High-strength aluminum-coated plate strip for corrosion-resistant structure and production method of high-strength aluminum-coated plate strip

By optimizing the chemical composition and process of aluminum-clad panels and strips, the deficiencies in steel-aluminum bonding performance and high strength in the existing technology have been solved, and aluminum-clad panels and strips with high yield strength and tensile strength have been achieved, which are suitable for high-strength corrosion-resistant structures. production, reducing production costs and painting requirements.

CN118721886AActive Publication Date: 2024-10-01BAOSHAN IRON & STEEL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310333023.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-01
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

Existing aluminum-clad strips have deficiencies in steel-aluminum bonding performance and high strength, especially in terms of width and production efficiency, which cannot meet the production needs of high-strength, corrosion-resistant structures.

Method used

By optimizing the chemical composition of the steel strip, including controlling the content of C, Si, Mn, P, S, Al, O, N, B, Ti, Nb, Cu, Cr, Ca and other elements, to meet the specific composition relationship formula, To achieve high yield strength, tensile strength and steel-aluminum bonding properties, room temperature rolling and annealing processes are adopted. The annealing temperature is controlled between 480 and 530°C. The annealing time is related to the steel coil specification and combined with finishing treatment.

Benefits of technology

An aluminum-clad strip with yield strength ≥350MPa and tensile strength ≥420MPa was obtained. It has good steel-aluminum bonding performance and surface quality, is suitable for the production of high-strength corrosion-resistant structures, and reduces production costs and painting requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118721886A_ABST
    Figure CN118721886A_ABST
Patent Text Reader

Abstract

The invention relates to a high-strength aluminum-coated plate strip for a corrosion-resistant structure and a production method of the high-strength aluminum-coated plate strip, the high-strength aluminum-coated plate strip is formed by coating a steel strip and an aluminum strip, the steel strip comprises the following chemical components in percentage by weight: 0.04-0.09% of C, 0 < Si < = 0.005%, 0.4-0.8% of Mn, 0.008-0.020% of P, < = 0.008% of S, 0 < Al < = 0.005%, 0.012-0.030% of N, 0 < O < = 0.01%, 0.0005-0.002% of B, one or more of 0.01-0.06% of Ti, 0.01-0.03% of Nb, 0.01-0.15% of Cu, 0.03-0.60% of Cr and 0.001-0.004% of Ca, and the balance of Fe and other inevitable impurities; the conditions that 0.5 C + 3.83 N + O-0. 89 Al-1.15 Si is greater than or equal to 0.08 are met at the same time; 150 (C-0.01) + 60P + 300N + 5Mn is greater than or equal to 13.0. The aluminum-coated plate strip has good steel-aluminum bonding performance, stamping and drawing performance and surface quality, can adapt to high-temperature nitriding or other high-temperature treatment, and meanwhile keeps good steel-aluminum bonding performance and cold bending performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of low alloy steel manufacturing, and specifically relates to a high-strength aluminum-clad plate strip for corrosion-resistant structures and a production method thereof. Background Art

[0002] Aluminum-clad strip is a composite strip formed by rolling an aluminum layer on the surface of strip steel at room temperature. It has both steel-aluminum structure and steel-aluminum-steel or aluminum-steel-aluminum structure. Aluminum-clad strip has the strength of steel and the characteristics of aluminum such as good heat dissipation, corrosion resistance, light weight and beautiful appearance. Compared with pure aluminum materials, it greatly reduces the cost, so it has been widely used in radiators, corrosion-resistant pipes, home appliance panels and other fields, and has gradually expanded to automobile engine protective covers, new energy vehicle parts, atmospheric corrosion resistance, cookers, construction and other fields.

[0003] In order to extend the service life, current container plates mostly use weathering steel, and its composition system needs to add many corrosion-resistant alloy elements; at the same time, in order to achieve high strength and weight reduction, some strengthening elements such as Ti and Nb need to be added, which significantly increases the cost. At the same time, weathering steel is overall corrosion-resistant, and the corrosion of steel structures mainly occurs on the surface of the material. The many corrosion-resistant alloys added inside the steel plate cannot fully play their role, which is also a waste of resources.

[0004] Aluminum is not only light, beautiful, and has good heat dissipation, but also has excellent corrosion resistance in atmospheric environments. Aluminum is an active metal that easily reacts chemically with oxygen in the air to form aluminum oxide, forming a dense film of micron thickness on the surface to prevent corrosion from deepening. In industrial atmospheric environments, the corrosion rate of aluminum is about 1μm / a, and its corrosion resistance is about 10 times that of conventional atmospheric corrosion-resistant steel. Therefore, the use of aluminum-clad plates to make container plates, corrosion-resistant components, etc. not only has excellent corrosion resistance, but also has a beautiful surface. Therefore, the surface of aluminum does not need to be painted, reducing the painting process, which not only reduces costs, but is also more energy-saving and environmentally friendly.

[0005] Chinese patent CN101660087 discloses "an aluminum-steel-aluminum composite material and its preparation method", which cold-rolls aluminum and steel into high-precision aluminum strips and steel strips respectively after surface treatment, and then cold-rolls them into high-precision aluminum-steel-aluminum composite strips again, and anneals them at 650-850℃ for 1-4 hours. Since the melting point of aluminum is about 640℃, annealing at such a high temperature seriously deteriorates the interface bonding strength between steel and aluminum. It cannot meet the performance and surface quality requirements of the current aluminum-clad strip application field.

[0006] Chinese patent CN102019727 discloses "aluminum-coated steel strip for cooler and its preparation method and steel strip and aluminum alloy strip used therein". This patent mainly relates to aluminum-coated steel strip for heat dissipation and its substrate, with a width not exceeding 500m.

[0007] The aluminum-clad materials involved in the Chinese patent CN107881410A, "A kind of aluminum-clad strip with excellent heat dissipation effect and its production method" and the Chinese patent CN108796384A, "A kind of aluminum-clad strip with high surface quality and its production method that is easy to stamp and process", are mainly used for the production of radiators, home appliance panels, etc., with a width of no more than 500m and low strength. Therefore, these two patents are significantly different from the present invention in terms of function and application field.

[0008] The "high-strength aluminum-clad strip and its manufacturing method" disclosed in Chinese patent CN107781426A ensures the steel-aluminum bonding performance of the aluminum-clad strip by controlling N and O and Si and Al, and has a yield strength of 280-400MPa, but contains up to 0.05% O (oxygen), which will lead to more defects such as pores and slag inclusions inside and on the surface of the ingot, increase the difficulty of cleaning the ingot, make the surface of the strip prone to warping defects, and reduce the yield rate. In addition, the aluminum-clad strip described in the application has the problem of insufficient width in terms of specifications, and when used for processing corrosion-resistant components such as containers, there are many splicing passes and low production efficiency, which increases production costs.

[0009] Chinese patent CN114250411A discloses "an aluminum-clad strip for kitchenware and its production method". The aluminum-clad strip used in the production of frying pans also involves nitriding treatment during the processing, and proposes strength requirements after nitriding. However, the aluminum-clad strip only requires a tensile strength of ≥320MPa, and the yield and tensile strength of the substrate used are ≤280MPa and 380MPa, respectively, which is significantly lower than the present invention. In addition, in terms of composition, the steel strip involved in the patent requires the carbon content to be controlled below 0.005%, and the P and S contents are limited to no more than 0.012% and 0.006%, respectively, which increases the difficulty of steelmaking and production costs. In terms of application areas, the application is limited to the processing of aluminum-clad materials for frying pans, and the thickness of the aluminum layer accounts for about 40-60% of the total thickness; and the width of the produced strip does not exceed 460mm.

[0010] From the comparison results, it can be seen that the existing steel-aluminum composite strips either have poor steel-aluminum bonding performance or do not meet the high strength requirements, especially the general width does not exceed 500mm. They are mainly used in radiators, home appliance panels, food trays and other fields, mainly using the high heat dissipation coefficient of aluminum. Summary of the invention

[0011] The purpose of the present invention is to provide a high-strength aluminum-clad strip for corrosion-resistant structures and a production method thereof. The aluminum-clad strip has high strength, good steel-aluminum bonding performance, stamping and drawing performance and surface quality, and its yield strength is ≥350MPa, tensile strength is ≥420MPa, and elongation A50 is ≥18%. At the same time, it maintains good cold bending performance and meets the requirements of D=1a and 180° cold bending. The product is suitable for the production and processing of high-strength corrosion-resistant structures, and has the characteristics of corrosion resistance, good heat dissipation performance, easy cold forming processing, beautiful appearance, and no painting.

[0012] To achieve the above object, the technical solution of the present invention is:

[0013] A high-strength aluminum-clad plate strip for corrosion-resistant structure, which is a steel strip and an aluminum strip laminated, wherein the chemical composition weight percentage of the steel strip is: C: 0.04-0.09%, 0<Si≤0.005%, Mn: 0.4-0.8%, P: 0.008-0.020%, S≤0.008%, 0<Al≤0.005%, N: 0.012-0.030%, 0<O≤0.01%, B: 0.0005-0.002%, and one or more of Ti: 0.01-0.06%, Nb: 0.01-0.03%, Cu: 0.01-0.15%, Cr: 0.03-0.60%, Ca: 0.001-0.004% is selectively added, and the balance contains Fe and other unavoidable impurities; and it is necessary to simultaneously meet the following requirements:

[0014] 0.5C+3.83N+O-0.89Al-1.15Si≥0.08;

[0015] 150(C-0.01)+60P+300N+5Mn≥13.0.

[0016] Furthermore, the balance is Fe and other inevitable impurities.

[0017] The steel strip of the present invention has a yield strength of ≥300 MPa, a tensile strength of ≥360 MPa, and an elongation of ≥30%.

[0018] The yield strength of the aluminum-clad plate strip of the present invention is ≥350MPa, the tensile strength is ≥420MPa, and the elongation A50 is ≥18%.

[0019] The aluminum-clad plate strip of the present invention is a steel-aluminum, aluminum-steel-aluminum or steel-aluminum-steel structure.

[0020] In the chemical composition design of the steel strip of the aluminum-clad plate strip of the present invention:

[0021] C improves yield strength through solid solution strengthening and phase transformation strengthening, while inhibiting the diffusion of Al in steel and the formation of iron-aluminum compounds. Too high C content is not good for the subsequent processing properties of the material such as stamping and drawing; however, higher C is easy to be concentrated at defective positions such as dislocations, which is not good for surface quality. According to the actual steelmaking process, the present invention controls the C content to 0.04-0.09%.

[0022] Si is a deoxidizing element and also a solid solution strengthening element, which increases the yield strength and reduces the elongation. Although an appropriate amount of Si is beneficial to improving the steel-aluminum interface bonding performance, it will also weaken the inhibitory effect of O (oxygen) on the formation of a brittle compound layer at the steel-aluminum interface. Therefore, the present invention controls 0<Si≤0.005%.

[0023] Mn is also a common strengthening element in steel. It increases yield strength and reduces elongation through solid solution strengthening. An appropriate amount of Mn can combine with S in steel to form MnS, reducing the hot brittleness of steel. However, excessive Mn solid solution hinders the recovery of the structure and inhibits the growth of recrystallized grains, reducing the γ texture (ND∥ <111> ) strength, which is very unfavorable for the stamping forming of steel plates and will also increase costs, so the present invention controls its content to 0.40-0.80%.

[0024] P is generally controlled as an impurity element in steel, and is only allowed to be added in a few special-purpose steels. For example, adding no more than 0.15% P to sulfur-containing free-cutting steel makes it solid-dissolved in ferrite, causing strengthening and embrittlement to improve its cutting performance. In addition, P is the main corrosion-resistant element in traditional atmospheric corrosion-resistant steel. P in steel can accelerate the uniform dissolution of steel and Fe 2+ The oxidation rate is high, which helps to form a uniform FeOOH rust layer on the steel surface and promotes the formation of amorphous iron oxyhydroxide FeO x (OH) 3-2x Dense protective film effectively improves the atmospheric corrosion resistance of steel. Generally, the corrosion resistance is best when the P content is 0.08% to 0.15%, so P was added as a corrosion-resistant element in some early atmospheric corrosion-resistant steels. However, too much P causes "cold brittleness" of steel, reduces plasticity and impact toughness, and deteriorates the welding performance and cold bending performance of steel, so the amount of addition is clearly limited for steel types with requirements for low-temperature impact toughness or high forming performance. In recent years, some atmospheric corrosion-resistant steels have also reduced the P content and selected other alternative corrosion-resistant elements to ensure corrosion resistance, and even controlled it as an impurity element, requiring the content to be ≤0.015%, but controlling the P content at such a low level will increase the difficulty of steelmaking and increase manufacturing costs. The present invention considers that P improves the strength of steel for aluminum-clad plates and strips by solid solution strengthening, phase transformation strengthening, etc., and uses it to improve the steel-aluminum bonding performance. Therefore, 0.008 to 0.020% of P is added in the present invention.

[0025] S is detrimental to the performance of steel, and can easily cause "hot brittleness" of steel, reduce the low-temperature toughness of steel, and deteriorate the steel-aluminum interface bonding performance. The addition of Mn can form MnS with S, and increasing the Mn / S ratio can improve hot ductility. It is required to control its content at a minimum level. Considering that too low a controlled content increases the difficulty of steelmaking and production costs, the present invention requires that the S content be controlled below 0.008%.

[0026] Al is an important deoxidizing element in steel, but a higher Al content is easy to diffuse to the steel-aluminum bonding interface, deteriorating the interface bonding strength. Therefore, its content must be controlled within a certain range, so the present invention controls 0<Al≤0.005%.

[0027] B is a very active element in steel, and it is easy to form compounds with C and N. At the same time, B is easy to segregate at austenite grain boundaries and dislocations, thereby suppressing the segregation of other interstitial atoms there. Moreover, the segregation of B does not hinder the movement of dislocations, making the strain uniform, improving the plasticity of the material, and being beneficial to improving the rolling performance of aluminum cladding; B significantly improves the hardenability, and a trace amount of B can effectively improve the strength of steel. However, too high a content of B is likely to promote the improvement of hardenability, resulting in excessive strength and reduced stamping performance, so the present invention controls its content to 0.0005-0.002%.

[0028] N can form AlN particles with Al in steel, thereby binding Al and limiting the diffusion of Al in steel. At the same time, N, like C, is easy to aggregate at dislocations to form Coriolis gas clusters, resulting in strain concentration, causing strain unevenness in the aluminum-clad material during processing, affecting the surface quality, and too high N also deteriorates impact toughness, so the present invention controls its content to 0.012-0.030%.

[0029] Oxygen (O) can inhibit the adverse effect of Al in steel on aluminum coating performance, so it is required to add a certain amount of O. However, too much oxygen will produce subcutaneous bubbles, looseness and other defects, and aggravate the thermal brittleness of sulfur, making it easy for the strip surface to have defects such as warping and slag inclusion. During the solidification process of steel, oxygen will precipitate in large quantities in the form of oxides, reducing the plasticity and impact toughness of the steel. Therefore, the O content is controlled to be ≤0.01% and less than 0.01%.

[0030] In addition to the above elements, the present invention also requires the addition of one or more of Ti: 0.01-0.06%, Nb: 0.01-0.03%, Cu: 0.01-0.15%, Cr: 0.03-0.60%, Ca: 0.001-0.004%, so as to further improve the room temperature strength. Among them:

[0031] Cr forms a continuous solid solution with Fe in steel, which has a solid solution strengthening effect, and forms various types of carbides with C, such as M3C, M7C3 and M 23C6, etc., produce a secondary strengthening effect. At the same time, the addition of Cr is beneficial to inhibit the diffusion of Al and improve the steel-aluminum bonding performance. Higher Cr is not good for toughness and increases the difficulty of welding. Cr is a precious alloy element, so the present invention controls its content to 0.03-0.6%.

[0032] Cu has solid solution and precipitation strengthening effects. When the content is high, tempering at an appropriate temperature has a secondary hardening effect, thereby improving the strength. At the same time, the addition of Cu is also beneficial to improving the steel-aluminum bonding performance. Too much Cu causes cracks in the steel billet during heating and hot rolling, deteriorating the surface properties, so the present invention controls the Cu content to 0.01-0.15%.

[0033] Nb is a strong nitrogen carbide-forming element. During the cooling process after rolling, it can combine with carbon and nitrogen in steel to form intermediate phases such as NbC, Nb(CN) and NbN. The fine carbide particles formed can refine the structure, produce fine grain strengthening and precipitation strengthening, and significantly improve the strength of the steel. In addition, Nb can inhibit the expansion of the austenite interface, increase the recrystallization temperature of the steel, and achieve non-recrystallization zone rolling at a higher temperature. Therefore, adding an appropriate amount of Nb to the steel is beneficial to improving the strength, but the effect of improving the strength will no longer increase after exceeding 0.06%. When the Nb content is high, coarse carbonitride particles are formed at the grain boundary, which deteriorates the impact toughness. It can be added selectively, and its content needs to be controlled to be 0.01-0.03%.

[0034] Ti has high chemical activity and is easy to form compounds with C, N, O, S, etc. and precipitate during rolling and cooling to increase strength; at the same time, fine precipitates can pin grain boundaries, thereby refining austenite grains and preventing grain growth in the heat-affected zone of welding, thereby improving the welding performance of steel. The composite addition of Ti and B can significantly reduce temper brittleness. When the Ti content is too high, titanium nitride particles are easy to grow and agglomerate at high temperatures, which damages the plasticity and toughness of the steel. Therefore, its content needs to be controlled at 0.01-0.06%.

[0035] Ca added to steel can change the shape of sulfides, inhibit the hot brittleness of S, and improve toughness. If the Ca content is too low, the effect is not obvious. If the Ca content exceeds 0.005%, the size of Ca(O,S) formed is too large, the brittleness is also increased, and it can become the starting point of fracture cracks. At the same time, the purity of steel is reduced and the toughness of the welding heat affected zone is deteriorated. Therefore, the present invention limits its content to 0.001-0.004%.

[0036] The steel strip for aluminum-clad plates and strips involved in the present invention is mainly aimed at structural parts with requirements for atmospheric corrosion resistance, such as containers, corrosion-resistant pipelines, etc., so there are clear requirements for strength. On the one hand, it is required to control the yield strength of the steel strip to be ≥300MPa; at the same time, the steel strip is required to have good plasticity to meet the requirements of aluminum-clad rolling, and also have good steel-aluminum bonding properties, so as to ensure that the obtained aluminum-clad material does not have steel-aluminum stratification problems during use.

[0037] In order to meet the above performance requirements, the present invention strictly designs the composition according to the influence of different alloy elements on the above performance, and achieves the performance requirements through the comprehensive effect of multiple elements. The addition of C has the effects of solid solution strengthening and phase transformation strengthening. The existing patents for aluminum-clad steel (such as Chinese patent CN114250411A) generally control C≤0.005% to ensure plasticity, which greatly increases the difficulty of steelmaking. In order to ensure the high strength of the aluminum-clad material and require the yield strength of the steel strip to be above 300MPa, the present invention adopts 0.04-0.09% C. On the one hand, it plays a role of solid solution strengthening. At the same time, in the steel production process, by controlling rolling and controlling post-rolling cooling, a ferrite + a small amount of bainite structure is formed in the steel, which plays a role of phase transformation strengthening and improves strength.

[0038] Since the aluminum-clad strip undergoes annealing heat treatment during the production process, conventional fine grain strengthening means have little effect after heat treatment, while solid solution strengthening is not limited by heat treatment. Therefore, the higher the strength of the substrate steel, the higher the strength of the finished aluminum-clad material. For this reason, the present invention adds 0.4-0.8% Mn to ensure the strength of the substrate steel through solid solution strengthening of Mn.

[0039] In the present invention, the P content is controlled at 0.008-0.020%. P is usually controlled as an impurity element in steel, so it is hoped that its content is as low as possible, and is generally required to be controlled below 0.015% or even lower. However, the lower the P content, the higher the steelmaking cost and the greater the difficulty. Since P is an element of the same family as N, appropriate P is beneficial to the steel-aluminum bonding performance, but the research of the present invention has found that its improvement effect on the steel-aluminum bonding performance is not linear. When the P content exceeds 0.020%, the steel-aluminum bonding performance begins to deteriorate. Therefore, considering the difficulty, cost and performance requirements of steelmaking, the upper limit of P control is relaxed to 0.020%, which ensures the steel-aluminum bonding performance on the one hand, while improving the strength and reducing the steelmaking cost.

[0040] In addition to solid solution strengthening, Cr in the steel of the present invention also has a secondary strengthening effect. Cu also has a solid solution strengthening effect in the steel and can precipitate strengthening to improve strength during heat treatment. Nb, V and Ti precipitate fine carbonitrides during rolling and cooling to strengthen the matrix.

[0041] According to the strengthening effect of the above elements on steel, it is required to control the contents of C, P, N and Mn in the steel to satisfy the relationship 1: 150(C-0.01)+60P+300N+5Mn≥13.0. If the value of the relationship is lower than 13.0, the problem of low strength is likely to occur.

[0042] The key to the steel-aluminum bonding performance is to control the formation of brittle iron-aluminum compounds at the steel-aluminum interface in the aluminum-clad material. The formation of iron-aluminum compounds is closely related to the diffusion of Al in steel. Controlling the diffusion of Al can inhibit the formation of iron-aluminum compounds within a certain temperature range. The research of the present invention shows that the steel-aluminum bonding performance is further improved through the synergistic effect of C, Cu, O, N and other elements, while O (oxygen) and N can inhibit the diffusion of Al and reduce the formation of brittle iron-aluminum compounds, thereby improving the steel-aluminum bonding performance. However, too high O will cause defects such as subcutaneous bubbles and looseness in the ingot, and aggravate the hot brittleness of sulfur, making it easy for defects such as warping and slag inclusion to appear on the steel surface. Therefore, the O content is limited to ≤0.01% in the present invention, and 0.012-0.03% N is used to ensure the steel-aluminum bonding performance. Si and Al, as deoxidizing elements, hinder the improvement of O on the steel-aluminum bonding performance, so their content should be limited.

[0043] Therefore, the present invention obtains good steel-aluminum bonding performance through the synergistic effect of C, Mn, Si, Al, O, N and other elements. According to the strength of the effect of C, N, O and Al, Si on the steel-aluminum bonding performance, their contents are required to satisfy the relationship 2: 0.5C+3.83N+O-0.89Al-1.15Si≥0.08 to ensure that the steel has excellent steel-aluminum bonding performance. The higher the value of formula 2, the better the aluminum coating performance. The research of this application shows that if the value of the relationship is lower than 0.08, steel-aluminum stratification is likely to occur during processing and use.

[0044] In general, the present invention adopts the component system required above, comprehensively considers the steel-aluminum bonding performance and high strength requirements, and through the joint action of various elements, it is possible to obtain steel for aluminum-clad plates and strips that meets the requirements.

[0045] The production method of the high-strength aluminum-clad plate strip for corrosion-resistant structure of the present invention comprises the following steps:

[0046] 1) Cleaning and polishing of the laminated surface of aluminum strip and steel strip;

[0047] 2) Rolling

[0048] Aluminum strip and steel strip are laminated and rolled at room temperature to form aluminum-clad strip, and the deformation of a single rolling pass is 50-85%;

[0049] 3) Annealing

[0050] Coil taking-up and bell furnace annealing; wherein, the annealing temperature is 480-530°C, the annealing holding time is t=120+3H, t is in min, H is the thickness of the aluminum-clad steel coil in cm, after annealing, water-cooling to below 200°C, and finally cooling to below 80°C with the furnace before being taken out of the furnace;

[0051] or,

[0052] Continuous annealing and coiling; wherein the annealing temperature is 480-530°C, the continuous annealing time t0=(h+1)×1.5±1min, h is the thickness of the aluminum-clad sheet and strip, in mm, h≥1mm; h<1mm, annealing time≥2min;

[0053] 4) Finishing.

[0054] Preferably, in step 1), the surface cleaning includes pickling, degreasing and drying.

[0055] Preferably, in step 1), the surface cleaning comprises sand blasting or shot blasting.

[0056] Preferably, in step 1), the grinding is performed using a grinding belt or a grinding wheel, and the grinding direction is parallel to the rolling direction.

[0057] Preferably, in step 2), the rolling is one-pass rolling or two-pass rolling.

[0058] In the production process of the aluminum-clad strip of the present invention:

[0059] The surface cleaning of aluminum strips and steel strips includes necessary pickling, degreasing and drying, or direct sandblasting and shot blasting to remove oil, rust and oxide scale on the laminated surface of aluminum strips and steel strips.

[0060] The purpose of grinding is to increase the roughness of the surface to be laminated and expose fresh base metal to improve the mechanical bonding strength between steel and aluminum during the aluminum coating rolling process. Grinding is preferably performed using a sanding belt or a grinding wheel, which can obtain a rough surface, thereby improving the mechanical bite of aluminum and steel during the aluminum coating rolling process and obtaining better steel-aluminum bonding strength; and after grinding, a microscopic work-hardened layer is formed on the surface to be laminated, which is broken during the aluminum coating rolling process, exposing a fresh metal base, achieving point contact bonding between steel and aluminum, and improving the steel-aluminum bonding strength.

[0061] When steel and aluminum are rolled at room temperature, the deformation of a single rolling pass is controlled within the range of 50-85%. According to the needs, steel strips and aluminum strips of different specifications are rolled into aluminum-clad strips of required thickness and structure through 1-2 passes. When the deformation is low, the number of rolling passes increases, and repeated loading and threading are required, which prolongs the production time, reduces production efficiency and increases costs. When the deformation is too low, the insufficient interface bonding strength will lead to direct delamination of steel and aluminum. Although the rolling efficiency is high when the deformation of a single pass is too large, the rolling load is large and the equipment requirements are high. The specific choice of 1 pass or 2 passes to complete the rolling can be determined according to the equipment capacity and the specifications of the finished product.

[0062] After aluminum cladding rolling, the strip needs to be annealed. The purpose of annealing is, on the one hand, to eliminate the work hardening caused by the room temperature rolling process, restore the plasticity of the aluminum clad material, and facilitate the subsequent product forming process; on the other hand, the steel-aluminum interface atoms diffuse with each other during the annealing process, transitioning from mechanical bonding during rolling to metallurgical bonding, further improving the interface bonding strength.

[0063] Since the melting point of aluminum is about 640°C (fluctuates according to the content of other alloys in aluminum), the corresponding recrystallization temperature is about 250°C. Generally, the annealing temperature is controlled to be 100-200°C above the recrystallization temperature. A lower annealing temperature will greatly increase the annealing time, reduce production efficiency and increase production costs. Excessively high annealing temperature will increase energy consumption and increase production costs. At the same time, higher temperatures provide power for the formation of brittle phases at the steel-aluminum interface, reducing the steel-aluminum interface bonding strength. Therefore, the present invention controls the annealing temperature at 480-530°C, which is specifically determined according to the size specifications of the aluminum-clad plate and the performance of the finished product.

[0064] There are usually two annealing methods, including conventional bell-type furnace annealing and continuous annealing. The annealing holding time t of the aluminum-clad sheet is determined based on the thickness h (mm) of the aluminum-clad sheet, the annealing furnace temperature T (℃) and the annealing method.

[0065] When continuous annealing is adopted, the annealing time t0 = (h + 1) × 1.5 ± 1 min, where h ≥ 1 mm. h < 1 mm, and the annealing time is not less than 2 min.

[0066] When annealing in a bell furnace, the annealing time includes three stages: heating section, insulation section and cooling section. The length of the annealing time is closely related to the thickness of the aluminum-clad sheet and strip. For the aluminum-clad steel coil, it corresponds to the difference between the inner and outer radii of the aluminum-clad steel coil. It is generally a linear relationship, and the specific ratio deviates according to the actual situation. According to the thickness H of the aluminum-clad steel coil (the difference between the inner and outer radii of the aluminum-clad steel coil), the annealing time t (min) of the insulation section is controlled, and the requirement is to meet: t = 120 + 3H, where H is in cm. According to the inner diameter of the bell furnace, the outer diameter of the aluminum-clad coil is generally below 1800mm, and the inner diameter is about 560mm. According to this calculation, the insulation time of the aluminum-clad steel coil in the bell furnace does not exceed 306min, about 5h. In the prior art, when the aluminum-clad coil is annealed in a bell furnace, the insulation time is set according to the experience of the operator, and the insulation time is mostly 15 to 18h. In addition, heating requires 6 to 8h and cooling requires about 6h.

[0067] The present invention clarifies the linear relationship between the annealing holding time and the steel coil specification, and has stronger operability. Compared with the existing process, the annealing process of the present invention greatly shortens the heat treatment time, reduces energy consumption, improves production efficiency, and reduces production costs.

[0068] After annealing, the aluminum-clad coil needs to be finished. On the one hand, the plate shape is improved while trimming, and on the other hand, the surface quality is further improved by slight pressure reduction.

[0069] Since aluminum has the characteristics of corrosion resistance and beauty, the aluminum-clad strip of the present invention can be used without painting when manufacturing corrosion-resistant components such as containers, corrosion-resistant pipes, and outdoor towers. Containers made of conventional weathering steel need to be sandblasted on the surface and sprayed with primer, intermediate paint, and topcoat. It is estimated that the cost of painting the container surface exceeds 1,000 yuan / ton. Therefore, the high-strength aluminum-clad strip of the present invention is used to manufacture high-strength corrosion-resistant components, which reduces surface painting compared to traditional weathering steel, significantly reduces production costs, and improves production efficiency.

[0070] The present invention has the following advantages:

[0071] 1. The present invention improves the strength of steel according to solid solution strengthening and phase transformation strengthening, adopts a simple C-Mn design in composition design, and controls the contents of C, P, N and Mn to satisfy the relationship: 150(C-0.01)

[0072] +60P+300N+5Mn≥13.0, to obtain higher strength. Its yield strength is ≥300MPa, and its tensile strength is ≥360MPa, so that the obtained aluminum-clad strip has a yield strength of ≥330MPa and a tensile strength of ≥420MPa. It is mainly used in the production of aluminum-clad strips for containers and other structures with corrosion resistance requirements. Compared with existing weathering steel, it has better corrosion resistance and longer service life; at the same time, it has the good appearance quality of aluminum, can be used without painting, reducing the painting cost and lowering the overall cost.

[0073] 2. In order to obtain higher steel-aluminum bonding performance, the present invention requires that the contents of C, Mn, Si, Al, O, and N satisfy the relationship:

[0074] 0.5C+3.83N+O-0.89Al-1.15Si≥0.08, which inhibits the formation of brittle iron-aluminum compounds at the steel-aluminum interface, thereby ensuring that the steel plate has good steel-aluminum bonding properties, thereby ensuring that the obtained aluminum-clad plate strip does not have steel-aluminum delamination problems during use.

[0075] 3. The present invention adopts a low-oxygen and high-nitrogen composition design, limits the O content to ≤0.01%, and uses 0.012-0.03% N to compensate for the steel-aluminum bonding performance, thereby solving the subcutaneous bubbles, looseness and other defects of the high-oxygen content ingot, reducing the occurrence of defects such as warping and slag inclusions on the surface of the steel strip, and further improving the steel-aluminum bonding performance and surface quality of the aluminum-clad plate.

[0076] 4. The present invention controls the P content to 0.008-0.020%, utilizes the solid solution strengthening effect of P and its influence on the steel-aluminum bonding performance, and further improves the steel-aluminum bonding performance of steel. The aluminum-clad plate and strip still have high steel-aluminum bonding performance after high-temperature nitriding treatment, while reducing the difficulty and cost of steelmaking, and achieving higher production efficiency.

[0077] 5. The present invention can adopt either hood annealing or continuous annealing in the annealing stage, and establishes a linear relationship between the annealing holding time and the steel coil specification. The annealing time is significantly shortened compared with the traditional hood annealing process, which reduces energy consumption, improves production efficiency, reduces production costs, and is more operable. BRIEF DESCRIPTION OF THE DRAWINGS

[0078] Figure 1 It is a schematic structural diagram of the aluminum-clad strip of the present invention.

[0079] Figure 2 It is a schematic structural diagram of the aluminum-clad strip of the present invention.

[0080] Figure 3 It is a schematic structural diagram of the aluminum-clad strip of the present invention. DETAILED DESCRIPTION

[0081] The present invention will be further described below in conjunction with the embodiments and drawings.

[0082] See also Figure 1 , Figure 2 and Figure 3 , which is a schematic structural diagram of an embodiment of the aluminum-clad plate strip of the present invention, wherein 1 is a steel strip and 2 is an aluminum strip.

[0083] According to the chemical composition requirements of the steel strip of the aluminum-clad plate and strip of the present invention, steel strips 1 and aluminum strips 2 of different specifications are selected, and the surfaces are cleaned and polished, and then aluminum-clad rolling and annealing are performed to obtain aluminum-clad plate and strip. The thickness of the prepared aluminum-clad plate and strip is 0.5-2.0 mm.

[0084] The chemical composition of the steel strip according to the embodiment of the present invention is shown in Table 1, the specific production process parameters are shown in Table 2, and the finished product properties are shown in Table 3.

[0085] The aluminum-clad plate and strip prepared by the composition and process of the present invention has a yield strength ≥350MPa, a tensile strength ≥420MPa, an elongation A50 ≥18%, good plasticity, and excellent steel-aluminum interface bonding performance (no iron-aluminum compound is formed).

[0086] Although the chemical composition of the steel strip used in the aluminum-clad strip of Comparative Examples 1-4 also adopts a low Si-Al design and adds a certain amount of O and N, the overall composition is different from that of the present invention. The final performance obtained is also greatly different from that of the present invention, as shown in Table 3.

[0087] The values ​​of Formula 1 and Formula 2 in Comparative Examples 1-4 are lower than those in the embodiments of the present invention. The aluminum-clad rolling and corresponding heat treatment are performed according to the same process.

[0088] It can be seen from the results in Table 3 that the strengths of Comparative Examples 1-4 are significantly lower than those of the present invention and do not meet the requirements of the present invention. Considering that there is a lot of welding involved in the processing of high-strength corrosion-resistant structural parts using the aluminum-clad sheet of the present invention, higher requirements are placed on the steel-aluminum bonding performance. Therefore, the steel-aluminum bonding performance is tested under annealing heat treatment conditions higher than those of conventional aluminum-clad materials.

[0089] The obtained aluminum-clad strip was heat treated at a temperature of 580°C for 5 hours, and the aluminum-clad performance of the aluminum-clad strip was tested and compared with the comparative example. From the results in Table 3, it can be seen that a small amount of iron-aluminum compounds appeared at the steel-aluminum interface of the aluminum-clad strip of the comparative example under the heat treatment conditions of 580°C and 5 hours, while the aluminum-clad strip of the present invention still kept the interface clean and no iron-aluminum compounds were formed, indicating that the aluminum-clad strip obtained by the present invention has better steel-aluminum bonding performance.

[0090] The process of the present invention can produce wide high-strength aluminum-clad strips of different specifications as needed, which are used for the production of container plates and other high-strength corrosion-resistant components, have good appearance, achieve the effect of free painting, reduce the painting process and cost, and have lower overall cost. In addition, the heat treatment temperature can be appropriately adjusted as needed to obtain higher strength or better plasticity, which can be used for the production of other structural parts with corrosion resistance and aesthetic requirements.

[0091]

[0092]

[0093]

Claims

1. A high-strength aluminum-clad plate strip for corrosion-resistant structure, which is a steel strip and an aluminum strip laminated, the chemical composition weight percentage of the steel strip is: C: 0.04-0.09%, 0 < Si ≤ 0.005%, Mn: 0.4-0.8%, P: 0.008-0.020%, S ≤ 0.008%, 0 < Al ≤ 0.005%, N: 0.012-0.030%, 0 < O ≤ 0.01%, B: 0.0005 ~0.002%, and one or more of Ti: 0.01~0.06%, Nb: 0.01~0.03%, Cu: 0.01~0.15%, Cr: 0.03~0.60%, Ca: 0.001~0.004% are optionally added, and the balance contains Fe and other unavoidable impurities; and it is necessary to simultaneously meet the following requirements: 0.5C+3.83N+O-0.89Al-1.15Si≥0.08; 150(C-0.01)+60P+300N+5Mn≥13.

0.

2. The high-strength aluminum-clad plate strip for corrosion-resistant structure according to claim 1, characterized in that: The balance is Fe and other inevitable impurities.

3. The high-strength aluminum-clad strip for corrosion-resistant structure according to claim 1 or 2, characterized in that: The yield strength of the steel strip is ≥300MPa, the tensile strength is ≥360MPa, and the elongation is ≥30%.

4. The high-strength aluminum-clad plate strip for corrosion-resistant structure according to claim 1, 2 or 3, characterized in that: The yield strength of the aluminum-clad strip is ≥350MPa, the tensile strength is ≥420MPa, and the elongation A50 is ≥18%.

5. The high-strength aluminum-clad sheet strip for corrosion-resistant structure according to any one of claims 1 to 4, characterized in that: The aluminum-clad plate strip is a steel-aluminum, aluminum-steel-aluminum or steel-aluminum-steel structure.

6. The method for producing a high-strength aluminum-clad sheet and strip for corrosion-resistant structures as claimed in any one of claims 1 to 5, characterized in that: The steps include: 1) Cleaning and polishing of the laminated surface of aluminum strip and steel strip; 2) Rolling Aluminum strip and steel strip are laminated and rolled at room temperature to form aluminum-clad strip, and the deformation of a single rolling pass is 50-85%; 3) Annealing Coil taking-up and bell furnace annealing; wherein, the annealing temperature is 480-530°C, the annealing holding time is t=120+3H, t is in min, H is the thickness of the aluminum-clad steel coil, in cm; after annealing, water cool to below 200°C, and finally cool to below 80°C with the furnace before being taken out of the furnace; or, Continuous annealing and coiling; wherein the annealing temperature is 480-530°C, the continuous annealing time t0=(h+1)×1.5±1min, h is the thickness of the aluminum-clad strip, in mm, h≥1mm; h<1mm, annealing time ≥2min; 4) Finishing.

7. The production method according to claim 6, characterized in that: In step 1), the surface cleaning includes pickling, degreasing and drying.

8. The production method according to claim 6, characterized in that: In step 1), the surface cleaning includes sand blasting and shot blasting.

9. The production method according to claim 6, characterized in that: In step 1), the grinding is performed using a grinding belt or a grinding wheel, and the grinding direction is parallel to the rolling direction.

10. The production method according to claim 6, characterized in that: In step 2), the rolling is one-pass rolling or two-pass rolling.

Citation Information

Patent Citations

  • BE726397A

  • High-strength steel for aluminum-coated base plate and production method thereof

    CN107881425A

  • High-strength aluminum-coated plate strip and production method thereof

    CN107881426A

  • Steel sheet for hot press forming having excellent heat treatment and impact property, hot press parts made of it and the method for manufacturing thereof

    WO2007064172A1