Low-porosity aluminum alloy additive manufacturing method based on material component control
By optimizing the elemental composition of Si and Mg in aluminum alloy additive manufacturing and using cold wire arc welding methods, the problem of pores in aluminum alloy additives is solved, the mechanical properties are significantly improved, and a method of improvement directly from raw materials is provided, which is suitable for for aluminum alloys and other materials.
Patent Information
- Application Number
- CN202410999070.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-01
AI Technical Summary
There is a lack of effective methods to solve the porosity problem in existing aluminum alloy additive manufacturing, which affects mechanical properties. Most improvement methods focus on equipment and methods in the process stage, while there is less research on the impact of raw material composition.
By controlling the Si and Mg elemental components in the aluminum alloy wire, cold wire arc welding is used for additive manufacturing, and the composition ratio of the welding wire is optimized to reduce pores and improve mechanical properties.
Under the same process parameters, by optimizing the content of Si and Mg elements, pore defects are significantly reduced and the mechanical properties of aluminum alloys are improved, providing a simple and economical method to improve directly from raw materials.
Smart Images

Figure CN118720523A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of additive manufacturing, and in particular relates to a low-porosity aluminum alloy additive manufacturing method based on material composition control. Background Art
[0002] Aluminum alloys are widely used in aerospace, automotive and shipbuilding industries due to their excellent properties in many aspects. They have high specific strength, excellent corrosion and heat resistance, good electrical conductivity and light weight. The cold metal transfer welding technology in arc additive manufacturing perfectly matches the welding requirements of low melting point aluminum alloys due to its low heat input and high deposition efficiency. However, pores are one of the most common and difficult defects in aluminum alloy welding. The size, distribution and number of pores greatly affect the mechanical properties of aluminum alloy components.
[0003] At present, there is no good way to solve the problem of pores in the aluminum alloy printing process, which greatly affects the mechanical properties. Other existing methods require complex equipment modifications, which are not as direct, simple and economical as the method of directly improving the raw materials. Moreover, most people's current methods for improving pores mainly focus on the additional equipment and methods in the process stage, and there is little research on the impact of the composition of the raw materials. Summary of the invention
[0004] The object of the present invention is to provide a method for additive manufacturing of low porosity aluminum alloy based on material composition control and to provide at least the advantages to be described below.
[0005] Another object of the present invention is to provide a low-porosity aluminum alloy additive manufacturing method based on material composition control. By controlling the content of the elemental components Si and Mg, the porosity of the aluminum alloy component is successfully further reduced, thereby obtaining excellent mechanical properties.
[0006] The technical solution of the present invention is as follows:
[0007] The low porosity aluminum alloy additive manufacturing method based on material composition control comprises the following steps:
[0008] Providing aluminum alloy wire, wherein the mass fraction of Si is 0.01%-0.2%, and the mass fraction of Mg is 0.0001%-0.1%;
[0009] The aluminum alloy wire is melted on the aluminum alloy substrate by cold wire arc welding method for additive manufacturing.
[0010] Preferably, in the low-porosity aluminum alloy additive manufacturing method based on material composition control, in the cold wire arc welding method, the current is 123A, the voltage is 17.4V, the wire feeding speed is 5.4m / min, the welding movement speed is 10mm / s, and the interlayer temperature is 120°C.
[0011] Preferably, in the low-porosity aluminum alloy additive manufacturing method based on material composition control, the mass fraction of Si is 0.1%-0.2%, and the mass fraction of Mg is 0.0001%-0.002%.
[0012] Preferably, in the low-porosity aluminum alloy additive manufacturing method based on material composition control, the mass fraction of Si is 0.01%-0.04%, and the mass fraction of Mg is 0.0001%-0.002%.
[0013] Preferably, in the low-porosity aluminum alloy additive manufacturing method based on material composition control, the mass fraction of Si is 0.04%-0.1%, and the mass fraction of Mg is 0.04%-0.1%.
[0014] The present invention has the following beneficial effects:
[0015] 1. The present invention starts with the material composition and finds that under the same process parameters, the ratio of elements in the aluminum alloy material composition has a significant effect on the porosity defects in the arc additive manufacturing process, and the mechanical properties are also improved to a certain extent;
[0016] 2. It can clearly reduce the porosity content from a macroscopic perspective rather than a microscopic perspective, thereby improving the mechanical properties of aluminum alloys.
[0017] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 Metallographic images of cross sections of aluminum alloy wires in three embodiments of the low-porosity aluminum alloy additive manufacturing method based on material composition control provided by the present invention;
[0019] Figure 2 Surface images of a single wall of additive material produced by three embodiments of the low-porosity aluminum alloy additive manufacturing method based on material composition control provided by the present invention;
[0020] Figure 3 Metallographic images of a single wall section of an additive material produced by three embodiments of the low-porosity aluminum alloy additive manufacturing method based on material composition control provided by the present invention;
[0021] Figure 4 Industrial CT images of a single wall of additive manufacturing produced by three embodiments of the low-porosity aluminum alloy additive manufacturing method based on material composition control provided by the present invention;
[0022] Figure 5A large-scale metallographic structure diagram of an additive material produced by an embodiment of the low-porosity aluminum alloy additive manufacturing method based on material composition control provided by the present invention. DETAILED DESCRIPTION
[0023] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.
[0024] The present invention optimizes the material composition of the aluminum alloy and controls the contents of several key elements therein, thereby achieving the purpose of reducing the H content after welding, reducing pores, and improving the longitudinal mechanical properties of the aluminum alloy.
[0025] The invention mainly improves the defects of the aluminum alloy component and improves its mechanical properties by optimizing the composition ratio of two elements of the welding wire.
[0026] 1. Reduce the amount and distribution of inclusions in the sample by reducing the content of Si element;
[0027] 2. Increase the content of Mg element to promote Mg to capture as much H in the aluminum alloy as possible, reduce the content of free H, and reduce the formation of pores.
[0028] By controlling the two elements, minimal defects and excellent mechanical properties can be obtained.
[0029] The method for suppressing the number and size of pores in the aluminum alloy additive process is to select the optimal welding material, which is an aluminum alloy wire with different mass fractions of Si and Mg elements, and is divided into three different compositions: high Si, low Mg; low Si, low Mg and medium Si, high Mg.
[0030] The arc additive process parameters are shown in Table 1, that is, all cases are made with the same parameters, thus eliminating the influence of external factors such as process parameters, and only comparing the influence of element composition on pore defects and performance.
[0031] Table 1 Process parameters of arc additive process
[0032]
[0033] Defect and performance evaluation method: After welding, the cross section is taken to evaluate the porosity defect and mechanical properties. During the experiment, the H element is tested on the raw material welding wire, and then the H element is also tested on the components after the additive process.
[0034] The H element results of different embodiments are shown in Table 2.
[0035] Finally, the component is stretched in the longitudinal direction, which is the weakest direction of the component. The results of different embodiments are shown in Table 3.
[0036] The specific embodiments are as follows:
[0037] Embodiment 1
[0038] The aluminum alloy wire has a high Si content and a low Mg content, that is, the mass fraction of Si is 0.1%-0.2%, and the mass fraction of Mg is 0.0001%-0.002%.
[0039] Wire cross section: Figure 1 As shown in (a), after polishing, sporadic granular inclusions appeared in the core of the welding wire cross section, which are suspected to be type C silicate inclusions of non-metallic inclusions in the national standard.
[0040] Single wall surface quality: Figure 2 As shown in (a), the outermost surface shows many granular slag inclusions and small pores.
[0041] Porosity defects: such as Figure 3 (a) and Figure 4 As shown in (a), a large number of pores are distributed between the layers, and millimeter-scale pores appear.
[0042] Comparison of H content before and after additive manufacturing: more H elements remain before and after additive manufacturing.
[0043] Mechanical properties: Overall performance is poor and tensile yield is low.
[0044] Embodiment 2
[0045] The aluminum alloy wire has low Si content and low Mg content, that is, the mass fraction of Si is less than 0.01%-0.04%, and the mass fraction of Mg is 0.0001%-0.002%.
[0046] Wire cross section: Figure 1 As shown in (b), after polishing, there are no obvious inclusions in the core of the welding wire.
[0047] Single wall surface quality: Figure 2 As shown in (b), there are almost no granular slag inclusions and small pores on the outermost surface.
[0048] Porosity defects: such as Figure 3 (b) and Figure 4 As shown in (b), the pores are reduced and a small amount is distributed between the layers.
[0049] Comparison of H content before and after additive manufacturing: The residual H element before and after additive manufacturing is less than the elemental composition sample of Case 1.
[0050] Mechanical properties: Overall performance is moderate, with slightly increased tensile yield.
[0051] Embodiment 3
[0052] An aluminum alloy with a moderate Si content and a high Mg content, that is, the mass fraction of Si is 0.04%-0.1%, and the mass fraction of Mg is 0.04%-0.1%.
[0053] Wire cross section: Figure 1 As shown in (c), after polishing, there are no obvious inclusions in the core of the welding wire.
[0054] Single wall surface quality: Figure 2 As shown in (c), the outermost surface is clean, with almost no granular slag inclusions and small pores.
[0055] Porosity defects: such as Figure 3 (c) and Figure 4 (c) As shown, the pores are reduced and very few are distributed between the layers.
[0056] Comparison of H content before and after additive manufacturing: The H content before additive manufacturing was the same as other cases, but the H content was greatly reduced after additive manufacturing. It is speculated that the Mg element has a certain adsorption and repair effect.
[0057] Mechanical properties: The overall performance is good, the tensile yield strength is high, and the elongation is also excellent.
[0058] Table 2. Mechanical properties of different cases
[0059] Wire H content (wt%) H content in the component after additive manufacturing (wt%) Example 1 0.0015 0.0004 Example 2 0.0013 0.0003 Example 3 0.0019 0.0001
[0060] Table 3 Mechanical properties of different cases
[0061] Tensile strength(MPa) Yield strength(MPa) Elongation(%) Example 1 220±1 98±1 9.5±0.5 Example 2 232±5 105±2 9±0.5 Example 3 255±1 127±1 12±0.5
[0062] According to different implementation cases, the material of Example 3 is in the optimal state of arc additive manufacturing based on the comprehensive porosity and mechanical properties. Figure 5 shown.
[0063] The present invention successfully suppresses the porosity problem in aluminum alloy arc additive manufacturing components by optimizing the element composition of the welding wire, improves the overall mechanical properties, and provides a new idea for defect optimization and improvement of metal arc additive manufacturing. At the same time, this method is not only applicable to aluminum alloys, but also to other materials such as copper alloys.
[0064] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.
Claims
1. A low porosity aluminum alloy additive manufacturing method based on material composition control, characterized in that: The following steps are involved: Providing aluminum alloy wire, wherein the mass fraction of Si is 0.01%-0.2%, and the mass fraction of Mg is 0.0001%-0.1%; The aluminum alloy wire is melted on the aluminum alloy substrate by cold wire arc welding method for additive manufacturing.
2. The low porosity aluminum alloy additive manufacturing method based on material composition control according to claim 1, characterized in that: In the cold wire arc welding method, the current is 123A, the voltage is 17.4V, the wire feeding speed is 5.4m / min, the welding moving speed is 10mm / s, and the interlayer temperature is 120°C.
3. The low porosity aluminum alloy additive manufacturing method based on material composition control according to claim 2, characterized in that: The mass fraction of Si is 0.1%-0.2%, and the mass fraction of Mg is 0.0001%-0.002%.
4. The low porosity aluminum alloy additive manufacturing method based on material composition control according to claim 2, characterized in that: The mass fraction of Si is 0.01%-0.04%, and the mass fraction of Mg is 0.0001%-0.002%.
5. The low porosity aluminum alloy additive manufacturing method based on material composition control according to claim 2, characterized in that: The mass fraction of Si is 0.04%-0.1%, and the mass fraction of Mg is 0.04%-0.1%.