Bone cement developing agent, preparation method and application thereof, and bone cement comprising bone cement developing agent

By modifying the surface of polydopamine microspheres with iodine-based substances, a modified developer is formed, which solves the problem of insufficient biocompatibility and mechanical properties of bone cement developers, significantly improves the development and biocompatibility, and prolongs the The service life of artificial joints.

CN118718085APending Publication Date: 2024-10-01BEIJING BONSCI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411040938.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing bone cement developers have problems with poor biocompatibility and insufficient mechanical properties in the human body, leading to wear and loosening of artificial joints, and commonly used developer materials have adverse effects on the human body.

Method used

The surface of polydopamine microspheres is modified with iodine-based substances to form surface-modified polydopamine microspheres as bone cement developer, which improves the development and biocompatibility, and at the same time enhances the mechanical properties of bone cement.

Benefits of technology

While the developer does not affect the mechanical properties of bone cement, it significantly improves the biocompatibility and mechanical properties of bone cement, extends the service life of artificial joints, and reduces adverse effects on the human body.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118718085A_ABST
    Figure CN118718085A_ABST
Patent Text Reader

Abstract

The invention provides a bone cement developing agent, a preparation method and application thereof and bone cement containing the bone cement developing agent, and relates to the technical field of orthopedic repair medical materials. The bone cement developing agent comprises surface modified polydopamine microspheres, wherein the surface modification comprises the step of carrying out surface modification on the polydopamine microspheres by utilizing iodine substances. The polydopamine microspheres subjected to surface modification by the iodine substances have good biocompatibility and biodegradability while having developability, and the biological activity and mechanical properties of bone cement can be effectively improved when the polydopamine microspheres are applied to the bone cement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of orthopedic repair medical materials, and in particular to a bone cement developer, a preparation method and application thereof, and bone cement comprising the same. Background Art

[0002] In orthopedic surgery, percutaneous vertebroplasty has become a minimally invasive treatment for vertebral metastatic tumors, vertebral primary tumors, vertebral compression fractures caused by osteoporosis, etc. The treatment is mainly achieved by percutaneous injection of PMMA bone cement into the vertebral body to strengthen the vertebral body. However, there are some fundamental problems with the existing bone cement products on the market, because percutaneous injection usually needs to be performed under the monitoring of an X-ray machine to prevent bone cement leakage from causing harm to the surgical operation and the patient, which requires bone cement to have good development properties. The developer material is an indispensable and important component of bone cement, which is used to display and track the growth of bone tissue around the implanted artificial joint.

[0003] Generally speaking, bone cement developers are divided into iodine-containing and non-iodine-containing types. Currently, the developer materials used in bone cement are mainly non-iodine BaSO4 or ZrO2 and other metal inorganic salt compounds. These materials have low irritation, high density and good contrast, and can effectively play a developing effect, but have a series of adverse effects on the human body, such as neurotoxicity, cell deformation, etc., and the interaction force between the developer and the polymer matrix in the bone cement is weak, the binding performance is poor, and it cannot form an effective whole. The developer is easy to separate from the bone cement, reducing the mechanical properties of the bone cement. For example, when used in artificial joints, it is easy to cause wear and loosening of the artificial joints, shortening the service life of the artificial joints. Therefore, the existing bone cement developers have general biocompatibility, and have a negative impact on the mechanical properties of bone cement, which may cause wear and loosening of artificial joints.

[0004] In recent years, some solutions have been proposed to improve the biocompatibility and mechanical properties of bone cement contrast agents, such as: 1. Reduce the size of developer particles. At present, micron-sized barium sulfate or magnesium oxide and nano-sized barium sulfate or magnesium oxide are usually added to bone cement as developers. Although compared with bone cement with micron-sized developer, bone cement with nano-sized developer has better mechanical properties and developing properties, nano-sized particles are very easy to agglomerate in bone cement and have poor dispersibility. Secondly, the interaction force between bone cement particles and polymer matrix is ​​weak, the binding performance is poor, and an effective whole cannot be formed, which easily causes phase separation between bone cement and developer.

[0005] 2. Replace with other substances such as bismuth phosphate. The results show that adding bismuth phosphate can significantly enhance the development performance of bone cement. When the addition of bismuth phosphate reaches more than 9%, bone cement obtains obvious development effect. Adding bismuth phosphate reduces the viscosity of bone cement, significantly improves injectability, increases compressive strength, and prolongs setting time. However, when the amount of bismuth phosphate added is greater than 12%, the strength of the material will decrease significantly.

[0006] 3. Bone cement polymer itself is combined with iodine. Studies have found that when iodine is introduced into bone cement as a developer, the development performance and mechanical properties of bone cement are slightly improved to a certain extent. However, since it is impossible for all iodine to participate in the polymerization of bone cement, iodine-containing monomers may precipitate from bone cement and enter the human body environment, causing certain adverse effects on human joints.

[0007] Therefore, in view of the above-mentioned deficiencies of existing bone cement developers, it is necessary and urgent to research and develop a bone cement developer with good biocompatibility, excellent mechanical strength, excellent biodegradability, and the ability to effectively improve the bioactivity of bone cement while ensuring the developer performance.

[0008] In view of this, the present invention is proposed. Summary of the invention

[0009] The first object of the present invention is to provide a bone cement developer, which includes surface-modified polydopamine microspheres modified with iodine-based substances. The polydopamine microspheres surface-modified with the iodine-based substances have excellent biocompatibility and biodegradability while having the ability to develop, and can effectively improve the biological activity and mechanical properties of bone cement.

[0010] The second object of the present invention is to provide a method for preparing a bone cement developer.

[0011] The third object of the present invention is to provide a bone cement comprising the above-mentioned bone cement developer.

[0012] A fourth object of the present invention is to provide an application of the above-mentioned bone cement developer or bone cement.

[0013] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted: The present invention provides a bone cement developer, which includes surface-modified polydopamine microspheres; Wherein, the surface modification includes using iodine substances to modify the surface of polydopamine microspheres.

[0014] Furthermore, the particle size of the polydopamine microspheres is 250-500 nm, preferably 300 nm.

[0015] Furthermore, the surface-modified iodine-based substance includes at least one of iohexol, iobitrol, iodixanol and ioversol, preferably iohexol.

[0016] The present invention provides a method for preparing the above-mentioned bone cement developer, the preparation method comprising the following steps: The polydopamine microspheres are suspended and dispersed in a buffer solution to obtain a polydopamine microsphere suspension; an iodine-based substance is then added to fully mix and react, followed by centrifugation to obtain a bone cement developer; Preferably, the buffer comprises at least one of Tris-HCl buffer and Tris buffer (Tris), preferably Tris-HCl buffer; Furthermore, the mass ratio of the polydopamine microspheres to the iodine-based substances is 1-2:0.75-1.5, preferably 1:1.

[0017] Furthermore, the method of suspending and dispersing the polydopamine microspheres in the buffer solution is ultrasonic dispersion; Preferably, the power of the ultrasonic dispersion is 500-800W, preferably 500W; Preferably, the ultrasonic dispersion time is 20 to 30 min, preferably 30 min.

[0018] Furthermore, the mixing reaction is a magnetic stirring reaction, and the time of the magnetic stirring reaction is 3 to 5 hours, preferably 4 hours; Preferably, the speed of the centrifugation is 8000-10000 rpm / min, preferably 10000 rpm / min; Preferably, the centrifugation time is 10 to 20 min, preferably 15 min.

[0019] Furthermore, the preparation method also includes the steps of washing and drying the bone cement developer obtained by centrifugation.

[0020] Preferably, the cleaning solution comprises at least one of ethanol and ultrapure water, preferably ethanol; Preferably, the drying temperature is 50-70°C, preferably 60°C.

[0021] The present invention provides a bone cement, which comprises the above-mentioned bone cement developer.

[0022] The invention provides an application of the bone cement developer or the bone cement in the preparation of medical orthopedic repair biomaterials.

[0023] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides a bone cement developer, which includes surface-modified polydopamine microspheres; wherein the surface modification includes surface modification of the polydopamine microspheres with iodine-based substances. The polydopamine microspheres surface-modified with the iodine-based substances have developing properties and do not affect the mechanical properties of bone cement, and can effectively improve the biocompatibility of bone cement.

[0024] The present invention provides a method for preparing a bone cement developer, which comprises suspending and dispersing polydopamine microspheres in a buffer solution to obtain a polydopamine microsphere suspension; then adding an iodine substance for sufficient mixing and reaction, followed by centrifugation to obtain a bone cement developer; the above-mentioned preparation method has the advantages of simple processing technology and easy operation.

[0025] The bone cement provided by the present invention includes the above-mentioned bone cement developer. Determined by the characteristics of the above-mentioned bone cement developer, the above-mentioned bone cement has the advantages of good biocompatibility and excellent mechanical strength.

[0026] The bone cement developer or bone cement provided by the present invention can be widely used in the preparation of medical orthopedic repair biomaterials. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0028] Figure 1 The image of the bone cement prepared in Example 5 provided in Experimental Example 1 of the present application under X-ray development ability; Figure 2 The image of the bone cement prepared in Example 6 provided in Experimental Example 1 of the present application showing its ability to be developed under X-ray; Figure 3 The image of the bone cement prepared in Example 7 provided in Experimental Example 1 of the present application under X-ray development ability; Figure 4 A graph showing the ability of bone cement prepared in Comparative Example 1 provided in Experimental Example 1 of the present application to develop images under X-ray; Figure 5 This is a comparison chart of the effects of bone cement provided in Example 5 provided in Experimental Example 1 of the present application and in Comparative Example 1 on cell proliferation. DETAILED DESCRIPTION

[0029] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] According to one aspect of the present invention, a bone cement developer is provided, comprising surface-modified polydopamine microspheres; wherein the surface modification comprises modifying the surface of the polydopamine microspheres using iodine-based substances.

[0031] The present invention provides a bone cement developer, which includes surface-modified polydopamine microspheres; wherein the surface modification includes surface modification of the polydopamine microspheres with iodine-based substances. The polydopamine microspheres surface-modified with the iodine-based substances have developing properties and do not affect the mechanical properties of bone cement, and can effectively improve the biocompatibility of bone cement.

[0032] In a preferred embodiment of the present invention, the particle size of the polydopamine microspheres is 250-500 nm, preferably 300 nm.

[0033] Preferably, the method for preparing polydopamine microspheres comprises the following steps: 1. Mix 5 ml of Tris-HCl (pH=8.5) buffer, 7.5 ml of anhydrous ethanol, 0.5 ml of concentrated ammonia (28%, w / w) and 18 ml of deionized water, and stir magnetically for 1 h to fully dissolve to obtain a mixed solution A.

[0034] 2. Dissolve 0.1 g of dopamine hydrochloride in 5 ml of deionized water to obtain a dopamine hydrochloride solution; 3. After mixing the mixed solution A with the dopamine hydrochloride solution, continue stirring. You can see that the solution quickly turns light yellow. After about 0.5 h, the solution turns brown and finally turns black. Keep magnetic stirring for 24 hours and then centrifuge (10000 rpm, 15 min). Wash with ethanol 3 times and dry in a vacuum oven at 60 ° C to obtain polydopamine microspheres with a particle size of 300 nm (300 nm PDA Ns).

[0035] In a preferred embodiment of the present invention, the surface-modified iodine-based substance comprises at least one of iohexol, iobitrol, iodixanol and ioversol, preferably iohexol.

[0036] According to one aspect of the present invention, a method for preparing the above-mentioned bone cement developer comprises the following steps: The polydopamine microspheres are suspended and dispersed in a buffer solution to obtain a polydopamine microsphere suspension; an iodine-based substance is then added to fully mix and react, followed by centrifugation to obtain a bone cement developer; The present invention provides a method for preparing a bone cement developer, which comprises suspending and dispersing polydopamine microspheres in a buffer solution to obtain a polydopamine microsphere suspension; then adding an iodine substance for sufficient mixing and reaction, followed by centrifugation to obtain a bone cement developer; the above-mentioned preparation method has the advantages of simple processing technology and easy operation.

[0037] In a preferred embodiment of the present invention, the buffer comprises at least one of Tris-HCl buffer and Tris buffer (Tris), preferably Tris-HCl buffer; In a preferred embodiment of the present invention, the mass ratio of the polydopamine microspheres to the iodine-based substances is 1-2:0.75-1.5, preferably 1:1.

[0038] In a preferred embodiment of the present invention, the method of suspending and dispersing the polydopamine microspheres in the buffer is ultrasonic dispersion; In the above preferred embodiment, the power of the ultrasonic dispersion is 500-800 W, preferably 500 W; In the above preferred embodiment, the ultrasonic dispersion time is 20 to 30 minutes, preferably 30 minutes.

[0039] In a preferred embodiment of the present invention, the mixing reaction is a magnetic stirring reaction, and the time of the magnetic stirring reaction is 3 to 5 h, preferably 4 h; In the above preferred embodiment, the centrifugal speed is 8000-10000 rpm / min, preferably 10000 rpm / min; In the above preferred embodiment, the centrifugation time is 10 to 20 minutes, preferably 15 minutes.

[0040] In a preferred embodiment of the present invention, the preparation method further comprises the steps of washing and drying the bone cement developer obtained by centrifugation.

[0041] In the above preferred embodiment, the cleaning solution includes at least one of ethanol and ultrapure water, preferably ethanol; In the above preferred embodiment, the drying temperature is 50-70°C, preferably 60°C.

[0042] According to one aspect of the present invention, a bone cement comprises the above-mentioned bone cement developer.

[0043] The bone cement provided by the present invention includes the above-mentioned bone cement developer. Determined by the characteristics of the above-mentioned bone cement developer, the above-mentioned bone cement has the advantages of good biocompatibility and excellent mechanical strength.

[0044] In a preferred embodiment of the present invention, the bone cement comprises a powder material and a liquid material; Wherein: the powder comprises the following components by mass percentage: 88.5-90.5% polymethyl methacrylate, 9-11% developer and 0.4-0.6% initiator, and the sum of the mass percentages of the powder is 100%; the developer is the above-mentioned bone cement developer; The liquid material comprises the following components by mass percentage: 96-98% of methyl methacrylate, 2.5-3.5% of accelerator and 0.009-0.011% of inhibitor, and the sum of the mass percentages of the liquid material is 100%; In the above preferred embodiment, the initiator includes at least one of benzoyl peroxide, cyclohexanone peroxide or methyl ethyl ketone peroxide, preferably benzoyl peroxide; In the above preferred embodiment, the accelerator is at least one of N,N-dimethyl-p-toluidine, N,N-dimethylaniline, N,N-diethylaniline or thiol, preferably N,N-dimethyl-p-toluidine; In the above preferred embodiment, the polymerization inhibitor is at least one of hydroquinone, 2,4-dimethyl-6-tert-butylphenol, and nitrosophenol, preferably hydroquinone.

[0045] Preferably, the method for preparing bone cement comprises the following steps: (a) mixing the components of the powder to obtain bone cement powder; (b) mixing the components of the liquid material to obtain a bone cement liquid material; (c) mixing the bone cement liquid with the solid phase powder to prepare the bone cement; The order of step (a) and step (b) can be reversed.

[0046] According to one aspect of the present invention, the above-mentioned bone cement developer or the above-mentioned bone cement is used in the preparation of medical orthopedic repair biomaterials.

[0047] The bone cement developer or bone cement provided by the present invention can be widely used in the preparation of medical orthopedic repair biomaterials.

[0048] The technical solution of the present invention will be further described below in conjunction with embodiments and comparative examples.

[0049] Example 1 A polydopamine microsphere, the preparation method comprises the following steps: 1. Mix 5 ml of Tris-HCl (pH=8.5) buffer, 7.5 ml of anhydrous ethanol, 0.5 ml of concentrated ammonia (28%, w / w) and 18 ml of deionized water, and stir magnetically for 1 h to fully dissolve to obtain a mixed solution A.

[0050] 2. Dissolve 0.1 g of dopamine hydrochloride in 5 ml of deionized water to obtain a dopamine hydrochloride solution; 3. After mixing the mixed solution A with the dopamine hydrochloride solution, continue stirring. You can see that the solution quickly turns light yellow. After about 0.5 h, the solution turns brown and finally turns black. Keep magnetic stirring for 24 hours and then centrifuge (10000 rpm, 15 min). Wash with ethanol 3 times and dry in a vacuum oven at 60 ° C to obtain polydopamine microspheres with a particle size of 300 nm (300 nm PDA Ns).

[0051] Example 2 A method for preparing a bone cement developer, the method comprising the following steps: (1) Add 0.1 g of polydopamine microspheres prepared in Example 1 to 50 ml of Tris-HCl and disperse by ultrasonication (500 w, 30 min) to obtain a polydopamine microsphere suspension; (2) adding 0.1 g of iohexol to the polydopamine microsphere suspension obtained in step (1) and reacting under magnetic stirring for 4 hours, followed by centrifugation at 10,000 rpm for 15 minutes to obtain a precipitate; (3) The precipitate obtained in step (2) was washed with ethanol three times, and then dried in a vacuum oven at 60° C. to obtain a bone cement developer.

[0052] Example 3 A method for preparing a bone cement developer, the method comprising the following steps: (1) Add 0.1 g of polydopamine microspheres prepared in Example 1 to 50 ml of Tris-HCl and disperse by ultrasonication (500 w, 30 min) to obtain a polydopamine microsphere suspension; (2) Add 0.15 g of iohexol to the polydopamine microsphere suspension obtained in step (1) and stir under magnetic stirring for 4 hours, followed by centrifugation at 10,000 rpm for 15 minutes to obtain a precipitate; (3) The precipitate obtained in step (2) was washed with ethanol three times, and then dried in a vacuum oven at 60° C. to obtain a bone cement developer.

[0053] Example 4 A method for preparing a bone cement developer, the method comprising the following steps: (1) Add 0.1 g of polydopamine microspheres prepared in Example 1 to 50 ml of Tris-HCl and disperse by ultrasonication (500 w, 30 min) to obtain a polydopamine microsphere suspension; (2) adding 0.075 g of iohexol to the polydopamine microsphere suspension obtained in step (1) and reacting under magnetic stirring for 4 hours, followed by centrifugation at 10,000 rpm for 15 minutes to obtain a precipitate; (3) The precipitate obtained in step (2) was washed with ethanol three times, and then dried in a vacuum oven at 60° C. to obtain a bone cement developer.

[0054] Example 5 A bone cement, comprising a powder material and a liquid material; Wherein: in terms of mass percentage, the powder comprises the following components:

[0055] In terms of mass percentage, the liquid material comprises the following components:

[0056] The preparation method of the bone cement comprises the following steps: 1. Mix the various components of the powder to obtain bone cement powder; mix the various components of the liquid to obtain bone cement liquid; 2. After mixing the bone cement powder and the bone cement liquid, stir them at a rate of 100 times / minute for 5 minutes, and then solidify them to prepare bone cement.

[0057] Example 6 A bone cement, comprising a powder material and a liquid material; Wherein: in terms of mass percentage, the powder comprises the following components:

[0058] In terms of mass percentage, the liquid material comprises the following components:

[0059] The preparation method is the same as that of Example 5.

[0060] Example 7 A bone cement, comprising a powder material and a liquid material; Wherein: in terms of mass percentage, the powder comprises the following components:

[0061] In terms of mass percentage, the liquid material comprises the following components:

[0062] The preparation method is the same as that of Example 5.

[0063] Comparative Example 1 A bone cement, comprising a powder material and a liquid material; Wherein: in terms of mass percentage, the powder comprises the following components:

[0064] In terms of mass percentage, the liquid material comprises the following components:

[0065] The preparation method of the bone cement comprises the following steps: 1. Mix the various components of the powder to obtain bone cement powder; mix the various components of the liquid to obtain bone cement liquid; 2. After mixing the bone cement powder and the bone cement liquid, stir them at a rate of 100 times / minute for 5 minutes, and then solidify them to prepare bone cement.

[0066] Experimental Example 1 In order to show that the bone cement prepared by using the bone cement developer of the present application has the advantage of good biocompatibility compared with the existing bone cement without affecting the developing property and mechanical properties, the applicant now performs performance testing on the bone cement prepared by Examples 5 to 7 and Comparative Example 1, and the specific method is as follows: 1. Mechanical properties: Refer to the method of standard YY0459-2003 for corresponding mechanical properties test: Compressive strength test: Mix a set of bone cement powder and liquid at (23±1)℃. When the mixed bone cement is in a dough-like state, carefully fill it into a specific mold to prepare a 6×12mm sample column. Soak the test specimen in an acidic buffer for 10 days and place it on the static compression test device of the test equipment. Start the test machine to apply a load to the sample at a constant crosshead rate within the range of 19.8mm / min–25.6mm / min. Stop when the sample breaks or has passed the upper yield point.

[0067] Flexural strength and flexural modulus test: Mix a set of bone cement powder and liquid under (23±1)℃ environmental conditions. When the mixed bone cement is in a dough-like state, carefully fill it into a specific mold to prepare a 75×10×3.3mm specimen. Soak the test specimen in an acidic buffer for 10 days and place it on the test equipment. Use a bending tester to apply force on the central load column from zero at a crosshead rate of 5mm / min±1mm / min, record the change of the test strip deflection with the applied force, and continue to apply force until the test strip breaks.

[0068] The specific results are as follows:

[0069] It can be seen from the above table that the bone cement prepared using the bone cement developer of the present application has significantly improved mechanical properties compared to existing bone cement, proving that the bone cement developer of the present application replaces the traditional bone cement developer to effectively improve the mechanical properties of bone cement.

[0070] 2. Development performance The bone cements prepared in Examples 5 to 7 and Comparative Example 1 were placed on an X-ray machine (52KV, 400mA, 14ms) for scanning. The X-ray development capabilities of the various samples were as follows: Figures 1 to 4 As shown: Figure 1 This is a graph showing the ability of bone cement prepared in Example 5 of the present application to be developed under X-ray; Figure 2 This is a graph showing the ability of bone cement prepared in Example 6 of the present application to develop images under X-ray; Figure 3 This is a graph showing the ability of bone cement prepared in Example 7 of the present application to develop under X-ray; Figure 4 This is a graph showing the ability of bone cement prepared in comparative example 1 of the present application to develop images under X-ray; By the above Figures 1 to 4 It can be seen that the bone cement prepared using the bone cement developer of the present application exhibits good development performance, proving that replacing the traditional bone cement developer with the bone cement developer of the present application will not affect the development performance of the bone cement. And as the developer content increases, the development ability is better, and the development ability of the bone cement prepared using the present application is significantly enhanced.

[0071] 3. Biocompatibility testing According to the national standard GB / T 16886.5-2003 "Biological Evaluation of Medical Devices Part 5: In Vitro Cytotoxicity Test", the extract test was selected, and the biocompatibility of the bone cement provided in Example 5 of the present invention and that in Comparative Example 1 was compared according to the tetrazolium (MTT) colorimetric method recommended in the cytotoxicity test in GB / T14233.2-2005. The effects of the bone cement provided in Example 5 and Comparative Example 1 on cell proliferation were used as the test standard. The test results are as follows: Figure 5 As shown: Figure 5 This is a comparison chart of the effects of bone cement provided in Example 5 and Comparative Example 1 on cell proliferation.

[0072] Depend on Figure 5It can be seen that the cell proliferation rate of the bone cement provided in Example 5 is in the range of 90%-100%, while the cell proliferation rate of the bone cement provided in Comparative Example 1 is in the range of 80%-90%, which proves that the bone cement provided by the present invention has better biocompatibility than the bone cement commonly used in the prior art provided in Comparative Example 1.

[0073] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A bone cement developer, characterized in that: The bone cement developer comprises surface-modified polydopamine microspheres; The surface modification includes using iodine substances to modify the surface of the polydopamine microspheres, thereby grafting the iodine-containing structure onto the surface of the polydopamine microspheres.

2. The bone cement developer according to claim 1, characterized in that: The particle size of the polydopamine microspheres is 250-500 nm, preferably 300 nm.

3. The bone cement developer according to claim 1, characterized in that: The surface-modified iodine-based substance comprises at least one of iohexol, iobitrol, iodixanol and ioversol, preferably iohexol.

4. A method for preparing a bone cement developer according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: The polydopamine microspheres are suspended and dispersed in a buffer solution to obtain a polydopamine microsphere suspension; an iodine-based substance is then added to fully mix and react, followed by centrifugation to obtain a bone cement developer; Preferably, the buffer comprises Tris-hydrochloric acid buffer or Tris-hydrochloric acid buffer, preferably Tris-hydrochloric acid buffer.

5. The method for preparing a bone cement developer according to claim 4, characterized in that: The mass ratio of the polydopamine microspheres to the iodine-based substances is 1-2:0.75-1.5, preferably 1:

1.

6. The method for preparing a bone cement developer according to claim 4, characterized in that: The method for suspending and dispersing the polydopamine microspheres in the buffer solution is ultrasonic dispersion; Preferably, the power of the ultrasonic dispersion is 500-800W, preferably 500W; Preferably, the ultrasonic dispersion time is 20 to 30 min, preferably 30 min.

7. The method for preparing a bone cement developer according to claim 4, characterized in that: The mixing reaction is a magnetic stirring reaction, and the time of the magnetic stirring reaction is 3 to 5 hours, preferably 4 hours; Preferably, the speed of the centrifugation is 8000-10000 rpm / min, preferably 10000 rpm / min; Preferably, the centrifugation time is 10 to 20 min, preferably 15 min.

8. The method for preparing a bone cement developer according to claim 4, characterized in that: The preparation method further comprises the steps of washing and drying the bone cement developer obtained by centrifugation; Preferably, the cleaning solution comprises at least one of ethanol and ultrapure water, preferably ethanol; Preferably, the drying temperature is 50-70°C, preferably 60°C.

9. A bone cement, characterized in that: The bone cement comprises the bone cement developer according to any one of claims 1 to 3.

10. Use of the bone cement developer according to any one of claims 1 to 3 or the bone cement according to claim 9 in the preparation of medical orthopedic repair biomaterials.