the line defect problem is solved, the crystal quality and luminous efficiency are improved, and high efficiency is achieved Preparation of light emitting diode epitaxial sheets.
Patent Information
- Application Number
- CN202411187408.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-28
AI Technical Summary
The existing GaN-based light-emitting diode epitaxial layer is prone to linear defects during the nucleation process, resulting in poor crystal quality and low luminous efficiency, and difficulty in controlling the growth of the nucleation layer. High island density leads to high linear defect density, affecting the performance of the light-emitting diode.
Using a three-dimensional nucleation layer structure including a C/Mg co-doped nitride layer, a first C-doped Ga nitride layer and a second C-doped Ga nitride layer, the line defects are reduced by isolation of the SiN layer and controlled to form a Nuclear point density reduces thermal expansion stress and improves crystal quality.
The crystal quality of the GaN epitaxial layer is improved, the non-radiation recombination efficiency of the quantum well is reduced, the luminous efficiency of the light emitting diode is improved, the preparation process is simplified, and the production of high-efficiency light emitting diode epitaxial sheets is stable.
Smart Images

Figure CN118693197B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of optoelectronic technology, and in particular to a light emitting diode epitaxial wafer and a preparation method thereof, and an LED. Background Art
[0002] At present, the epitaxial layer structure of GaN-based light-emitting diodes includes a substrate, on which a buffer layer, a three-dimensional nucleation layer, a non-doped GaN layer, a multi-quantum well layer, an electron blocking layer and a P-type GaN layer are deposited in sequence. The linear defects generated in the nucleation layer during the growth process have a great impact on the crystal quality of the GaN epitaxial layer.
[0003] At present, the deposition of three-dimensional nucleation layers mainly has the following problems: first, the low deposition temperature of the buffer layer leads to poor crystal quality of the thin film, which affects the crystal quality of the subsequent nucleation layer. Second, the density of the nucleation islands cannot be controlled during the deposition process of the nucleation layer, resulting in high island density, small distance between islands, premature fusion of islands to produce line defects, and high line defect density. Line defects not only act as non-radiative recombination centers, but also introduce energy levels in the bandgap, reduce the minority carrier lifetime, and reduce the luminous efficiency of the light-emitting diode. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a light-emitting diode epitaxial wafer, which improves the crystal quality of the GaN epitaxial layer, reduces the quantum well non-radiative recombination efficiency, and improves the luminous efficiency of the light-emitting diode.
[0005] The technical problem to be solved by the present invention is to provide a method for preparing a light emitting diode epitaxial wafer, which has a simple process and can stably prepare a light emitting diode epitaxial wafer with good luminous efficiency.
[0006] In order to solve the above technical problems, the present invention provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a SiN layer, a three-dimensional nucleation layer, a non-doped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer are sequentially arranged;
[0007] The three-dimensional nucleation layer includes a C / Mg co-doped nitride layer, a first C-doped Ga-containing nitride layer, and a second C-doped Ga-containing nitride layer stacked in sequence, and the growth temperature of the C / Mg co-doped nitride layer is less than the growth temperature of the first C-doped Ga-containing nitride layer and less than the growth temperature of the second C-doped Ga-containing nitride layer.
[0008] In some embodiments, the SiN layer has a thickness of 1 nm to 50 nm.
[0009] In some embodiments, the nitride of the C / Mg co-doped nitride layer is one of GaN, AlGaN, InGaN, AlN, AlInGaN, BGaN, BAlN, and BInGaN.
[0010] In some embodiments, the thickness of the C / Mg co-doped nitride layer is 0.05 μm to 0.5 μm;
[0011] The C doping concentration of the C / Mg co-doped nitride layer is 5×10 16 atoms / cm 3 ~5×10 17 atoms / cm 3 ;
[0012] The Mg doping concentration of the C / Mg co-doped nitride layer is 1×10 17 atoms / cm 3 ~1×10 18 atoms / cm 3 .
[0013] In some embodiments, the Ga-containing nitride of the first C-doped Ga-containing nitride layer is one of GaN, AlGaN, InGaN, AlInGaN, BGaN, and BInGaN.
[0014] In some embodiments, the thickness of the first C-doped Ga-containing nitride layer is 0.1 μm to 2 μm;
[0015] The C doping concentration of the first C-doped Ga-containing nitride layer is 1×10 16 atoms / cm 3 ~1×10 18 atoms / cm 3 .
[0016] In some embodiments, the Ga-containing nitride of the second C-doped Ga-containing nitride layer is one of GaN, AlGaN, InGaN, AlInGaN, BGaN, and BInGaN.
[0017] In some embodiments, the thickness of the second C-doped Ga-containing nitride layer is 0.1 μm to 2 μm;
[0018] The C doping concentration of the second C-doped Ga-containing nitride layer is 1×10 16 atoms / cm 3 ~1×10 17 atoms / cm 3 .
[0019] In order to solve the above technical problems, the present invention also provides a method for preparing a light emitting diode epitaxial wafer, comprising the following steps:
[0020] S1. providing a substrate;
[0021] S2, depositing a buffer layer, a SiN layer, a three-dimensional nucleation layer, an undoped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer on the substrate in sequence;
[0022] The three-dimensional nucleation layer includes a C / Mg co-doped nitride layer, a first C-doped Ga-containing nitride layer, and a second C-doped Ga-containing nitride layer stacked in sequence, and the C doping concentration of the C / Mg co-doped nitride layer is greater than the C doping concentration of the first C-doped Ga-containing nitride layer and is greater than the C doping concentration of the second C-doped Ga-containing nitride layer.
[0023] Correspondingly, the present invention further provides an LED, wherein the LED comprises the light emitting diode epitaxial wafer as described above.
[0024] The implementation of the present invention has the following beneficial effects:
[0025] The SiN layer is used as an isolation layer to reduce the extension of line defects caused by lattice mismatch and thermal mismatch in the buffer layer deposited on the substrate to the epitaxial layer, improve the crystal quality of the subsequent three-dimensional nucleation layer, and reduce the leakage of the light-emitting diode.
[0026] When depositing the C / Mg co-doped nitride layer, the growth temperature is low, which can release the thermal expansion stress of the epitaxial layer and reduce the warping of the epitaxial layer. The C impurities can annihilate the point defects of the epitaxial layer, while the Mg impurities can control the density of the nucleation points and improve the crystal quality.
[0027] The growth temperature of the first C-doped Ga-containing nitride layer is higher than that of the C / Mg co-doped nitride layer, which improves the mobility of atoms and promotes the gradual increase of nucleation points into small island-shaped nucleation layers, thereby avoiding premature fusion of small islands in the nucleation layer to produce line defects. Doping a small amount of C impurities is also for annihilating defects and improving crystal quality.
[0028] The growth temperature of the second C-doped Ga-containing nitride layer is higher than the deposition temperature of the first C-doped Ga-containing nitride layer, which further promotes the growth and fusion of the small island-shaped nucleation layer, reduces the contact angle of the nucleation growth for the subsequent deposition of the non-doped GaN layer, and enables the island-grown GaN grains to be connected into a surface within a smaller thickness, transforming into two-dimensional epitaxial growth, thereby improving the crystal quality of the subsequent deposited epitaxial layer, reducing the quantum well non-radiative recombination efficiency, and improving the luminous efficiency of the light-emitting diode. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1This is a schematic structural diagram of the light emitting diode epitaxial wafer provided by the present invention. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. Examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention. In addition, it should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0031] In the description of the present invention, it is necessary to understand that the terms "length", "width", "up", "down", "left", "right", "horizontal", "top", "bottom", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0032] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0033] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or mutual communication; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0034] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.
[0035] The disclosure below provides many different embodiments or examples to realize different structures of the present invention. In order to simplify the disclosure of the present invention, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present invention. In addition, the present invention can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplification and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed. In addition, the examples of various specific processes and materials provided by the present invention, but those of ordinary skill in the art can be aware of the application of other processes and / or the use of other materials.
[0036] In the present invention, "preferred" and "better" are only used to describe implementation methods or embodiments with better effects, and it should be understood that they do not constitute a limitation on the scope of protection of the present invention. In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features. In the present invention, when involving numerical ranges, unless otherwise specified, the two endpoints of the numerical range are included.
[0037] To solve the above problems, the present invention provides a light emitting diode epitaxial wafer, such as Figure 1 As shown, it includes a substrate 100, on which a buffer layer 200, a SiN layer 300, a three-dimensional nucleation layer 400, an undoped GaN layer 500, an N-type GaN layer 600, an active layer 700, an electron blocking layer 800, and a P-type GaN layer 900 are sequentially arranged;
[0038] The three-dimensional nucleation layer 400 includes a C / Mg co-doped nitride layer 410, a first C-doped Ga-containing nitride layer 420, and a second C-doped Ga-containing nitride layer 430 stacked in sequence, and the growth temperature of the C / Mg co-doped nitride layer 410 is less than the growth temperature of the first C-doped Ga-containing nitride layer 420 and less than the growth temperature of the second C-doped Ga-containing nitride layer 430.
[0039] The specific structures of the SiN layer 300 and the three-dimensional nucleation layer 400 provided by the present invention are as follows:
[0040] In some embodiments, the thickness of the SiN layer 300 is 1 nm to 50 nm. Exemplary thicknesses of the SiN layer 300 are 5 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, and 45 nm, but are not limited to the above. The SiN layer acts as an isolation layer to reduce the extension of line defects generated by lattice mismatch and thermal mismatch when the buffer layer is deposited on the substrate to the epitaxial layer, improve the crystal quality of the subsequently deposited three-dimensional nucleation layer, and reduce leakage of the light-emitting diode.
[0041] In some embodiments, the nitride of the C / Mg co-doped nitride layer 410 is one of GaN, AlGaN, InGaN, AlN, AlInGaN, BGaN, BAlN, and BInGaN.
[0042] In some embodiments, the thickness of the C / Mg co-doped nitride layer 410 is 0.05 μm to 0.5 μm; exemplary thicknesses of the C / Mg co-doped nitride layer 410 are 0.1 μm, 0.15 μm, 0.2 μm, 0.25 μm, 0.3 μm, 0.35 μm, 0.4 μm, and 0.45 μm, but are not limited to the above. In some embodiments, the C doping concentration of the C / Mg co-doped nitride layer 410 is 5×10 16 atoms / cm 3 ~5×10 17 atoms / cm 3 The Mg doping concentration of the C / Mg co-doped nitride layer 410 is 1×10 17 atoms / cm 3 ~1×10 18 atoms / cm 3 .
[0043] In some embodiments, the growth temperature of the C / Mg co-doped nitride layer 410 is 900° C. to 1050° C. When the C / Mg co-doped nitride layer is deposited, the growth temperature is low, which can release the thermal expansion stress of the epitaxial layer and reduce the warping of the epitaxial layer. The C impurities can annihilate the point defects of the epitaxial layer, while the Mg impurities can control the density of the nucleation points and improve the crystal quality.
[0044] In some embodiments, the Ga-containing nitride of the first C-doped Ga-containing nitride layer 420 is one of GaN, AlGaN, InGaN, AlInGaN, BGaN, and BInGaN. In some embodiments, the thickness of the first C-doped Ga-containing nitride layer 420 is 0.1 μm to 2 μm; the exemplary thickness of the first C-doped Ga-containing nitride layer 420 is 0.2 μm, 0.4 μm, 0.6 μm, 0.8 μm, 1 μm, 1.2 μm, 1.4 μm, 1.6 μm, and 1.8 μm, but is not limited to the above. In some embodiments, the C doping concentration of the first C-doped Ga-containing nitride layer 420 is 1×10 16 atoms / cm 3 ~1×10 18 atoms / cm 3 In some embodiments, the growth temperature of the first C-doped Ga-containing nitride layer 420 is 1000°C to 1150°C. The growth temperature of the first C-doped Ga-containing nitride layer is higher than that of the C / Mg co-doped nitride layer, which improves the mobility of atoms and promotes the gradual increase of nucleation points into small island-shaped nucleation layers, thereby avoiding premature fusion of small islands in the nucleation layer to generate line defects. Doping a small amount of C impurities is also to annihilate defects and improve crystal quality.
[0045] In some embodiments, the Ga-containing nitride of the second C-doped Ga-containing nitride layer 430 is one of GaN, AlGaN, InGaN, AlInGaN, BGaN, and BInGaN. In some embodiments, the thickness of the second C-doped Ga-containing nitride layer 430 is 0.1 μm to 2 μm; the exemplary thickness of the second C-doped Ga-containing nitride layer 430 is 0.2 μm, 0.4 μm, 0.6 μm, 0.8 μm, 1 μm, 1.2 μm, 1.4 μm, 1.6 μm, and 1.8 μm, but is not limited to the above. In some embodiments, the C doping concentration of the second C-doped Ga-containing nitride layer 430 is 1×10 16 atoms / cm 3 ~1×10 17 atoms / cm 3 . In some embodiments, the growth temperature of the second C-doped Ga-containing nitride layer 430 is 1000°C to 1150°C. The growth temperature of the second C-doped Ga-containing nitride layer is higher than the deposition temperature of the first C-doped Ga-containing nitride layer, which further promotes the further growth and fusion of the small island-shaped nucleation layer, reduces the contact angle of the nucleation growth for the subsequent deposition of the non-doped GaN layer, enables the island-shaped GaN grains to be connected to form a surface within a smaller thickness, and transforms into two-dimensional epitaxial growth, thereby improving the crystal quality of the subsequent deposited epitaxial layer, reducing the quantum well non-radiative recombination efficiency, and improving the luminous efficiency of the light-emitting diode.
[0046] In summary, the present invention improves the crystal quality of the GaN epitaxial layer, reduces the quantum well non-radiative recombination efficiency, and improves the luminous efficiency of the light-emitting diode.
[0047] Accordingly, the present invention provides a method for preparing a light emitting diode epitaxial wafer, comprising the following steps:
[0048] S1, providing a substrate 100;
[0049] In some embodiments, the substrate 100 may be selected from one of a sapphire substrate, a SiO2 sapphire composite substrate, a silicon substrate, a silicon carbide substrate, a gallium nitride substrate, and a zinc oxide substrate. Preferably, the substrate 100 is a sapphire substrate, which is a commonly used GaN-based LED substrate material. The sapphire substrate has a mature preparation process, a low price, is easy to clean and handle, and has good stability at high temperatures.
[0050] S2, sequentially depositing a buffer layer 200, a SiN layer 300, a three-dimensional nucleation layer 400, a non-doped GaN layer 500, an N-type GaN layer 600, an active layer 700, an electron blocking layer 800, and a P-type GaN layer 900 on the substrate 100;
[0051] The three-dimensional nucleation layer 400 includes a C / Mg co-doped nitride layer 410, a first C-doped Ga-containing nitride layer 420, and a second C-doped Ga-containing nitride layer 430 stacked in sequence, and the growth temperature of the C / Mg co-doped nitride layer 410 is less than the growth temperature of the first C-doped Ga-containing nitride layer 420 and less than the growth temperature of the second C-doped Ga-containing nitride layer 430.
[0052] Specifically, the above step S2 specifically includes the following steps:
[0053] S21 , depositing the buffer layer 200 on the substrate 100 .
[0054] In some embodiments, the buffer layer 200 is an AlN buffer layer.
[0055] S22 , depositing the SiN layer 300 on the buffer layer 200 .
[0056] In some embodiments, the growth temperature of the SiN layer is 900° C. to 1100° C., and the growth pressure is 50 torr to 500 torr.
[0057] S23 , depositing the three-dimensional nucleation layer 400 on the SiN layer 300 .
[0058] In some embodiments, the C / Mg co-doped nitride layer 410 is grown at a temperature of 900° C. to 1050° C. and a pressure of 50 torr to 500 torr.
[0059] In some embodiments, the growth temperature of the first C-doped Ga-containing nitride layer 420 is 1000° C. to 1150° C., and the growth pressure is 50 torr to 500 torr.
[0060] In some embodiments, the second C-doped Ga-containing nitride layer 430 is grown at a temperature of 1000° C. to 1150° C. and at a pressure of 50 torr to 500 torr.
[0061] S24 , depositing the undoped GaN layer 500 on the three-dimensional nucleation layer 400 .
[0062] In some embodiments, the temperature of the reaction chamber is controlled at 1050° C. to 1200° C., the pressure is controlled at 100 torr to 600 torr, N source and Ga source are introduced, and a non-doped GaN layer with a thickness of 1 μm to 5 μm is grown.
[0063] S25 , depositing the N-type GaN layer 600 on the undoped GaN layer 500 .
[0064] In some embodiments, the temperature of the reaction chamber is controlled at 1050° C. to 1200° C., the pressure is controlled at 100 torr to 600 torr, and an N source, a Ga source, and a Si source are introduced to grow the N-type GaN layer.
[0065] S26 , depositing the active layer 700 on the N-type GaN layer 600 .
[0066] In some embodiments, the active layer is an alternately stacked InGaN quantum well layer and an AlGaN quantum barrier layer, with a stacking period number of 1 to 20. The growth temperature of the InGaN quantum well layer is 750°C to 850°C, the thickness is 2nm to 5nm, and the growth pressure is 50torr to 300torr; the growth temperature of the AlGaN quantum barrier layer is 800°C to 900°C, the thickness is 5nm to 15nm, and the growth pressure is 50torr to 300torr.
[0067] S27, depositing the electron blocking layer 800 on the active layer 700;
[0068] In some embodiments, the temperature of the reaction chamber is controlled at 900° C. to 1000° C., the pressure is controlled at 100 torr to 300 torr, N source, Al source, Ga source, and In source are introduced, and an AlInGaN electron blocking layer with a thickness of 10 nm to 40 nm is grown.
[0069] S28 , depositing the P-type GaN layer 900 on the electron blocking layer 800 .
[0070] In some embodiments, the temperature of the reaction chamber is controlled at 900° C. to 1050° C., the pressure is controlled at 100 torr to 600 torr, and an N source, a Mg source, and a Ga source are introduced to grow the P-type GaN layer.
[0071] Accordingly, the present invention further provides an LED, which comprises the above-mentioned light-emitting diode epitaxial wafer, wherein the photoelectric efficiency of the LED is effectively improved and other electrical properties are good.
[0072] The present invention is further described below with specific embodiments:
[0073] Example 1
[0074] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a SiN layer, a three-dimensional nucleation layer, an undoped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;
[0075] The three-dimensional nucleation layer includes a C / Mg co-doped AlInGaN layer, a first C-doped GaN layer, and a second C-doped GaN layer stacked in sequence;
[0076] The thickness of the SiN layer is 15 nm;
[0077] The thickness of the C / Mg co-doped AlInGaN layer is 0.2 μm, and the C doping concentration is 2.5×10 17 atoms / cm 3 , the Mg doping concentration is 4.3×10 17 atoms / cm 3 , the growth temperature is 950℃;
[0078] The thickness of the first C-doped GaN layer is 1.1 μm and the C doping concentration is 1.6×10 17 atoms / cm 3 , the growth temperature is 1050℃;
[0079] The thickness of the second C-doped GaN layer is 1.3 μm, and the C doping concentration is 8×10 16 atoms / cm 3 , the growth temperature is 1100℃.
[0080] Example 2
[0081] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a SiN layer, a three-dimensional nucleation layer, an undoped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;
[0082] The three-dimensional nucleation layer includes a C / Mg co-doped AlInGaN layer, a first C-doped GaN layer, and a second C-doped GaN layer stacked in sequence;
[0083] The thickness of the SiN layer is 10 nm;
[0084] The thickness of the C / Mg co-doped AlInGaN layer is 0.3 μm, and the C doping concentration is 2.5×10 17 atoms / cm 3 , the Mg doping concentration is 4.3×10 17 atoms / cm 3 , the growth temperature is 950℃;
[0085] The thickness of the first C-doped GaN layer is 1.3 μm, and the C doping concentration is 1.6×10 17 atoms / cm 3 , the growth temperature is 1050℃;
[0086] The thickness of the second C-doped GaN layer is 1.5 μm, and the C doping concentration is 8×10 16 atoms / cm 3 , the growth temperature is 1100℃.
[0087] Example 3
[0088] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a SiN layer, a three-dimensional nucleation layer, an undoped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;
[0089] The three-dimensional nucleation layer includes a C / Mg co-doped AlInGaN layer, a first C-doped GaN layer, and a second C-doped GaN layer stacked in sequence;
[0090] The thickness of the SiN layer is 20 nm;
[0091] The thickness of the C / Mg co-doped AlInGaN layer is 0.15 μm, and the C doping concentration is 2.5×10 17 atoms / cm 3 , the Mg doping concentration is 4.3×10 17 atoms / cm 3 , the growth temperature is 950℃;
[0092] The thickness of the first C-doped GaN layer is 0.9 μm and the C doping concentration is 1.6×10 17 atoms / cm 3 , the growth temperature is 1050℃;
[0093] The thickness of the second C-doped GaN layer is 1.1 μm, and the C doping concentration is 8×10 16 atoms / cm 3 , the growth temperature is 1100℃.
[0094] Example 4
[0095] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a SiN layer, a three-dimensional nucleation layer, an undoped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;
[0096] The three-dimensional nucleation layer includes a C / Mg co-doped AlInGaN layer, a first C-doped GaN layer, and a second C-doped GaN layer stacked in sequence;
[0097] The thickness of the SiN layer is 15 nm;
[0098] The thickness of the C / Mg co-doped AlInGaN layer is 0.2 μm, and the C doping concentration is 3×10 17 atoms / cm 3 , Mg doping concentration is 2.5×10 17 atoms / cm 3 , the growth temperature is 950℃;
[0099] The thickness of the first C-doped GaN layer is 1.1 μm and the C doping concentration is 1.6×10 17 atoms / cm 3 , the growth temperature is 1050℃;
[0100] The thickness of the second C-doped GaN layer is 1.3 μm, and the C doping concentration is 8×10 16 atoms / cm 3 , the growth temperature is 1100℃.
[0101] Example 5
[0102] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a SiN layer, a three-dimensional nucleation layer, an undoped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;
[0103] The three-dimensional nucleation layer includes a C / Mg co-doped AlInGaN layer, a first C-doped GaN layer, and a second C-doped GaN layer stacked in sequence;
[0104] The thickness of the SiN layer is 15 nm;
[0105] The thickness of the C / Mg co-doped AlInGaN layer is 0.2 μm, and the C doping concentration is 2×10 17 atoms / cm 3 , Mg doping concentration is 5×10 17 atoms / cm 3 , the growth temperature is 950℃;
[0106] The thickness of the first C-doped GaN layer is 1.1 μm and the C doping concentration is 1.6×10 17 atoms / cm 3 , the growth temperature is 1050℃;
[0107] The thickness of the second C-doped GaN layer is 1.3 μm, and the C doping concentration is 8×10 16 atoms / cm 3 , the growth temperature is 1100℃.
[0108] Example 6
[0109] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a SiN layer, a three-dimensional nucleation layer, an undoped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;
[0110] The three-dimensional nucleation layer includes a C / Mg co-doped AlInGaN layer, a first C-doped GaN layer, and a second C-doped GaN layer stacked in sequence;
[0111] The thickness of the SiN layer is 15 nm;
[0112] The thickness of the C / Mg co-doped AlInGaN layer is 0.2 μm, and the C doping concentration is 2.5×10 17 atoms / cm 3 , the Mg doping concentration is 4.3×10 17 atoms / cm 3 , the growth temperature is 950℃;
[0113] The thickness of the first C-doped GaN layer is 1.1 μm and the C doping concentration is 1.1×10 17 atoms / cm 3 , the growth temperature is 1050℃;
[0114] The thickness of the second C-doped GaN layer is 1.3 μm, and the C doping concentration is 7×10 16 atoms / cm 3, the growth temperature is 1100℃.
[0115] Example 7
[0116] This embodiment provides a light-emitting diode epitaxial wafer, comprising a substrate, on which a buffer layer, a SiN layer, a three-dimensional nucleation layer, an undoped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer are sequentially provided;
[0117] The three-dimensional nucleation layer includes a C / Mg co-doped AlInGaN layer, a first C-doped GaN layer, and a second C-doped GaN layer stacked in sequence;
[0118] The thickness of the SiN layer is 15 nm;
[0119] The thickness of the C / Mg co-doped AlInGaN layer is 0.2 μm, and the C doping concentration is 2.5×10 17 atoms / cm 3 , the Mg doping concentration is 4.3×10 17 atoms / cm 3 , the growth temperature is 950℃;
[0120] The thickness of the first C-doped GaN layer is 1.1 μm and the C doping concentration is 2×10 17 atoms / cm 3 , the growth temperature is 1050℃;
[0121] The thickness of the second C-doped GaN layer is 1.3 μm, and the C doping concentration is 8.5×10 16 atoms / cm 3 , the growth temperature is 1100℃.
[0122] Comparative Example 1
[0123] This comparative example provides a light emitting diode epitaxial wafer, which is different from the other embodiment 1 in that there is no SiN layer, and the rest is the same as the embodiment 1.
[0124] Comparative Example 2
[0125] This comparative example provides a light-emitting diode epitaxial wafer, and the difference between the other embodiments and the first embodiment is that: its three-dimensional nucleation layer is a three-dimensional GaN nucleation layer, and the rest is the same as the first embodiment.
[0126] The light-emitting diode epitaxial wafers prepared in Examples 1 to 7 and Comparative Examples 1 and 2 were prepared into 10 mil × 24 mil chips using the same chip process conditions. 300 LED chips were respectively extracted and tested at a current of 120 mA. Compared with the LED prepared in Comparative Example 2, the luminous efficiency improvement rate of each example was calculated. The specific test results are shown in Table 1.
[0127] Table 1 Performance test results of LEDs obtained from Examples 1 to 7 and Comparative Examples 1 and 2
[0128]
[0129] Among them, XRD (002) data can characterize screw dislocations, and XRD (102) data can characterize mixed dislocations of screw dislocations and edge dislocations. The smaller the value of XRD (002) or XRD (102), the lower the dislocation density and the better the crystal quality. From the above results, it can be seen that the light-emitting diode epitaxial wafer provided by the present invention can improve the crystal quality of the GaN epitaxial layer, reduce the non-radiative recombination efficiency of the quantum well, and improve the luminous efficiency of the light-emitting diode.
[0130] In the description of this specification, the description with reference to the terms "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiments or examples are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0131] The above is a preferred embodiment of the invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the invention. These improvements and modifications are also considered to be within the scope of protection of the invention.
Claims
1. A light emitting diode epitaxial wafer, characterized in that: It comprises a substrate, on which a buffer layer, a SiN layer, a three-dimensional nucleation layer, a non-doped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer are sequentially arranged; The three-dimensional nucleation layer includes a C / Mg co-doped nitride layer, a first C-doped Ga-containing nitride layer, and a second C-doped Ga-containing nitride layer stacked in sequence, and the growth temperature of the C / Mg co-doped nitride layer is less than the growth temperature of the first C-doped Ga-containing nitride layer and less than the growth temperature of the second C-doped Ga-containing nitride layer.
2. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The thickness of the SiN layer is 1 nm to 50 nm.
3. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The nitride of the C / Mg co-doped nitride layer is one of GaN, AlGaN, InGaN, AlN, AlInGaN, BGaN, BAlN, and BInGaN.
4. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The thickness of the C / Mg co-doped nitride layer is 0.05 μm to 0.5 μm; The C doping concentration of the C / Mg co-doped nitride layer is 5×10 16 atoms / cm 3 ~5×10 17 atoms / cm 3 ; The Mg doping concentration of the C / Mg co-doped nitride layer is 1×10 17 atoms / cm 3 ~1×10 18 atoms / cm 3 .
5. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The Ga-containing nitride of the first C-doped Ga-containing nitride layer is one of GaN, AlGaN, InGaN, AlInGaN, BGaN, and BInGaN.
6. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The thickness of the first C-doped Ga-containing nitride layer is 0.1 μm to 2 μm; The C doping concentration of the first C-doped Ga-containing nitride layer is 1×10 16 atoms / cm 3 ~1×10 18 atoms / cm 3 .
7. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The Ga-containing nitride of the second C-doped Ga-containing nitride layer is one of GaN, AlGaN, InGaN, AlInGaN, BGaN, and BInGaN.
8. The light emitting diode epitaxial wafer according to claim 1, characterized in that: The thickness of the second C-doped Ga-containing nitride layer is 0.1 μm to 2 μm; The C doping concentration of the second C-doped Ga-containing nitride layer is 1×10 16 atoms / cm 3 ~1×10 17 atoms / cm 3 .
9. A method for preparing a light emitting diode epitaxial wafer according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1. providing a substrate; S2, depositing a buffer layer, a SiN layer, a three-dimensional nucleation layer, an undoped GaN layer, an N-type GaN layer, an active layer, an electron blocking layer, and a P-type GaN layer on the substrate in sequence; The three-dimensional nucleation layer includes a C / Mg co-doped nitride layer, a first C-doped Ga-containing nitride layer, and a second C-doped Ga-containing nitride layer stacked in sequence, and the C doping concentration of the C / Mg co-doped nitride layer is greater than the C doping concentration of the first C-doped Ga-containing nitride layer and is greater than the C doping concentration of the second C-doped Ga-containing nitride layer.
10. An LED, characterized in that: The LED comprises the light emitting diode epitaxial wafer as described in any one of claims 1 to 8.
Citation Information
Patent Citations
High-resistance III-nitride semiconductor epitaxial structure and method for preparing same
CN108110048A
Epitaxial wafer of light emitting diode, and preparation method thereof
CN109509820A
Epitaxial structure of high electron mobility transistor and preparation method thereof
CN117727782A
Epitaxial structure for GaN power device and growth method thereof
CN117766570A
Doped buffer layer for group iii-v devices on silicon
US20200075314A1