Dry desulfurizer and preparation method thereof
Through the synergistic use and conditioning reaction of calcium hydroxide, dihydrogen phosphate and other raw materials, the microstructure of the dry desulfurizer is improved, the problem of insufficient penetration capacity and insufficient time of the desulfurizer in the existing technology is solved, and high efficiency is achieved. , long-lasting desulfurization effect, meeting ultra-low emission requirements.
Patent Information
- Application Number
- CN202411064817.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-10-01
AI Technical Summary
Existing dry desulfurizers have low penetration sulfur capacity and short penetration time, making it difficult to meet ultra-low emission requirements. They also have a short service life and serious problems with frequent material changes.
Calcium hydroxide, dihydrogen phosphate, humidifiers, regulators, pore-forming agents and molding aids are used in conjunction to improve the microstructure of the desulfurizer through conditioning reaction and molding process, and improve the migration ability of calcium ions and the desulfurization reaction. activity to prepare a dry desulfurizer with high penetration sulfur capacity and long penetration time.
It achieves high penetration sulfur capacity and long penetration time, extends the service life of the desulfurizer, improves the desulfurization efficiency, reduces the number of replacements, meets ultra-low sulfur dioxide emission requirements, and can effectively remove dust particles in the flue gas. .
Smart Images

Figure BDA0004979044250000101
Abstract
Description
Technical Field
[0001] The invention relates to a dry desulfurizing agent and a preparation method thereof. Background Art
[0002] my country has proposed ultra-low emission transformation requirements for the steel, cement, coking industry and coal-fired boilers. Specific emission targets for sulfur dioxide, nitrogen oxides and smoke are given. The sulfur dioxide emission target is no more than 35mg / m 3 .
[0003] Flue gas desulfurization generally includes three types of desulfurization processes: wet, semi-dry, and dry. Dry flue gas desulfurization is widely promoted and applied due to its unique process advantages. Commonly used dry desulfurizers are mainly calcium-based desulfurizers. Existing calcium-based desulfurizers still have the problems of low penetration sulfur capacity and short effective use period.
[0004] CN112295400A discloses a method for preparing a calcium-based dry desulfurizer composited with activated red mud, comprising: grinding red mud and mixing it with a first activator, and then reacting at high temperature to obtain activated red mud; mixing the activated red mud with a second activator, extruding and molding the mixed powder after ripening, and drying to obtain a calcium-based dry desulfurizer, wherein the second activator comprises a second reinforcing agent, a second catalyst, a second molding agent, and a second active component. The first active component and the second active component respectively comprise Ca(OH)2 and / or Mg(OH)2. The second reinforcing agent comprises one or more of CaSO4, CaCO3, and TiO2. The second catalyst comprises Co2O3 and / or Fe2O3. The second molding agent comprises one or more of dextrin, polyethylene glycol, and pre-paste starch. The desulfurizer of the patent document still needs to be further improved in terms of the performance of penetration sulfur capacity and penetration time.
[0005] CN109603459A discloses a low-temperature dry flue gas desulfurizer, preparation method and application, the desulfurizer includes active component CaO, reaction auxiliary silicon source, catalytic active component V, Fe or Co, the raw material of the active component is cheap quicklime; the auxiliary is silicon source, including diatomaceous earth, bentonite, silica sol and other silicon sources, the catalytic component is V2O5, Fe2O3, Co2O3 or a combination thereof. The total penetration sulfur capacity of the desulfurizer in this patent document is still low, and the penetration time is still short.
[0006] CN109364878A discloses a method for preparing an adsorbent for dry desulfurization and denitrification, which uses semi-coke as a carrier and adopts an ultrasonic-assisted pressure impregnation method to load metal components onto the surface of the semi-coke to prepare a series of Mn-Cu adsorbents. The adsorbent is a non-calcium-based desulfurizer, and its penetration time and penetration sulfur capacity still need to be further improved.
[0007] CN112516780A discloses a calcium-based desulfurizer and a preparation method thereof, wherein the calcium-based desulfurizer comprises the following components: calcium carbonate, calcium hydroxide, kaolin, pore-forming agent sodium silicate, water and sodium carboxymethyl cellulose CMC-Na, in parts by weight: 100-200 parts of light calcium carbonate, 300-500 parts of calcium hydroxide, 100-200 parts of kaolin, 20-50 parts of sodium silicate, 5-10 parts of CMC-Na, and 150-250 parts of water. The desulfurizer of the patent document has a high penetration sulfur capacity, but its penetration time is still short. Summary of the invention
[0008] In view of this, one object of the present invention is to provide a dry desulfurization agent, which has a high breakthrough sulfur capacity and a long breakthrough time. Another object of the present invention is to provide a method for preparing the dry desulfurization agent as described above.
[0009] The present invention adopts the following technical solutions to achieve the above-mentioned purpose.
[0010] In one aspect, the present invention provides a dry desulfurization agent, which is made of the following raw materials in parts by weight: 40 to 80 parts by weight of calcium hydroxide, 2 to 10 parts by weight of dihydrogen phosphate, 13 to 23 parts by weight of a moisturizer, 0.5 to 8.5 parts by weight of a regulator, 0.5 to 6.5 parts by weight of a pore former, and 0.5 to 20 parts by weight of a molding aid;
[0011] Wherein, the humidifier is selected from at least one of nitrates, chlorides and acetates; and the humidifier is used in the form of a humidifier aqueous solution;
[0012] Wherein, the regulator is selected from at least one of sodium carbonate and aluminum hydroxide.
[0013] The dry desulfurizer according to the present invention is preferably made of the following raw materials in parts by weight: 50-70 parts by weight of calcium hydroxide, 4-8 parts by weight of dihydrogen phosphate, 15-21 parts by weight of humidifier, 1.5-5.5 parts by weight of regulator, 1-4.5 parts by weight of pore former, and 1-10 parts by weight of molding aid.
[0014] The dry desulfurizer according to the present invention is preferably made of only the following raw materials in parts by weight: 40 to 80 parts by weight of calcium hydroxide, 2 to 10 parts by weight of dihydrogen phosphate, 13 to 23 parts by weight of a humidifier, 0.5 to 8.5 parts by weight of a regulator, 0.5 to 6.5 parts by weight of a pore-forming agent, and 0.5 to 20 parts by weight of a molding aid.
[0015] The dry desulfurizer according to the present invention is preferably made of only the following raw materials in parts by weight: 50-70 parts by weight of calcium hydroxide, 4-8 parts by weight of dihydrogen phosphate, 15-21 parts by weight of humidifier, 1.5-5.5 parts by weight of regulator, 1-4.5 parts by weight of pore former, and 1-10 parts by weight of molding aid.
[0016] According to the dry desulfurization agent of the present invention, preferably, the humidifier is selected from at least one of calcium nitrate, potassium nitrate, sodium nitrate, magnesium nitrate, calcium chloride, potassium chloride, sodium chloride, magnesium chloride, calcium acetate, potassium acetate, sodium acetate and magnesium acetate; in the humidifier aqueous solution, the concentration of the humidifier is above 30wt%.
[0017] According to the dry desulfurization agent of the present invention, preferably, the dihydrogen phosphate is selected from sodium dihydrogen phosphate or potassium dihydrogen phosphate.
[0018] According to the dry desulfurization agent of the present invention, preferably, the pore-forming agent is selected from at least one of sodium bicarbonate, urea, chitosan and copper oxalate; the molding aid is selected from at least one of diatomaceous earth, kaolin, attapulgite, bentonite, gypsum, citric acid, sesbania powder, carboxymethyl cellulose and aluminum dihydrogen phosphate.
[0019] According to the dry desulfurization agent of the present invention, preferably, the regulator is sodium carbonate; the pore-forming agent is chitosan; and the molding aid is carboxymethyl cellulose.
[0020] On the other hand, the present invention also provides a method for preparing the dry desulfurization agent as described above, comprising the following steps:
[0021] 1) mixing calcium hydroxide and a wetting agent aqueous solution to obtain an initial clay mixture; subjecting the initial clay mixture to a conditioning reaction to obtain a first clay mixture;
[0022] 2) mixing the first clay mixture with dihydrogen phosphate, a regulator, a pore-forming agent and a molding aid to obtain a second mixture;
[0023] 3) Extruding or tableting the second mixture to obtain a semi-finished desulfurizer;
[0024] 4) Drying the semi-finished desulfurizer to obtain a dry desulfurizer.
[0025] According to the preparation method of the present invention, preferably, the tempering reaction time is 2 to 6 hours; a granulating extruder is used for extrusion molding or a tablet press is used for tablet molding to obtain a semi-finished desulfurizer; the drying temperature is 100 to 200° C., and the drying time is 1 to 4 hours.
[0026] The dry desulfurizer of the present invention has a high penetration sulfur capacity, a long penetration time, and a long service life, which can solve the problems of low utilization rate of the desulfurizer and frequent material changes. At the same time, it can also remove dust particles in the flue gas during the desulfurization process, and can meet the long-term ultra-low sulfur dioxide emission requirements. The raw materials are widely available and the cost is low; the product is mainly calcium sulfate, which is conducive to subsequent processing and utilization. According to the preferred technical scheme of the present invention, the present invention adopts specific humidifiers, dihydrogen phosphates, regulators, pore-forming agents and calcium hydroxide for coordinated use, which is conducive to improving the microstructure of the desulfurizer, improving the migration ability of calcium ions, and improving the desulfurization reaction activity. The preparation method of the present invention is not complicated, and the equipment used is conventional equipment. It can be applied to fixed bed or moving bed dry flue gas desulfurization, which is conducive to promotion and application. DETAILED DESCRIPTION
[0027] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0028] <Dry desulfurization agent>
[0029] The dry desulfurizer of the present invention is made of the following raw materials in parts by weight: 40 to 80 parts by weight of calcium hydroxide, 2 to 10 parts by weight of dihydrogen phosphate, 13 to 23 parts by weight of a humidifier, 0.5 to 8.5 parts by weight of a regulator, 0.5 to 6.5 parts by weight of a pore-forming agent, and 0.5 to 20 parts by weight of a molding aid, wherein the humidifier is used in the form of a humidifier aqueous solution.
[0030] In the present invention, 13 to 23 parts by weight of the moisturizing agent refers to the amount of the moisturizing agent, not the amount of the moisturizing agent aqueous solution.
[0031] Preferably, the dry desulfurizer of the present invention is made of raw materials including the following parts by weight: 50-70 parts by weight of calcium hydroxide, 4-8 parts by weight of dihydrogen phosphate, 15-21 parts by weight of wetting agent, 1.5-5.5 parts by weight of regulator, 1-4.5 parts by weight of pore former, and 1-10 parts by weight of molding aid, wherein the wetting agent is used in the form of a wetting agent aqueous solution.
[0032] More preferably, the dry desulfurizer of the present invention is made of the following raw materials in parts by weight: 60-65 parts by weight of calcium hydroxide, 5-7 parts by weight of dihydrogen phosphate, 18-20 parts by weight of humidifier, 3-4 parts by weight of regulator, 2-3 parts by weight of pore-forming agent, and 2-5 parts by weight of molding aid, wherein the humidifier is used in the form of a humidifier aqueous solution. Such a dry desulfurizer can take into account both the penetration sulfur capacity and the penetration time, that is, the penetration sulfur capacity is higher and the penetration time is longer. This can improve the desulfurization efficiency, extend the service life, and reduce the number of times the desulfurizer is replaced.
[0033] In certain specific preferred embodiments, the dry desulfurizer of the present invention is made of only the following raw materials in parts by weight: 40 to 80 parts by weight of calcium hydroxide, 2 to 10 parts by weight of dihydrogen phosphate, 13 to 23 parts by weight of wetting agent, 0.5 to 8.5 parts by weight of regulator, 0.5 to 6.5 parts by weight of pore former, and 0.5 to 20 parts by weight of molding aid, wherein the wetting agent is used in the form of a wetting agent aqueous solution.
[0034] In other specific preferred embodiments, the dry desulfurizer of the present invention is made of only the following raw materials in parts by weight: 50-70 parts by weight of calcium hydroxide, 4-8 parts by weight of dihydrogen phosphate, 15-21 parts by weight of wetting agent, 1.5-5.5 parts by weight of regulator, 1-4.5 parts by weight of pore former, and 1-10 parts by weight of molding aid, wherein the wetting agent is used in the form of a wetting agent aqueous solution.
[0035] In some further specific preferred embodiments, the dry desulfurizer of the present invention is made of only the following raw materials in parts by weight: 60-65 parts by weight of calcium hydroxide, 5-7 parts by weight of dihydrogen phosphate, 18-20 parts by weight of wetting agent, 3-4 parts by weight of regulator, 2-3 parts by weight of pore former, and 2-5 parts by weight of molding aid, wherein the wetting agent is used in the form of a wetting agent aqueous solution.
[0036] In the present invention, the humidifier is selected from at least one of nitrates, chlorides and acetates. Nitrates are water-soluble nitrates, for example, can be selected from at least one of potassium nitrate, calcium nitrate, sodium nitrate, and magnesium nitrate. Chlorides can be selected from at least one of potassium chloride, sodium chloride, calcium chloride, and magnesium chloride. Acetates can be selected from at least one of calcium acetate, potassium acetate, sodium acetate, and magnesium acetate. Preferably, the humidifier is selected from one of calcium nitrate, sodium nitrate, magnesium chloride, and sodium acetate.
[0037] In the moisturizing agent aqueous solution of the present invention, the concentration of the moisturizing agent is above 30wt%, preferably 35-85wt%, more preferably 40-75wt%, for example, 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, 65wt%.
[0038] The present invention surprisingly found that when the humidifier is used in the form of a humidifier aqueous solution, the penetration sulfur capacity and penetration time of the obtained dry desulfurizer can be significantly improved. The present invention believes that the humidifier is used to improve the hydrophilicity of the inner and outer surfaces of the desulfurizer material, the moisture adsorbed on the surface of calcium hydroxide has an important influence on the desulfurization reaction, the diffusion and dissolution of sulfur dioxide gas into the liquid film is the key to controlling the reaction rate, and the humidifier can increase the local moisture content due to its hygroscopic characteristics, creating a liquid phase environment that is conducive to gas absorption and improving the desulfurization reaction activity.
[0039] In the present invention, the dihydrogen phosphate is selected from sodium dihydrogen phosphate or potassium dihydrogen phosphate, preferably potassium dihydrogen phosphate. The present invention believes that the dihydrogen phosphate can promote ion diffusion, and is used to enhance the calcium ion migration ability, replace the position of calcium ions in the crystal lattice by metal ions, increase the degree of crystal defects, increase the defect concentration in the product layer, and promote the diffusion and transfer of calcium ions to cause desulfurization reaction.
[0040] In the present invention, the regulator is selected from at least one of sodium carbonate and aluminum hydroxide, preferably sodium carbonate. The present invention believes that the regulator can be used to buffer the change of local alkalinity after the desulfurization reaction occurs and maintain a relatively high local alkalinity.
[0041] In the present invention, the pore-forming agent is selected from at least one of sodium bicarbonate, urea, chitosan and copper oxalate, preferably selected from one of urea, chitosan and copper oxalate, and more preferably chitosan. The present invention believes that these pore-forming agents are used to increase the contact reaction area of the material, inhibit the coverage of the product layer, and improve the utilization rate of the material.
[0042] In the present invention, the molding aid is selected from at least one or more of diatomaceous earth, kaolin, attapulgite, bentonite, gypsum, citric acid, sesbania powder, carboxymethyl cellulose and aluminum dihydrogen phosphate. Preferably, the molding aid is selected from one of citric acid, sesbania powder and carboxymethyl cellulose. More preferably, the molding aid is carboxymethyl cellulose.
[0043] According to a specific embodiment of the present invention, the dry desulfurizer of the present invention is made of only the following raw materials in parts by weight: 40 to 80 parts by weight of calcium hydroxide, 2 to 10 parts by weight of dihydrogen phosphate, 13 to 23 parts by weight of a humidifier, 0.5 to 8.5 parts by weight of a regulating agent sodium carbonate, 0.5 to 6.5 parts by weight of a pore-forming agent chitosan, and 0.5 to 20 parts by weight of a molding aid carboxymethyl cellulose; wherein the humidifier is used in the form of an aqueous solution of the humidifier; in the aqueous solution of the humidifier, the concentration of the humidifier is above 30wt%.
[0044] The dry desulfurizer of the present invention is particularly suitable for removing SO2 from flue gas. The SO2 penetration sulfur capacity of the dry desulfurizer of the present invention is above 11.5%, preferably above 13%, more preferably above 14%, and can reach 16.9%; the SO2 penetration time of the dry desulfurizer of the present invention is above 40h, preferably above 42h, more preferably above 43.5h, and can reach 48.5h.
[0045] <Preparation method>
[0046] The present invention also provides a method for preparing the dry desulfurization agent as described above, comprising the following steps: (1) forming a first sludge mixture; (2) forming a second mixture; (3) forming a semi-finished desulfurization agent; (4) obtaining the dry desulfurization agent. Optionally, the method further comprises preparing a humidifying agent aqueous solution.
[0047] First mud mixture forming step
[0048] The humidifier is formulated as an aqueous humidifier solution. Calcium hydroxide and the humidifier aqueous solution are mixed to obtain an initial mud mixture; the initial mud mixture is subjected to a tempering reaction to obtain a first mud mixture. The present invention finds that the use of a specific humidifier aqueous solution to first react with calcium hydroxide for tempering is beneficial to improving the penetration sulfur capacity and penetration time of the resulting dry desulfurizer. In the present invention, the tempering reaction specifically includes: allowing the initial mud mixture to stand, and during the standing process, intermittently adding a small amount of water and stirring the mixture to keep it in a wet mud state. When adding water, water can be sprayed by a spray device for wetting. The amount of water added each time can be 0.02 to 1.2 times the amount of water in the humidifier aqueous solution. The tempering reaction time is 2 to 6 hours, preferably 2 to 5 hours, and more preferably 3 to 4 hours.
[0049] The present invention believes that, on the one hand, the humidifier aqueous solution forms grooves on the surface of the calcium hydroxide single crystal to increase the roughness through the tempering effect, improves the microstructure of the calcium hydroxide, increases the reaction contact area, and adjusts the growth mode of the desulfurization product layer; on the other hand, the alkali metal salt substances therein can be evenly dispersed and attached to the inner and outer surfaces of the calcium hydroxide after dissolution and recrystallization, thereby enhancing the absorption and dissolution of sulfur dioxide under water conditions, thereby effectively improving the desulfurization reaction activity.
[0050] In the present invention, the humidifier aqueous solution can be prepared by dissolving the humidifier in water and stirring evenly. The specific type and amount of the humidifier are described above and will not be described here.
[0051] Second mixture forming step
[0052] The first mud mixture is mixed with dihydrogen phosphate, a regulator, a pore-forming agent and a molding aid to obtain a second mixture.
[0053] According to one embodiment of the present invention, the first clay mixture is mixed with potassium dihydrogen phosphate, a regulator, a pore-forming agent and a molding aid in a mixer to obtain a second mixture. The mixing time may be 20 to 40 minutes, preferably 20 to 30 minutes.
[0054] The dosage of dihydrogen phosphate is described above, which will not be repeated here. The specific types and dosages of the regulator, pore-forming agent and molding aid are described above, which will not be repeated here.
[0055] Steps for forming semi-finished desulfurizer
[0056] The second mixture is extruded or tableted to obtain a semi-finished desulfurizer.
[0057] According to one embodiment of the present invention, a semi-finished desulfurizing agent is obtained by extrusion molding using a granulating extruder or tablet molding using a tablet press.
[0058] The semi-finished desulfurizer may be in the shape of a column, a four-leaf clover or a sheet. According to one embodiment of the present invention, the semi-finished desulfurizer is in the shape of a column.
[0059] Steps for obtaining dry desulfurization agent
[0060] The semi-finished desulfurizer is dried to obtain a dry desulfurizer.
[0061] The drying temperature is 100 to 200° C., preferably 150 to 190° C., more preferably 150 to 180° C. The drying time is 1 to 4 hours, preferably 1 to 3 hours, more preferably 2 to 3 hours.
[0062] In the present invention, a drying device such as a mesh belt kiln or a rotary kiln can be used for drying to obtain a dry desulfurization agent.
[0063] Unless otherwise specified, in the following examples, the parts mentioned are parts by weight.
[0064] Embodiments 1 to 4
[0065] According to the formula in Table 1, the dry desulfurization agent is prepared in the following steps:
[0066] Dissolve the humidifier in water to prepare a humidifier aqueous solution. Evenly mix calcium hydroxide and the humidifier aqueous solution to obtain an initial clay mixture in a slightly wet clay state; subject the initial clay mixture to a tempering reaction for 2 hours in a static state (the tempering reaction specifically includes: allowing the initial clay mixture to stand, and during the standing process, intermittently adding a small amount of water and stirring the mixture to keep it in a wet clay state. When adding water, water can be sprayed by a spray device to moisten it) to obtain a first clay mixture.
[0067] The first mud mixture was mixed with potassium dihydrogen phosphate, a regulator, sodium carbonate, a pore-forming agent, chitosan, and a molding aid, carboxymethyl cellulose, in a mixer for 20 minutes to obtain a second mixture.
[0068] The second mixture is extruded in a granulator to obtain a semi-finished desulfurizer, and the semi-finished desulfurizer is placed in a mesh belt kiln and baked at 150° C. for 2 hours to obtain a columnar dry desulfurizer.
[0069] Table 1
[0070]
[0071] Comparative Example 1
[0072] 60 parts of calcium hydroxide, 18 parts of calcium chloride, 5 parts of potassium dihydrogen phosphate, 3 parts of sodium carbonate as a regulator, 2 parts of chitosan as a pore-forming agent, and 2 parts of carboxymethyl cellulose as a molding aid are mixed in a mixer for 20 minutes to obtain a mixture. The mixture is extruded in a granulator to obtain a semi-finished desulfurizer. The semi-finished desulfurizer is placed in a mesh belt kiln and baked at 150°C for 2 hours to obtain a columnar dry desulfurizer.
[0073] Comparative Example 2
[0074] 78 parts of calcium hydroxide, 5 parts of potassium dihydrogen phosphate, 3 parts of sodium carbonate as a regulator, 2 parts of chitosan as a pore-forming agent, and 2 parts of carboxymethyl cellulose as a molding aid are mixed in a mixer for 20 minutes to obtain a mixture. The mixture is extruded in a granulator to obtain a semi-finished desulfurizer. The semi-finished desulfurizer is placed in a mesh belt kiln and baked at 150°C for 2 hours to obtain a columnar dry desulfurizer.
[0075] The dry desulfurizers obtained in Examples 1 to 4 and Comparative Examples 1 to 2 were tested respectively, and the breakthrough time and breakthrough sulfur capacity were calculated. The results are shown in Table 2.
[0076] The test method is as follows: Use Testo 340 to detect sulfur dioxide concentration. Simulate fixed bed reaction device, at a temperature of 120°C, an oxygen content of 10%, a moisture content of 5%, and a SO2 concentration of 200mg / m 3 , reaction space velocity 1000h -1 , detect the SO2 concentration of sulfur-containing flue gas before and after desulfurization treatment. When the SO2 concentration reaches 35mg / m 3 Stop the test and calculate the breakthrough time and breakthrough sulfur capacity (the breakthrough sulfur capacity is the capacity of the desulfurizer to absorb sulfur dioxide).
[0077] The calculation formula of the breakthrough sulfur capacity is: breakthrough sulfur capacity = (weight M1 of the dry desulfurization agent after absorbing sulfur dioxide - initial weight M0 of the dry desulfurization agent) / initial weight M0 of the dry desulfurization agent × 100%.
[0078] The penetration time refers to the time from the sulfur-containing flue gas being treated with the desulfurizer to the time when the concentration of SO2 in the sulfur-containing flue gas after being treated with the desulfurizer reaches 35mg / m 3 Length of time.
[0079] Table 2
[0080] project Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Penetration time / h 43.5 42.6 40.2 48.5 10.7 10.2 Sulfur breakthrough capacity% 14.6 13.2 11.8 16.9 5 4.9
[0081] From the comparison between the examples and the comparative examples, it can be seen that the dry desulfurizer of the present invention has high sulfur penetration capacity and long duration, which improves the utilization rate of the desulfurizer. Preferably, the SO2 penetration capacity of the dry desulfurizer of Example 4 of the present invention reaches 16.9%, and the penetration time is as long as 48.5h.
[0082] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.
Claims
1. A dry desulfurization agent, It is characterized in that The invention is prepared from the following raw materials in parts by weight: 40 to 80 parts by weight of calcium hydroxide, 2 to 10 parts by weight of dihydrogen phosphate, 13 to 23 parts by weight of a moisturizer, 0.5 to 8.5 parts by weight of a regulator, 0.5 to 6.5 parts by weight of a pore-forming agent, and 0.5 to 20 parts by weight of a molding aid. Wherein, the humidifier is selected from at least one of nitrates, chlorides and acetates; and the humidifier is used in the form of a humidifier aqueous solution; Wherein, the regulator is selected from at least one of sodium carbonate and aluminum hydroxide.
2. The dry desulfurization agent according to claim 1, It is characterized in that The invention is prepared from the following raw materials in parts by weight: 50-70 parts by weight of calcium hydroxide, 4-8 parts by weight of dihydrogen phosphate, 15-21 parts by weight of a moisturizing agent, 1.5-5.5 parts by weight of a regulating agent, 1-4.5 parts by weight of a pore-forming agent and 1-10 parts by weight of a molding aid.
3. The dry desulfurization agent according to claim 1, It is characterized in that The invention is prepared from the following raw materials in parts by weight: 40-80 parts by weight of calcium hydroxide, 2-10 parts by weight of dihydrogen phosphate, 13-23 parts by weight of a moisturizer, 0.5-8.5 parts by weight of a regulator, 0.5-6.5 parts by weight of a pore-forming agent and 0.5-20 parts by weight of a molding aid.
4. The dry desulfurization agent according to claim 1, It is characterized in that The invention is prepared from the following raw materials in parts by weight: 50-70 parts by weight of calcium hydroxide, 4-8 parts by weight of dihydrogen phosphate, 15-21 parts by weight of a moisturizing agent, 1.5-5.5 parts by weight of a regulating agent, 1-4.5 parts by weight of a pore-forming agent and 1-10 parts by weight of a molding aid.
5. The dry desulfurization agent according to claim 1, It is characterized in that The humidifier is selected from at least one of calcium nitrate, potassium nitrate, sodium nitrate, magnesium nitrate, calcium chloride, potassium chloride, sodium chloride, magnesium chloride, calcium acetate, potassium acetate, sodium acetate and magnesium acetate; the concentration of the humidifier in the humidifier aqueous solution is above 30wt%.
6. The dry desulfurization agent according to claim 1, It is characterized in that The dihydrogen phosphate is selected from sodium dihydrogen phosphate or potassium dihydrogen phosphate.
7. The dry desulfurization agent according to claim 1, It is characterized in that The pore-forming agent is selected from at least one of sodium bicarbonate, urea, chitosan and copper oxalate; the molding aid is selected from at least one of diatomaceous earth, kaolin, attapulgite, bentonite, gypsum, citric acid, sesbania powder, carboxymethyl cellulose and aluminum dihydrogen phosphate.
8. The dry desulfurization agent according to claim 7, It is characterized in that The regulator is sodium carbonate; the pore-forming agent is chitosan; and the molding aid is carboxymethyl cellulose.
9. A method for preparing a dry desulfurization agent according to any one of claims 1 to 8, It is characterized in that The following steps are involved: 1) mixing calcium hydroxide and a wetting agent aqueous solution to obtain an initial clay mixture; subjecting the initial clay mixture to a conditioning reaction to obtain a first clay mixture; 2) mixing the first clay mixture with dihydrogen phosphate, a regulator, a pore-forming agent and a molding aid to obtain a second mixture; 3) Extruding or tableting the second mixture to obtain a semi-finished desulfurizer; 4) Drying the semi-finished desulfurizer to obtain a dry desulfurizer.
10. The preparation method according to claim 9, It is characterized in that The time of the conditioning reaction is 2 to 6 hours; the semi-finished desulfurizer is obtained by extrusion molding using a granulating extruder or tablet molding using a tablet press; the drying temperature is 100 to 200° C., and the drying time is 1 to 4 hours.