Production technology of wear-resistant control valves by plasma cladding coupled with external field treatment

Through the plasma cladding coupling external field treatment process, nano-oxide hardened layer and high-density dislocation fine crystal layer are formed, which solves the problem of peeling off the hardened layer on the surface of the wear-resistant control valve, improves wear resistance and service performance, and extends the use Lifespan and reduce thermal conductivity.

CN118704005BActive Publication Date: 2024-11-05SICHUAN SUKE FLUID CONTROL EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411197494.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-05
Estimated Expiration
2044-08-29

Smart Images

  • Figure CN118704005B_ABST
    Figure CN118704005B_ABST
Patent Text Reader

Abstract

The present invention belongs to the fields of advanced manufacturing, new materials, surface engineering and new energy, and discloses a production process for wear-resistant control valves by plasma cladding coupled with external field treatment, which is characterized by preparing metal-ceramic composite powder feed, and performing plasma cladding treatment on the opening and closing parts and valve seat surfaces of the wear-resistant control valve, thereby forming a hardened layer containing dispersedly distributed nano-oxides and interface phases on the surface of the wear-resistant control valve, and then performing laser shock treatment to achieve grain refinement and strengthening of the surface layer, and finally performing pulse electromagnetic field treatment to produce high-density dislocations, grain refinement and phase change to further strengthen the surface layer and reduce thermal conductivity. The production process for wear-resistant control valves by plasma cladding coupled with external field treatment of the present invention can effectively improve the surface hardness and wear resistance of the wear-resistant control valve, and the surface hardened layer has low porosity, high bonding strength and low thermal conductivity, and can be used for surface hardening of wear-resistant control valves in silicon chemical industry, coal chemical industry and other industries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a production process for a wear-resistant control valve, in particular to a production process for a wear-resistant control valve using plasma cladding coupled with external field treatment, and belongs to the fields of advanced manufacturing, new materials, surface engineering and new energy. Background Art

[0002] Wear-resistant control valves are widely used in silicon chemical industry, coal chemical industry, petrochemical industry and other industries. In these fields, the conveyed media usually contain high-hardness solid particles, and also have certain corrosiveness and high temperature. Therefore, in the production process of wear-resistant control valves, surface hardening of the valve opening and closing parts and valve seat sealing surfaces can play a good protective role.

[0003] CN101545546A discloses a tungsten carbide metal ceramic composite wear-resistant ball valve, including a valve ball, a valve seat, and a valve body, characterized in that a tungsten carbide metal ceramic composite wear-resistant coating is sprayed on the inner wall of the flow channel through which the fluid passes, and the sealing surfaces of the valve ball and the valve seat. In order to ensure that the tungsten carbide coating has a high bonding strength with the carbon steel substrate, the parts to be sprayed are firstly injected with tungsten carbide ions before spraying to form a transition layer. In addition, due to the provision of a transition arc surface, the bonding force between the tungsten carbide coating and the carbon steel body is further guaranteed. However, the ion implantation process will greatly increase the cost, and does not fundamentally solve the problem of heat transfer of the coating. CN115451148A discloses a wear-resistant ball valve and a method for spraying a tungsten carbide and DLC composite coating. The invention provides a convex ridge on the spherical surface of the valve core, thereby reducing the pressure of the sealing ring contacting the valve core surface when the valve core changes state, thereby reducing the friction between the sealing ring and the valve core, greatly improving the wear resistance of the valve core, and combining the spraying of the tungsten carbide and DLC composite coating on the convex ridge, which is more conducive to extending the service life of the valve core.

[0004] As the service conditions of wear-resistant control valves become increasingly harsh, the existing surface hardening treatment methods can no longer meet the service requirements of wear-resistant control valves. The opening and closing parts and valve seats of wear-resistant control valves are in contact with high-hardness solid particles and are prone to surface wear. In high-temperature media, the thermal expansion coefficients of the surface hardened layer and the substrate are quite different, which will form residual stress at the interface. Under the contact stress during the opening and closing process, the hardened layer is prone to peeling, which eventually leads to damage to the sealing surface between the opening and closing parts and the valve seat, and seal failure. Therefore, it is very necessary to develop a new production process for wear-resistant control valves, which can achieve excellent wear resistance, bonding strength and the ability to serve in harsh conditions through surface hardening and structural regulation. Summary of the invention

[0005] The present invention aims to provide a production process for wear-resistant control valves by plasma cladding coupled with external field treatment, so as to improve the wear resistance of the surface, the coating bonding performance and the service performance in harsh working conditions. The present invention proposes to prepare a metal-ceramic composite powder feed, and to perform plasma cladding treatment on the opening and closing parts and the valve seat surface of the wear-resistant control valve, so as to form a hardened layer containing dispersed nano-oxides and interface phases on the surface of the wear-resistant control valve, and then to perform laser shock treatment to achieve grain refinement and strengthening of the surface layer, and finally to perform pulsed electromagnetic field treatment to produce high-density dislocations, grain refinement and phase change to further strengthen the surface layer and reduce the thermal conductivity, and to produce a wear-resistant control valve with a hardened layer of high hardness, wear resistance, low thermal conductivity and high bonding strength on the surface after assembly with other accessories.

[0006] The plasma cladding coupled external field treatment wear-resistant control valve production process of the present invention comprises the following steps in sequence:

[0007] (1) Preparation of metal-ceramic composite slurry for plasma cladding of wear-resistant control valves: First, C 18 H 29 NaO 3 S, isopropanol, cyclohexane added to deionized water, by weight percentage C 18 H 29 NaO 3 S accounts for 15% to 30%, isopropanol accounts for 6% to 16%, cyclohexane accounts for 5% to 15%, and the rest is ionized water. Stir with a magnetic stirrer at 60 to 90 ° C for 3 to 10 hours, and then leave it for 6 to 12 hours to form a reverse microemulsion. Use the reverse microemulsion as the solvent and add C 16 H 36 O 4 Ti, the concentration is 0.5-1 mol / L, and then ammonia water is added to adjust the solution pH to 8-9, and stirred at 60-90℃ for 3-6 hours with a magnetic stirrer, and then left for 3-6 hours to form Ti(OH) 4 Sol; C 15 H 35 MoO 5 As raw material, using Ti(OH) 4 Mo(OH) was prepared with the same parameters as the sol 6 Sol; weigh the prepared Mo(OH) 6 Sol, Ti(OH) 4 Sol, (Ti, W) C powder with an average particle size D50 of 2.6~3.0μm, Co powder with an average particle size D50 of 1.0~1.2μm, Re powder with an average particle size D50 of 2.0~4.0μm are used as raw materials for mixing, and the Co element accounts for 10~15% by mole percentage, the Re element accounts for 30~50% of the Co element, and the Mo element accounts for 1~5% by mole percentage. 6Sol, weigh Ti(OH) based on Ti element accounting for 3~6% 4 sol, the rest is (Ti, W)C; firstly, Mo(OH) 6 Sol and (Ti, W) C are mixed, and then 0.5~1% of the total weight of the mixture is added. 18 H 34 O 2 and 1-2% PEG2000 by weight, and stirred magnetically for 30-60 min, then ammonia water was added to adjust the pH value of the mixture to 8-9, and the Zeta potential of the mixture was 22-34 mV, so that Mo(OH) 6 Coated on the surface of (Ti, W) C; then add Co powder and Re powder for ball milling, the ball-to-material weight ratio during ball milling is 10:1, WC-Co carbide grinding balls with a diameter of 6-10 mm are used, the ball milling time is 24-36 hours, and the ball milling speed is 300-400 r / min; after the ball milling, a 400-mesh screen is used for filtration to prepare a product with the surface coated with Mo(OH) 6 Metal-ceramic composite slurry for plasma cladding composed of (Ti, W) C, Co, Re powders;

[0008] (2) Preparation of metal-ceramic composite powder feed for plasma cladding of wear-resistant control valves: First, the metal-ceramic composite slurry is spray dried. During spray drying, the atomizing disk speed is 5000~7000r / min and the drying temperature is 120~130℃. After spray drying, the powder agglomerates are placed in a vacuum sintering furnace and sintered at 1100~1200℃ for 60~90min. The initial vacuum degree of sintering is 1~5Pa and the heating rate is 5℃ / min. After sintering, spherical powder agglomerates with a particle size of 35~45μm are formed through crushing and airflow classification. Then, all the spherical powder agglomerates are immersed in Ti(OH) 4 The sol is dried at 100-110℃, and after 10-20 times of impregnation and drying, the Ti(OH) 4 The sol is completely immersed in the pores of the spherical powder agglomerates to prepare a metal-ceramic composite powder feed for plasma cladding of a wear-resistant control valve, and its phase composition is (Ti, W) C phase with NaCl structure + MoO coated on the surface of (Ti, W) C phase. 3 Orthorhombic phase + Ti(OH) 4 Gel + Co phase + Re phase, HCP:FCC in Co phase = 0.2~0.3, (Ti,W)C particle size is 2.2~2.5μm;

[0009] (3) Plasma cladding surface hardening treatment of wear-resistant control valve: First, the opening and closing parts and valve seat surfaces of the wear-resistant control valve are ground to make their surface roughness Ra0.6~0.8μm, and the prepared metal ceramic composite powder is used to feed the opening and closing parts and valve seat surfaces of the wear-resistant control valve for plasma cladding surface hardening treatment. The working voltage is 20~24V, the working current is 100~240A, the ionization gas argon flow rate is 10~13L / min, the protective gas argon flow rate is 13~15L / min, the scanning rate is 10~15cm / min, and the coaxial powder feeding is used with a powder feeding rate of 8~10g / min. During the plasma cladding process, MoO coated on the surface of the (Ti,W)C phase 3 It undergoes solid solution reaction and carbon thermal reduction with (Ti, W) C to transform into (Ti, W, Mo) C interfacial phase in situ and still covers the (Ti, W) C surface. The thickness of (Ti, W, Mo) C interfacial phase is 0.1~0.3 μm and the grain size and phase remain unchanged in subsequent treatment. Ti(OH) 4 The gel is transformed into dispersed nano-TiO with a particle size of 50-90 nm. 2 , nano-TiO 2 In the subsequent treatment, the grain size and phase remain unchanged, Re dissolves in Co and promotes the martensitic transformation from FCC to HCP in the Co phase and the grain refinement of the (Ti, W) C phase. The plasma cladding forms a surface hardening layer containing an interface phase and oxides. The grain size of (Ti, W) C in the surface hardening layer is 1.8-2.0 μm, the porosity is 0.1-0.5%, the thickness is 600-1200 μm, and the phase composition is (Ti, W) C phase with NaCl structure + (Ti, W, Mo) C interface phase with NaCl structure coated on the surface of (Ti, W) C phase + TiO with rutile structure 2 phase + CoRe solid solution bonding phase, HCP:FCC in CoRe bonding phase = 0.4~0.7; the composition of the surface hardening layer is Co accounting for 10~15% by mole percentage, Re accounting for 30~50% of Co, (Ti, W, Mo) C accounting for 1~5%, TiO 2 3-6% and the rest is (Ti, W) C; the dislocation density in the plasma cladding hardened layer is 1×10 7 ~6×10 7 mm -2 , the dislocation density in the steel matrix is ​​3×10 6 ~7×10 6 mm -2 The plasma cladding hardened layer is metallurgically bonded to the opening and closing parts and the valve seat substrate. There is a transition zone with a thickness of 40-50 μm between the two, and its phase composition is α-Fe+(Ti, W)C+CoRe solid solution+(Ti, W, Mo)C;

[0010] (4) Formation of a fine-grained layer on the surface of the plasma cladding hardened layer: First, polydimethylsiloxane with a viscosity of 1500~3000cps, blocked isocyanate and dibutyltin dilaurate are mixed into a glue solution in a volume ratio of 100:(0.8~1.5):(0.1~0.3), stirred for 10~20min, and subjected to high-speed centrifugal degassing treatment. The speed of the centrifugal degassing treatment is 600~1000r / min, and the centrifugal time is 5~10min. The glue solution is injected into the mold and cured at 50~60℃ to form a transparent silicone gel film with a thickness of 1.0~1.3mm; then the opening and closing parts and valve seats after plasma cladding hardening treatment are finely ground to a roughness of Ra0.2~0.4μm. The surface of the prepared plasma cladding hardened layer was sprayed with black paint as an absorption layer, and then cooled to -190°C in liquid nitrogen and maintained for 30 to 60 minutes. After being taken out, a silicone gel film was attached to the surface of the black paint absorption layer as a constraint layer. The plasma cladding hardened layer attached with the silicone gel film was subjected to laser shock treatment within 3 to 5 minutes. The laser wavelength was 1.064 μm, the laser spot diameter was 1 to 4 mm, the spot overlap rate was 20 to 60%, the pulse energy was 10 to 15 J, and the pulse width was 15 to 25 ns. During the laser treatment, plasma was generated between the constraint layer and the absorption layer, and its shock wave formed a high dislocation density fine crystal layer on the surface of the plasma cladding hardened layer; the high-density dislocation fine crystal layer had a thickness of 20 to 50 μm, and its dislocation density increased to 2×10 9 ~6×10 9 mm -2 Its surface is in a compressive stress state. After liquid nitrogen cooling and laser shock hot and cold cycles, the grain size of (Ti, W) C is 1.3~1.6μm, and the CoRe bonding phase undergoes a martensitic phase transformation, where HCP:FCC=0.8~1.0; except for the surface high dislocation density fine grain layer in the plasma cladding hardened layer, the dislocation density, phase composition, and grain size of the steel matrix remain unchanged;

[0011] (5) Dislocation density and phase regulation based on external field treatment and wear-resistant control valve manufacturing: The plasma cladding hardened layer with a high dislocation density fine-grained layer on the surface was treated with a pulsed electromagnetic field. The intensity of the pulsed magnetic field was 0.5-1.5 T, the magnetic pulse frequency was 1-5 Hz, the number of magnetic pulses was 30-40, the electric field intensity was 1-2 V, the frequency of the electric pulse was 50 Hz, and the number of electric pulses was 5-10. The pulsed electromagnetic field treatment caused the CoRe bonding phase in the plasma cladding hardened layer to continue to transform from FCC to HCP, the dislocation density increased, and the grains were refined. After the pulsed electromagnetic field treatment, the HCP of the CoRe bonding phase in the plasma cladding hardened layer except for the surface high-density fine-grained layer was FCC = 0.8-1.0, and the dislocation density increased to 1×10 8 ~8×10 8mm -2 , the grain size of (Ti,W)C is reduced to 1.4~1.7μm; the HCP:FCC of CoRe bonding phase in the fine-grained layer with high dislocation density on the surface of plasma cladding hardened layer is 1.3~1.4, and the dislocation density increases to 3×10 10 ~9×10 10 mm -2 , the grain size of (Ti,W)C decreased to 1.0~1.2μm; the dislocation density in the steel matrix increased to 1×10 7 ~7×10 7 mm -2 ; After the pulse electromagnetic field treatment, the dislocation density and phase regulation are completed; the opening and closing parts and valve seats of the wear-resistant control valve treated by the external field are ground and assembled with the matching valve body, valve stem, valve cover and spring to manufacture the wear-resistant control valve. The hardness of the surface hardening layer of the opening and closing parts and valve seats is ≧950HV, the coating bonding strength is ≧420MPa, and the wear rate is ≦4×10 -6 mm 3 / (N·mm), thermal conductivity is 30~40W·m -1 ·K -1 The maximum service temperature of the wear-resistant control valve is 660℃.

[0012] The wear-resistant control valve of the present invention is subjected to plasma cladding coupled external field treatment, and the surfaces of the opening and closing parts and the valve seat have a phase composition of a (Ti, W) C phase with a NaCl structure + a (Ti, W, Mo) C interface phase coated on the surface of the (Ti, W) C phase and having a NaCl structure + a TiO 2 The plasma cladding hardened layer is composed of a phase + CoRe solid solution bonding phase, and the HCP:FCC in the CoRe bonding phase is 0.4~0.7; the composition of the surface hardened layer is 10~15% Co, 30~50% Re, 1~5% (Ti, W, Mo)C, and TiO 2 The thickness of the (Ti, W, Mo) C interface phase is 0.1~0.3μm, and the thickness of TiO 2 The grain size is 50~90nm; the porosity of the surface hardened layer is 0.1~0.5%, the total thickness is 600~1200μm, and the surface layer is a high dislocation density fine crystal layer with a thickness of 20~50μm; the HCP:FCC of the CoRe bonding phase in the plasma cladding hardened layer except the surface high density fine crystal layer is 0.8~1.0, and the dislocation density increases to 1×10 8 ~8×10 8 mm -2, the grain size of (Ti,W)C is reduced to 1.4~1.7μm; the HCP:FCC of CoRe bonding phase in the fine-grained layer with high dislocation density on the surface of plasma cladding hardened layer is 1.3~1.4, and the dislocation density increases to 3×10 10 ~9×10 10 mm -2 , the grain size of (Ti, W) C is reduced to 1.0~1.2μm; the plasma cladding hardened layer is metallurgically bonded with the opening and closing parts and the valve seat substrate, and there is a transition zone with a thickness of 40~50μm between the two. Its phase composition is α-Fe+(Ti, W) C+CoRe solid solution+(Ti, W, Mo) C; the hardness of the opening and closing parts and the valve seat surface hardened layer is ≧950HV, the coating bonding strength is ≧420MPa, and the wear rate is ≦4×10 -6 mm 3 / (N·mm), thermal conductivity is 30~40W·m -1 ·K -1 The maximum service temperature of the wear-resistant control valve is 660℃.

[0013] The advantages of the present invention are: (1) The wear-resistant control valve produced by the present invention based on plasma cladding coupled external field treatment uses laser impact and external field treatment to form high-density dislocations in the material as microstructural defects. The dislocations strengthen the surface hardened layer, thereby improving the hardness and wear resistance. (2) The wear-resistant control valve produced by the present invention based on plasma cladding coupled external field treatment has a metallurgical bond between the surface hardened layer and the substrate, forming a special interface transition layer. The bonding strength between the surface hardened layer and the substrate is high and the porosity is low. (3) In the surface hardened layer of the wear-resistant control valve produced by the present invention based on plasma cladding coupled external field treatment, a (Ti, W, Mo) C interface phase with a NaCl structure is formed, which can not only improve the interface wettability and reduce the porosity of the coating, but also strengthen the surface hardened layer, thereby improving its hardness and wear resistance. (4) The present invention introduces Re element into the wear-resistant control valve produced by plasma cladding coupled with external field treatment, combines the subsequent formation of a surface fine-grained layer with high dislocation density and the control of dislocation density and phase under the action of external field, refines the grains of the hardened layer, and improves the hardness and wear resistance. (5) In the present invention, the Co phase undergoes a martensitic phase transformation, and the FCC transforms to the HCP, so that the bonding phase of the plasma cladding layer is strengthened, and the hardness and wear resistance are improved. (5) In the present invention, Mo(OH) 6 The coated (Ti,W)C undergoes carbothermal reduction reaction, while Ti(OH) 4 It will not be carbonized during the thermal spraying process, thus forming a dispersed TiO with low thermal conductivity. 2Nanophase plays a role in dispersion strengthening of the plasma cladding layer. (6) The surface hardened layer in the present invention has good wear resistance, the surface is in a compressive stress state, and will not reduce the mechanical properties of the base material, which is beneficial to improving the service life of wear-resistant control valve parts. (7) The wear-resistant control valve produced by the present invention based on plasma cladding coupled external field treatment, the formed nano-TiO 2 , (Ti, W, Mo)C interface phase, HCP phase, high-density dislocations and interfaces, which hinder and scatter phonons during propagation, reduce the mean free path of phonons, and thus reduce the thermal conductivity of the hardened layer, thereby reducing the heat transfer between the wear-resistant control valve substrate and the high-temperature medium, avoiding excessive thermal expansion of the substrate, alleviating the residual stress between the coating and the substrate, and avoiding coating peeling. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 Schematic diagram of the production process of wear-resistant control valves by plasma cladding coupled with external field treatment of the present invention.

[0015] Figure 2 Schematic diagram of the opening and closing parts and valve seat characteristics of the wear-resistant control valve of the present invention. DETAILED DESCRIPTION

[0016] Example 1:

[0017] A plasma cladding coupled external field treatment wear-resistant control valve production process, such as Figure 1 As shown, the following steps are included in sequence:

[0018] (1) Preparation of metal-ceramic composite slurry for plasma cladding of wear-resistant control valves: First, C 18 H 29 NaO 3 S, isopropanol, cyclohexane added to deionized water, by weight percentage C 18 H 29 NaO 3 S accounts for 16%, isopropanol accounts for 7%, cyclohexane accounts for 5%, and the rest is ionized water. Stir with a magnetic stirrer at 60°C for 3 hours, then leave it for 8 hours to form a reverse microemulsion. Use the reverse microemulsion as the solvent and add C 16 H 36 O 4 Ti, the concentration of which was 0.5 mol / L, was then added with ammonia water to adjust the solution pH to 8, stirred at 65 ° C for 3 h with a magnetic stirrer, and then left for 4 h to form Ti(OH) 4 Sol; C 15 H 35 MoO 5 As raw material, using Ti(OH) 4 Mo(OH) was prepared with the same parameters as the sol 6Sol; weigh the prepared Mo(OH) 6 Sol, Ti(OH) 4 Sol, (Ti, W) C powder with an average particle size D50 of 2.6 μm, Co powder with an average particle size D50 of 1.1 μm, and Re powder with an average particle size D50 of 2.0 μm are used as raw materials for mixing. By molar percentage, Co element accounts for 10%, Re element accounts for 35% of Co element, and Mo element accounts for 2%. Mo(OH) 6 Sol, weigh Ti(OH) based on the Ti element accounting for 3% 4 sol, the rest is (Ti, W)C; firstly, Mo(OH) 6 Sol and (Ti, W) C are mixed, and then 0.5% of the total weight of the mixture is added to C 18 H 34 O 2 and 1.2% PEG2000 by total weight, and stirred magnetically for 35 min, then ammonia water was added to adjust the pH value of the mixture to 8, and the Zeta potential of the mixture was 24 mV, so that Mo(OH) 6 Coated on the surface of (Ti, W) C; then Co powder and Re powder were added for ball milling, the ball-to-material weight ratio during ball milling was 10:1, WC-Co carbide grinding balls with a diameter of 6 mm were used, the ball milling time was 24 hours, and the ball milling speed was 350 r / min; after the ball milling was completed, a 400-mesh sieve was used for filtration to prepare a product with the surface coated with Mo(OH) 6 Metal-ceramic composite slurry for plasma cladding composed of (Ti, W) C, Co, Re powders;

[0019] (2) Preparation of metal-ceramic composite powder feed for plasma cladding of wear-resistant control valves: First, the metal-ceramic composite slurry was spray dried. During spray drying, the atomizing disk speed was 5500r / min and the drying temperature was 120℃. After spray drying, the powder agglomerates were placed in a vacuum sintering furnace and sintered at 1100℃ for 70min. The initial vacuum degree of sintering was 2Pa and the heating rate was 5℃ / min. After sintering, they were crushed and air flow classified to form spherical powder agglomerates with a particle size of 42μm. Then, all the spherical powder agglomerates were immersed in Ti(OH) 4 Sol and dried at 100℃, after 10 times of impregnation and drying, the Ti(OH) 4 The sol is completely immersed in the pores of the spherical powder agglomerates to prepare a metal-ceramic composite powder feed for plasma cladding of a wear-resistant control valve, and its phase composition is (Ti, W) C phase with NaCl structure + MoO coated on the surface of (Ti, W) C phase. 3 Orthorhombic phase + Ti(OH) 4Gel + Co phase + Re phase, HCP:FCC in Co phase = 0.22, (Ti,W)C particle size is 2.3 μm;

[0020] (3) Plasma cladding surface hardening treatment of wear-resistant control valve: The opening and closing parts and valve seat surfaces of the wear-resistant control valve were first ground to a surface roughness of Ra0.6μm, and the prepared metal ceramic composite powder was fed to the opening and closing parts and valve seat surfaces of the wear-resistant control valve for plasma cladding surface hardening treatment. The working voltage was 20V, the working current was 120A, the ionized gas argon flow rate was 11L / min, the protective gas argon flow rate was 13L / min, the scanning rate was 10cm / min, and the coaxial powder feeding was used with a powder feeding rate of 8g / min. During the plasma cladding process, the MoO coated on the surface of the (Ti,W)C phase 3 It undergoes solid solution reaction with (Ti, W) C and carbon thermal reduction to transform into (Ti, W, Mo) C interfacial phase in situ and still covers the (Ti, W) C surface. The thickness of (Ti, W, Mo) C interfacial phase is 0.12 μm and the grain size and phase remain unchanged in subsequent treatment. Ti(OH) 4 The gel transforms into dispersed nano-TiO with a particle size of 55 nm. 2 , nano-TiO 2 In the subsequent treatment, the grain size and phase remain unchanged, Re dissolves in Co and promotes the martensitic transformation from FCC to HCP in the Co phase and the grain refinement of the (Ti, W) C phase. Plasma cladding forms a surface hardening layer containing an interface phase and oxides. The grain size of (Ti, W) C in the surface hardening layer is 1.8 μm, the porosity is 0.3%, the thickness is 1120 μm, and the phase composition is (Ti, W) C phase with NaCl structure + (Ti, W, Mo) C interface phase with NaCl structure coated on the surface of (Ti, W) C phase + TiO with rutile structure 2 phase + CoRe solid solution bonding phase, HCP:FCC in CoRe bonding phase = 0.48; the composition of the surface hardening layer is 10% Co, 35% Re, 2% (Ti, W, Mo) C, and 2% TiO 2 3%, and the rest is (Ti, W) C; the dislocation density in the plasma cladding hardened layer is 2×10 7 mm -2 , the dislocation density in the steel matrix is ​​4×10 6 mm -2 ; The plasma cladding hardened layer is metallurgically bonded to the opening and closing parts and the valve seat substrate. There is a transition zone with a thickness of 42μm between the two, and its phase composition is α-Fe+(Ti,W)C+CoRe solid solution+(Ti,W,Mo)C;

[0021] (4) Formation of a fine-grained layer on the surface of the plasma cladding hardened layer: First, polydimethylsiloxane with a viscosity of 1500cps, blocked isocyanate and dibutyltin dilaurate were mixed into a glue solution in a volume ratio of 100:0.8:0.1, stirred for 10 minutes, and subjected to high-speed centrifugal degassing treatment. The speed of the centrifugal degassing treatment was 700r / min and the centrifugal time was 5 minutes. The glue solution was injected into the mold and cured at 50°C to form a transparent silicone gel film with a thickness of 1.1mm. Then, the opening and closing parts and valve seats after the plasma cladding hardening treatment were finely ground to a roughness of Ra0.2μm. The surface of the cladding layer was sprayed with black paint as an absorption layer, and then cooled to -190 °C in liquid nitrogen and kept for 30 min. After being taken out, the organic silicone gel film was attached to the surface of the black paint absorption layer as a constraint layer. The plasma cladding hardened layer attached with the organic silicone gel film was subjected to laser shock treatment within 3 min. The laser wavelength was 1.064 μm, the laser spot diameter was 2 mm, the spot overlap rate was 25%, the pulse energy was 10 J, and the pulse width was 15 ns. During the laser treatment, plasma was generated between the constraint layer and the absorption layer, and its shock wave formed a high dislocation density fine crystal layer on the surface of the plasma cladding hardened layer; the high-density dislocation fine crystal layer was 22 μm thick, and its dislocation density increased to 3×10 9 mm -2 The surface is in a compressive stress state. After liquid nitrogen cooling and laser shock hot and cold cycles, the grain size of (Ti, W) C is 1.3 μm, and the CoRe bonding phase undergoes a martensitic phase transformation, where HCP: FCC = 0.84; except for the surface high dislocation density fine-grained layer in the plasma cladding hardened layer, the dislocation density, phase composition, and grain size of the steel matrix remain unchanged;

[0022] (5) Dislocation density and phase regulation based on external field treatment and wear-resistant control valve manufacturing: The plasma cladding hardened layer with a high dislocation density fine-grained layer on the surface was treated with a pulsed electromagnetic field. The intensity of the pulsed magnetic field was 0.5 T, the magnetic pulse frequency was 1 Hz, the number of magnetic pulses was 30, the electric field intensity was 1 V, the frequency of the electric pulse was 50 Hz, and the number of electric pulses was 5. The pulsed electromagnetic field treatment caused the CoRe bonding phase in the plasma cladding hardened layer to continue to transform from FCC to HCP, the dislocation density increased, and the grains were refined. The HCP of the CoRe bonding phase in the plasma cladding hardened layer except for the surface high-density fine-grained layer was FCC=0.82, and the dislocation density increased to 3×10 8 mm -2 , the grain size of (Ti,W)C is reduced to 1.5μm; the HCP:FCC of CoRe binder phase in the fine-grained layer with high dislocation density on the surface of plasma cladding hardened layer is 1.32, and the dislocation density increases to 3.5×10 10 mm -2, the grain size of (Ti,W)C decreased to 1.1μm; the dislocation density in the steel matrix increased to 2.2×10 7 mm -2 ; After pulse electromagnetic field treatment, dislocation density and phase regulation are completed; the characteristics of the opening and closing parts and valve seats of the wear-resistant control valve are as follows Figure 2 As shown in the figure, the wear-resistant control valve opening and closing parts and valve seats that have been treated in the field are ground and assembled with the matching valve body, valve stem, valve cover and spring to manufacture a wear-resistant control valve. The hardness of the surface hardening layer of the opening and closing parts and valve seats is 980HV, the coating bonding strength is 460MPa, and the wear rate is 3×10 -6 mm 3 / (N·mm), thermal conductivity is 38W·m -1 ·K -1 The maximum service temperature of the wear-resistant control valve is 660℃.

[0023] The wear-resistant control valve of the present invention is subjected to plasma cladding coupled external field treatment, and the surfaces of the opening and closing parts and the valve seat have a phase composition of a (Ti, W) C phase with a NaCl structure + a (Ti, W, Mo) C interface phase coated on the surface of the (Ti, W) C phase and having a NaCl structure + a TiO 2 The plasma cladding hardened layer of the phase + CoRe solid solution bonding phase; the composition of the surface hardened layer is 10% Co, 35% Re, 2% (Ti, W, Mo) C, and 2% TiO 2 The thickness of the (Ti, W, Mo) C interface phase is 0.12 μm, and the thickness of TiO 2 The grain size is 55nm; the porosity of the surface hardened layer is 0.3%, the total thickness is 1120μm, and the surface layer is a high dislocation density fine-grained layer with a thickness of 22μm; the HCP:FCC of the CoRe bonding phase in the plasma cladding hardened layer except the surface high-density fine-grained layer is 0.82, and the dislocation density increases to 3×10 8 mm -2 , the grain size of (Ti,W)C is reduced to 1.5μm; the HCP:FCC of CoRe binder phase in the fine-grained layer with high dislocation density on the surface of plasma cladding hardened layer is 1.32, and the dislocation density increases to 3.5×10 10 mm -2 , the grain size of (Ti, W) C is reduced to 1.1 μm; the plasma cladding hardened layer is metallurgically bonded with the opening and closing parts and the valve seat substrate, and there is a transition zone with a thickness of 42 μm between the two. Its phase composition is α-Fe+(Ti, W) C+CoRe solid solution+(Ti, W, Mo) C; the hardness of the opening and closing parts and the valve seat surface hardened layer is 980 HV, the coating bonding strength is 460 MPa, and the wear rate is 3×10 -6 mm 3 / (N·mm), thermal conductivity is 38W·m -1 ·K -1 The maximum service temperature of the wear-resistant control valve is 660℃.

[0024] Example 2:

[0025] A plasma cladding coupled external field treatment wear-resistant control valve production process, such as Figure 1 As shown, the following steps are included in sequence:

[0026] (1) Preparation of metal-ceramic composite slurry for plasma cladding of wear-resistant control valves: First, C 18 H 29 NaO 3 S, isopropanol, cyclohexane added to deionized water, by weight percentage C 18 H 29 NaO 3 S accounts for 20%, isopropanol accounts for 16%, cyclohexane accounts for 10%, and the rest is ionized water. Stir with a magnetic stirrer at 80°C for 8 hours, then leave it for 12 hours to form a reverse microemulsion. Use the reverse microemulsion as the solvent and add C 16 H 36 O 4 Ti, the concentration is 1 mol / L, and then ammonia water is added to adjust the solution pH to 9, stirred at 80 ° C for 6 hours with a magnetic stirrer, and then left for 5 hours to form Ti(OH) 4 Sol; C 15 H 35 MoO 5 As raw material, using Ti(OH) 4 Mo(OH) was prepared with the same parameters as the sol 6 Sol; weigh the prepared Mo(OH) 6 Sol, Ti(OH) 4 Sol, (Ti, W) C powder with an average particle size D50 of 2.8 μm, Co powder with an average particle size D50 of 1.2 μm, and Re powder with an average particle size D50 of 3.0 μm are used as raw materials for mixing. By molar percentage, Co element accounts for 15%, Re element accounts for 40% of Co element, and Mo element accounts for 5%. Mo(OH) 6 Sol, weigh Ti(OH) based on 5% Ti element 4 sol, the rest is (Ti, W)C; firstly, Mo(OH) 6 Sol and (Ti, W) C were mixed, and then 0.8% of the total weight of the mixture was added to C 18 H 34 O 2and 2% PEG2000 by weight, and stirred magnetically for 60 min, then ammonia water was added to adjust the pH value of the mixture to 9, and the Zeta potential of the mixture was 31 mV, making Mo(OH) 6 Coated on the surface of (Ti, W) C; then added Co powder and Re powder for ball milling, the ball-to-material weight ratio during ball milling was 10:1, WC-Co carbide grinding balls with a diameter of 10 mm were used, the ball milling time was 30 hours, and the ball milling speed was 380 r / min; after the ball milling was completed, a 400-mesh sieve was used for filtration to prepare a product with the surface coated with Mo(OH) 6 Metal-ceramic composite slurry for plasma cladding composed of (Ti, W) C, Co, Re powders;

[0027] (2) Preparation of metal-ceramic composite powder feed for plasma cladding of wear-resistant control valves: First, the metal-ceramic composite slurry is spray dried. During spray drying, the atomizing disk speed is 6000r / min and the drying temperature is 130℃. After spray drying, the powder agglomerates are placed in a vacuum sintering furnace and sintered at 1200℃ for 80min. The initial vacuum degree of sintering is 4Pa and the heating rate is 5℃ / min. After sintering, they are crushed and air-graded to form spherical powder agglomerates with a particle size of 38μm. Then, all the spherical powder agglomerates are immersed in the Ti(OH) 4 Sol and dried at 110℃, after 20 times of impregnation and drying, the Ti(OH) 4 The sol is completely immersed in the pores of the spherical powder agglomerates to prepare a metal-ceramic composite powder feed for plasma cladding of a wear-resistant control valve, and its phase composition is (Ti, W) C phase with NaCl structure + MoO coated on the surface of (Ti, W) C phase. 3 Orthorhombic phase + Ti(OH) 4 Gel + Co phase + Re phase, HCP:FCC in Co phase = 0.3, (Ti,W)C particle size is 2.4μm;

[0028] (3) Plasma cladding surface hardening treatment of wear-resistant control valve: The opening and closing parts and valve seat surfaces of the wear-resistant control valve were first ground to a surface roughness of Ra0.8μm, and the prepared metal-ceramic composite powder was fed to the opening and closing parts and valve seat surfaces of the wear-resistant control valve for plasma cladding surface hardening treatment. The working voltage was 22V, the working current was 200A, the ionization gas argon flow rate was 12L / min, the protective gas argon flow rate was 15L / min, the scanning rate was 15cm / min, and the coaxial powder feeding was used with a powder feeding rate of 10g / min. During the plasma cladding process, the MoO coated on the surface of the (Ti,W)C phase 3It undergoes solid solution reaction with (Ti, W) C and carbon thermal reduction to transform into (Ti, W, Mo) C interfacial phase in situ and still covers the (Ti, W) C surface. The thickness of (Ti, W, Mo) C interfacial phase is 0.26 μm and the grain size and phase remain unchanged in subsequent treatments. Ti(OH) 4 The gel transforms into dispersed nano-TiO with a particle size of 82 nm. 2 , nano-TiO 2 In the subsequent treatment, the grain size and phase remain unchanged, Re dissolves in Co and promotes the martensitic transformation from FCC to HCP in the Co phase and the grain refinement of the (Ti, W) C phase. Plasma cladding forms a surface hardening layer containing an interface phase and oxides. The grain size of (Ti, W) C in the surface hardening layer is 1.9 μm, the porosity is 0.2%, and the thickness is 680 μm. The phase composition is (Ti, W) C phase with NaCl structure + (Ti, W, Mo) C interface phase with NaCl structure coated on the surface of (Ti, W) C phase + TiO with rutile structure 2 phase + CoRe solid solution bonding phase, HCP:FCC in CoRe bonding phase = 0.67; the composition of the surface hardening layer is 15% Co, 50% Re, 5% (Ti, W, Mo) C, and 5% TiO 2 5%, and the rest is (Ti, W) C; the dislocation density in the plasma cladding hardened layer is 5×10 7 mm -2 , the dislocation density in the steel matrix is ​​6×10 6 mm -2 ; The plasma cladding hardened layer is metallurgically bonded to the opening and closing parts and the valve seat substrate. There is a transition zone with a thickness of 46μm between the two, and its phase composition is α-Fe+(Ti,W)C+CoRe solid solution+(Ti,W,Mo)C;

[0029] (4) Formation of fine crystal layer on the surface of plasma cladding hardened layer: First, polydimethylsiloxane with a viscosity of 000cps, blocked isocyanate and dibutyltin dilaurate were mixed into a glue solution in a volume ratio of 100:1:0.3, stirred for 20 minutes, and subjected to high-speed centrifugal degassing treatment. The speed of the centrifugal degassing treatment was 1000r / min and the centrifugal time was 10 minutes. The glue solution was injected into the mold and cured at 60°C to form a transparent silicone gel film with a thickness of 1.2mm. Then, the opening and closing parts and valve seats after plasma cladding hardening treatment were finely ground to a roughness of Ra0.3μm. The surface of the cladding layer was sprayed with black paint as an absorption layer, and then cooled to -190 °C in liquid nitrogen and kept for 50 min. After being taken out, the organic silicone gel film was attached to the surface of the black paint absorption layer as a constraint layer. The plasma cladding hardened layer attached with the organic silicone gel film was subjected to laser shock treatment within 5 min. The laser wavelength was 1.064 μm, the laser spot diameter was 4 mm, the spot overlap rate was 50%, the pulse energy was 15 J, and the pulse width was 20 ns. During the laser treatment, plasma was generated between the constraint layer and the absorption layer, and its shock wave formed a high dislocation density fine crystal layer on the surface of the plasma cladding hardened layer; the high-density dislocation fine crystal layer was 40 μm thick, and its dislocation density increased to 5×10 9 mm -2 The surface is in a compressive stress state. After liquid nitrogen cooling and laser shock hot and cold cycles, the grain size of (Ti, W) C is 1.5 μm, and the CoRe bonding phase undergoes a martensitic phase transformation, where HCP: FCC = 0.92; except for the surface high dislocation density fine-grained layer in the plasma cladding hardened layer, the dislocation density, phase composition, and grain size of the steel matrix remain unchanged;

[0030] (5) Dislocation density and phase regulation based on external field treatment and wear-resistant control valve manufacturing: The plasma cladding hardened layer with a high dislocation density fine-grained layer on the surface was treated with a pulsed electromagnetic field. The intensity of the pulsed magnetic field was 1.5 T, the magnetic pulse frequency was 4 Hz, the number of magnetic pulses was 35, the electric field intensity was 2 V, the frequency of the electric pulse was 50 Hz, and the number of electric pulses was 10. The pulsed electromagnetic field treatment caused the CoRe bonding phase in the plasma cladding hardened layer to continue to transform from FCC to HCP, the dislocation density increased, and the grains were refined. The HCP of the CoRe bonding phase in the plasma cladding hardened layer except for the surface high-density fine-grained layer was FCC = 0.94, and the dislocation density increased to 7 × 10 8 mm -2 , the grain size of (Ti,W)C is reduced to 1.6μm; the HCP:FCC of CoRe bonding phase in the fine-grained layer with high dislocation density on the surface of plasma cladding hardened layer is 1.38, and the dislocation density increases to 8×10 10 mm -2, the grain size of (Ti,W)C decreased to 1.2μm; the dislocation density in the steel matrix increased to 5×10 7 mm -2 ; After the pulse electromagnetic field treatment, the dislocation density and phase regulation are completed; the opening and closing parts and valve seats of the wear-resistant control valve treated by the external field are ground and assembled with the matching valve body, valve stem, valve cover and spring to manufacture the wear-resistant control valve. The hardness of the surface hardening layer of the opening and closing parts and valve seats is 960HV, the coating bonding strength is 430MPa, and the wear rate is 2×10 -6 mm 3 / (N·mm), thermal conductivity is 32W·m -1 ·K -1 The maximum service temperature of the wear-resistant control valve is 660℃.

[0031] The wear-resistant control valve of the present invention is subjected to plasma cladding coupled external field treatment, and the surfaces of the opening and closing parts and the valve seat have a phase composition of a (Ti, W) C phase with a NaCl structure + a (Ti, W, Mo) C interface phase coated on the surface of the (Ti, W) C phase and having a NaCl structure + a TiO 2 The plasma cladding hardened layer of the phase + CoRe solid solution bonding phase; the composition of the surface hardened layer is 15% Co, 50% Re, 5% (Ti, W, Mo) C, and 5% TiO 2 The thickness of the (Ti, W, Mo) C interface phase is 0.26 μm, and the thickness of TiO 2 The grain size is 82nm; the porosity of the surface hardened layer is 0.2%, the total thickness is 680μm, and the surface layer is a high dislocation density fine-grained layer with a thickness of 40μm; the HCP:FCC of the CoRe bonding phase in the plasma cladding hardened layer except the surface high-density fine-grained layer is 0.94, and the dislocation density increases to 7×10 8 mm -2 , the grain size of (Ti,W)C is reduced to 1.6μm; the HCP:FCC of CoRe bonding phase in the fine-grained layer with high dislocation density on the surface of plasma cladding hardened layer is 1.38, and the dislocation density increases to 8×10 10 mm -2 , the grain size of (Ti, W) C is reduced to 1.2 μm; the plasma cladding hardened layer is metallurgically bonded with the opening and closing parts and the valve seat substrate, and there is a transition zone with a thickness of 46 μm between the two. Its phase composition is α-Fe+(Ti, W) C+CoRe solid solution+(Ti, W, Mo) C; the hardness of the opening and closing parts and the valve seat surface hardened layer is 960 HV, the coating bonding strength is 430 MPa, and the wear rate is 2×10 -6 mm 3 / (N·mm), thermal conductivity is 32W·m -1 ·K-1 The maximum service temperature of the wear-resistant control valve is 660℃.

Claims

1. A process for producing wear-resistant control valves by plasma cladding coupled with external field treatment, characterized in that: The following steps are involved: (1) Preparation of metal-ceramic composite slurry for plasma cladding of wear-resistant control valves: C 16 H 36 O4Ti and C 15 H 35 MoO5 is used as a raw material to prepare Ti(OH)4 sol and Mo(OH)6 sol; Mo(OH)6 sol, Ti(OH)4 sol, (Ti, W)C powder, Co powder, and Re powder are weighed, and Co accounts for 10-15% and Re accounts for 30-50% of Co by mole percentage; Mo accounts for 1-5% of Mo and Ti(OH)4 sol is weighed for 3-6% of Ti, and the rest is (Ti, W)C; Mo(OH)6 is first coated on the surface of (Ti, W)C, and then Co and Re are added for ball milling and filtering to prepare a metal ceramic composite slurry for plasma cladding; (2) Preparation of metal-ceramic composite powder feed for plasma cladding of wear-resistant control valves: First, the metal-ceramic composite slurry is spray-dried and sintered at 1100-1200°C to form spherical powder agglomerates; then, the Ti(OH)4 sol weighed during batching is completely immersed in the pores of the spherical powder agglomerates to prepare a metal-ceramic composite powder feed for plasma cladding of wear-resistant control valves, and its phase composition is (Ti, W)C phase with NaCl structure + MoO3 orthorhombic phase coated on the surface of (Ti, W)C phase + Ti(OH)4 gel + Co phase + Re phase; (3) Plasma cladding surface hardening treatment of wear-resistant control valves: Plasma cladding surface hardening treatment is performed on the opening and closing parts and valve seat surfaces using metal-ceramic composite powder feeding. MoO3 undergoes solid solution reaction and carbon thermal reduction with (Ti, W) C to transform into (Ti, W, Mo) C interface phase in situ and still coat the (Ti, W) C surface. The Ti(OH) 4 gel in the pores is transformed into dispersed nano-TiO2. Re is solid-dissolved in Co and promotes the martensitic phase transformation from FCC to HCP in the Co phase and the grain refinement of the (Ti, W) C phase. Plasma cladding forms a surface hardening layer containing an interface phase and oxides, and its phase composition is (Ti, W) C phase with NaCl structure + (Ti, W, Mo) C interface phase with NaCl structure coated on the (Ti, W) C phase surface + TiO2 phase with rutile structure + CoRe solid solution bonding phase. (4) Formation of fine crystal layer on the surface of plasma cladding hardened layer: Polydimethylsiloxane, blocked isocyanate and dibutyltin dilaurate are mixed to form a transparent silicone gel film; the opening and closing parts and valve seats after hardening treatment are finely ground, and black paint is sprayed on the surface as an absorption layer. Then, after cooling in liquid nitrogen, the silicone gel film is attached to the surface of the black paint absorption layer as a constraint layer. The hardened layer attached with the silicone gel film is laser impact treated to generate a plasma shock wave between the constraint layer and the absorption layer to form a high dislocation density fine crystal layer on the surface of the hardened layer; the high-density dislocation fine crystal layer has a thickness of 20~50μm and a dislocation density of 2×10 9 ~6×10 9 mm -2 ; (5) Dislocation density and phase regulation based on external field treatment and wear-resistant control valve manufacturing: The hardened layer with a high dislocation density fine-grained layer on the surface was treated with a pulsed electromagnetic field, and the CoRe bonding phase continued to transform from FCC to HCP, the dislocation density increased, and the grains were refined; the HCP of the CoRe bonding phase in the hardened layer except the surface high-density fine-grained layer: FCC = 0.8~1.0, the dislocation density 1×10 8 ~8×10 8 mm -2 ; HCP:FCC of CoRe binder phase in high dislocation density fine grain layer of hardened layer is 1.3~1.4, dislocation density is 3×10 10 ~9×10 10 mm -2 The opening and closing parts and valve seats that have been treated in the field are ground and assembled with matching parts to produce a wear-resistant control valve. The hardness of the surface hardening layer of the opening and closing parts and valve seats is ≧950HV, the coating bonding strength is ≧420MPa, and the wear rate is ≦4×10 -6 mm 3 / (N·mm), thermal conductivity is 30~40W·m -1 ·K -1 , the maximum service temperature is 660℃.

2. The process for producing a wear-resistant control valve by plasma cladding coupled with external field treatment according to claim 1 is characterized in that: When preparing the metal-ceramic composite slurry for plasma cladding of wear-resistant control valves, first 18 H 29 NaO3S, isopropanol, and cyclohexane were added to deionized water, and the weight percentage was C 18 H 29 NaO3S accounts for 15% to 30%, isopropanol accounts for 6% to 16%, cyclohexane accounts for 5% to 15%, and the rest is ionized water; stir with a magnetic stirrer at 60 to 90°C for 3 to 10 hours, and then leave for 6 to 12 hours to form a reverse microemulsion; use the reverse microemulsion as the solvent, add C 16 H 36 O4Ti, the concentration is 0.5 ~ 1mol / L, and then add ammonia water to adjust the solution pH to 8 ~ 9, stir with a magnetic stirrer at 60 ~ 90 ℃ for 3 ~ 6h, and then leave for 3 ~ 6h to form Ti (OH) 4 sol; C 15 H 35 Mo(OH)6 sol was prepared by using MoO5 as raw material and the same parameters as Ti(OH)4 sol; the average particle sizes D50 of (Ti,W)C powder, Co powder and Re powder were 2.6~3.0μm, 1.0~1.2μm and 2.0~4.0 μm respectively; Mo(OH)6 sol and (Ti,W)C were first mixed, and then 0.5~1% of C in the total weight of the mixed solution was added. 18 H 34 O2 and 1-2% PEG2000 by total weight, and magnetically stirred for 30-60 minutes, and then ammonia water was dropped into the mixture to adjust the pH value of the mixture to 8-9, and the Zeta potential of the mixture was 22-34 mV, so that Mo(OH)6 was coated on the (Ti, W)C surface; Co powder and Re powder were added for ball milling, the ball-to-material weight ratio was 10:1, WC-Co carbide grinding balls with a diameter of 6-10 mm were used, the ball milling time was 24-36 hours, and the ball milling speed was 300-400 r / min; after the ball milling, a 400-mesh sieve was used for filtration to prepare a metal-ceramic composite slurry for plasma cladding composed of (Ti, W)C, Co, and Re powders coated with Mo(OH)6 on the surface.

3. The process for producing a wear-resistant control valve by plasma cladding coupled with external field treatment according to claim 1 is characterized in that: When the metal-ceramic composite powder for plasma cladding of wear-resistant control valves is prepared, the atomizing disk speed is 5000~7000r / min during spray drying, and the drying temperature is 120~130℃; after spray drying, the spherical powder agglomerates are placed in a vacuum sintering furnace and sintered at 1100~1200℃ for 60~90min, the initial vacuum degree of sintering is 1~5Pa, and the heating rate is 5℃ / min; after sintering, the spherical powder agglomerates with a particle size of 35~45μm are formed through crushing and airflow classification; then The classified spherical powder agglomerates are completely immersed in the Ti(OH)4 sol weighed during batching and dried at 100-110°C. After 10-20 times of immersion and drying, the Ti(OH)4 sol weighed during batching is completely immersed in the pores of the classified spherical powder agglomerates to prepare a metal-ceramic composite powder feed for plasma cladding of a wear-resistant control valve, wherein the HCP:FCC in the Co phase is 0.2-0.3, and the particle size of (Ti,W)C is 2.2-2.5μm.

4. The process for producing a wear-resistant control valve by plasma cladding coupled with external field treatment according to claim 1 is characterized in that: When the plasma cladding surface hardening treatment of the wear-resistant control valve is carried out, the opening and closing parts and the valve seat surface of the wear-resistant control valve are first ground to make the surface roughness Ra0.6~0.8μm. The working voltage of the plasma cladding surface hardening treatment is 20~24V, the working current is 100~240A, the ionized gas argon flow rate is 10~13L / min, the protective gas argon flow rate is 13~15L / min, the scanning rate is 10~15cm / min, and the coaxial powder feeding is used, and the powder feeding rate is 8~10g / min; the (Ti, W formed during the plasma cladding process ,Mo)C interface phase thickness is 0.1~0.3μm and the grain size and phase remain unchanged in subsequent treatment; the formed nano-TiO2 has a grain size of 50~90nm, and the grain size and phase remain unchanged in subsequent treatment; the surface hardening layer composition is Co accounts for 10~15% by mole, Re accounts for 30~50% of Co, (Ti,W,Mo)C accounts for 1~5%, TiO2 accounts for 3~6%, and the rest is (Ti,W)C; HCP:FCC in the CoRe bonding phase in the plasma cladding hardening layer is 0.4~0.7, and the dislocation density is 1×10 7 ~6×10 7 mm -2 , the dislocation density in the steel matrix is ​​3×10 6 ~7×10 6 mm -2 ; The grain size of (Ti, W) C in the surface hardened layer is 1.8~2.0μm, the porosity is 0.1~0.5%, and the thickness is 600~1200μm; the plasma cladding hardened layer is metallurgically bonded to the opening and closing parts and the valve seat substrate, and there is a transition zone with a thickness of 40~50μm between the two, and its phase composition is α-Fe+(Ti, W) C+CoRe solid solution+(Ti, W, Mo) C.

5. The process for producing a wear-resistant control valve by plasma cladding coupled with external field treatment according to claim 1 is characterized in that: When the fine crystal layer on the surface of the plasma cladding hardened layer is formed, polydimethylsiloxane with a viscosity of 1500~3000cps, blocked isocyanate and dibutyltin dilaurate are first mixed into a glue solution in a volume ratio of 100:(0.8~1.5):(0.1~0.3), stirred for 10~20min, and subjected to high-speed centrifugal degassing treatment. The speed of the centrifugal degassing treatment is 600~1000r / min, and the centrifugal time is 5~10min. The glue solution is injected into the mold and cured at 50~60℃ to form a transparent silicone gel film with a thickness of 1.0~1.3mm; then the opening and closing parts and valve seats after the plasma cladding hardening treatment are finely ground to make their roughness Ra0.2~0.4μm, and black paint is sprayed on the surface of the prepared plasma cladding hardened layer as an absorbent. layer, and then cooled to -190℃ in liquid nitrogen and kept for 30-60min. After taking it out, the silicone gel film was attached to the surface of the black paint absorption layer as a constraint layer. The plasma cladding hardened layer attached with the silicone gel film was laser impact treated within 3-5min. The laser wavelength was 1.064μm, the laser spot diameter was 1-4mm, the spot overlap rate was 20-60%, the pulse energy was 10-15J, and the pulse width was 15-25ns. The surface of the high dislocation density fine grain layer was in a compressive stress state, the grain size of (Ti,W)C was 1.3-1.6μm, and the CoRe bonding phase underwent a martensitic phase transformation, in which HCP:FCC=0.8-1.

0. The dislocation density, phase composition and grain size of the plasma cladding hardened layer, except for the surface high dislocation density fine grain layer and the steel matrix, remained unchanged.

6. The process for producing a wear-resistant control valve by plasma cladding coupled with external field treatment according to claim 1 is characterized in that: Based on the dislocation density and phase regulation of external field treatment and the manufacture of wear-resistant control valves, the plasma cladding hardened layer with a surface high dislocation density fine crystal layer was treated with a pulsed electromagnetic field. The intensity of the pulsed magnetic field was 0.5-1.5T, the magnetic pulse frequency was 1-5Hz, the number of magnetic pulses was 30-40, the electric field intensity was 1-2V, the frequency of the electric pulse was 50Hz, and the number of electric pulses was 5-10. The grain size of (Ti, W) C in the hardened layer except the surface high-density fine crystal layer was 1.4-1.7μm; the grain size of (Ti, W) C in the high dislocation density fine crystal layer in the hardened layer was 1.0-1.2μm; the dislocation density in the steel matrix increased to 1×10 7 ~7×10 7 mm -2 The wear-resistant control valve opening and closing parts and valve seats that have been processed in the field are ground and assembled with the matching valve body, valve stem, valve cover and spring to manufacture the wear-resistant control valve.

7. A wear-resistant control valve subjected to plasma cladding coupled external field treatment, obtained by using the wear-resistant control valve production process subjected to plasma cladding coupled external field treatment according to any one of claims 1 to 6, characterized in that: The invention comprises an opening and closing part and a valve seat, wherein the surfaces of the opening and closing part and the valve seat have a plasma cladding hardened layer with a phase composition of a (Ti, W) C phase with a NaCl structure + a (Ti, W, Mo) C interface phase coated on the surface of the (Ti, W) C phase and having a NaCl structure + a TiO2 phase with a rutile structure + a CoRe solid solution bonding phase; the surface hardened layer has a porosity of 0.1-0.5% and a total thickness of 600-1200 μm, and its surface layer is a high dislocation density fine grain layer with a thickness of 20-50 μm; the plasma cladding hardened layer is metallurgically bonded to the opening and closing part and the valve seat substrate, and there is a transition zone with a thickness of 40-50 μm between the two, and its phase composition is α-Fe+(Ti, W) C+CoRe solid solution+(Ti, W, Mo) C; the hardness of the surface hardened layer of the opening and closing part and the valve seat is ≧950 HV, the coating bonding strength is ≧420 MPa, and the wear rate is ≦4×10 -6 mm 3 / (N·mm), thermal conductivity is 30~40W·m -1 ·K -1 The maximum service temperature of the wear-resistant control valve is 660℃.

8. The wear-resistant control valve treated by plasma cladding coupled with external field treatment according to claim 7, characterized in that: The composition of the surface hardened layer of the opening and closing parts and valve seats is Co accounting for 10-15%, Re accounting for 30-50% of Co, (Ti, W, Mo) C accounting for 1-5%, TiO2 accounting for 3-6%, and the rest is (Ti, W) C; the thickness of the (Ti, W, Mo) C interface phase is 0.1-0.3 μm, and the grain size of TiO2 is 50-90 nm; in the plasma cladding hardened layer, except for the surface high-density fine-grained layer, the HCP: FCC of the CoRe bonding phase is 0.8-1.0, and the dislocation density increases to 1×10 8 ~8×10 8 mm -2 , the grain size of (Ti,W)C is reduced to 1.4~1.7μm; the HCP:FCC of CoRe bonding phase in the fine-grained layer with high dislocation density on the surface of plasma cladding hardened layer is 1.3~1.4, and the dislocation density increases to 3×10 10 ~9×10 10 mm -2 , the grain size of (Ti,W)C is reduced to 1.0~1.2μm.