OLED panel laminating process based on ultra-thin glass

By using a silicon-based substrate and a transparent protective film made of hybrid resin and a chitosan-silver nanocomposite film layer in the ultra-thin glass OLED panel bonding process, combined with an ultra-thin bendable glass bonding fixture, the problem is solved It solves the problems of clamping size adjustment and bacterial contamination, and achieves efficient, convenient glass bonding and antibacterial effects.

CN118721891APending Publication Date: 2024-10-01HUZHOU SHENGXI ELECTRONICS & TECH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410772311.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing ultra-thin bendable glass laminating jig cannot adjust the clamping size, and the operation to adapt to glass of different shapes and sizes is complicated, which reduces work efficiency and production effects. At the same time, the protective film is susceptible to bacterial contamination and loss of viscosity.

Method used

It uses a transparent protective film made of silicon-based substrate and hybrid resin, adds an antibacterial coating of chitosan-silver nanocomposite film, and uses ultra-thin bendable glass lamination fixtures, including electric slide rails, two-way screws and Motor driven to realize clamping and bending functions.

Benefits of technology

The sturdiness, flexibility and antibacterial properties of the protective film are improved, making it easier to clamp and fit different types of glass, improving work efficiency and ease of operation, and reducing the risk of bacterial contamination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118721891A_ABST
    Figure CN118721891A_ABST
Patent Text Reader

Abstract

The invention relates to an OLED (Organic Light Emitting Diode) panel laminating process based on ultra-thin glass, which comprises four steps of preparing a protective film base material layer, preparing a protective film antibacterial protective coating, attaching a release film and mechanically laminating the film, by adding a transparent protective film made of hybrid resin, a nano flexible film substrate and a protective film antibacterial coating and cooperatively using an ultrathin bendable glass fitting jig, the aging of the film is delayed, the antibacterial effect of the film in the storage and use processes is improved, the bending resistance is also improved to a certain extent compared with the prior art, and the application range of the ultrathin bendable glass fitting jig is widened. And the method has great significance to the film product market.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of glass film lamination, and in particular to an OLED panel lamination process based on ultra-thin glass. Background Art

[0002] With the vigorous development of high-tech electronic information industry, consumer electronic products have become necessities in people's daily life, and many consumer electronic products have been moving towards the trend of being thin, light and short, especially the touch display panel that combines the two technologies of display and input. It has the functions of liquid crystal display and touch input at the same time, and can greatly improve the practical performance of various consumer electronic products. Therefore, the equipment of screen film is very necessary.

[0003] The rapid development of electronic products has led to higher and higher requirements for protective films for electronic equipment accessories, and ultra-thin films are becoming more and more popular. This is not limited to the film itself. Problems arising from the lamination of the film have also become an important factor. People frequently use and touch electronic products, and the problem of bacterial infection on the film has also begun to attract attention. In addition, problems such as the loss of stickiness of the protective film due to time or environmental factors during use are also prominent.

[0004] In addition, for ultra-thin glass, the existing ultra-thin bendable glass bonding jig cannot adjust the clamping size when in use, and thus cannot adapt to clamping glass of different shapes and sizes. Glass of different sizes requires replacement of different jigs for operation, which is very inconvenient, and the working process is very complicated, which reduces work efficiency and production effects, resulting in high limitations in its use. Summary of the invention

[0005] The technical purpose of the present invention is to solve the problems in the background technology and provide an OLED panel bonding process based on ultra-thin glass.

[0006] The above technical objectives of the present invention are achieved through the following technical solutions: An OLED panel laminating process based on ultra-thin glass, the laminating process includes the following steps: Step S1: Preparation of protective film substrate layer: The protective film substrate layer is composed of a silicon substrate and a transparent protective film made of a hybrid resin; Step S2: Preparation of the protective film antibacterial protective coating: The protective film antibacterial protective coating is composed of a chitosan-silver nanocomposite film layer; Step S3: attaching a release film: applying the antibacterial protective coating of step S2 to the protective film substrate layer of step S1, and attaching a release film after curing; Step S4: Machine film lamination: The protective film obtained from steps S1-S3 is laminated on the glass device, and an ultra-thin bendable glass lamination jig is used.

[0007] Preferably, the hybrid resin made into a transparent protective film in step S1 is synthesized from 3-glycidoxypropyltrimethoxysilane (KH560) and 4,4'-methylenebiscyclohexylamine (PACM) through a simple ring-opening reaction, wherein the preparation process is to prepare 50-80 parts by mass of 3-glycidoxypropyltrimethoxysilane and 20-50 parts by mass of 4,4'-methylenebiscyclohexylamine, mix them in a container, stir vigorously at 50-100°C, and perform a ring-opening reaction for 3-8 hours to obtain a transparent viscous liquid resin.

[0008] The advantage of the present invention is that unlike the disadvantages of low surface hardness, easy scratching and poor surface wear resistance of most organic polymer materials, the present invention uses ultraviolet (UV) light of photocurable protective material to initiate crosslinking reaction, produces a cured film layer on the surface, and the active siloxane functional groups retained in the resin participate in the sol-gel curing reaction at room temperature to generate a hybrid film. A silane-terminated, environmentally cured hybrid resin (ACHR) is synthesized through a simple ring-opening reaction of the epoxy group on KH560, and the synthesized ACHR is applied to the PET surface and easily wet-cured at room temperature to prepare a protective hybrid film. The hybrid film prepared in this process performs well in transparency, surface hardness, wear resistance and flexibility, and not only has good scratch resistance, but also exhibits excellent bending resistance.

[0009] Preferably, there is a layer of nano flexible film between the protective film substrate layer and the protective film antibacterial protective coating layer, and the thickness is between 40-80 μm.

[0010] The invention has the advantages that the nano flexible film is low in price, easy to obtain, process and manufacture, and when used as a flexible substrate, it has high transparency, high mechanical strength, and the comprehensive performance of the product is also high.

[0011] Preferably, the chitosan-silver nanocomposite film preparation process in step S2 is as follows: after chitosan powder is added to glacial acetic acid solution and stirred evenly, 100 mL of the solution is added with 1-5 mL of silver nitrate solution and 1-5 mL of sodium hydroxide solution respectively, and stirred at 50-90°C to form a viscous chitosan-silver nanoparticle film solution, the principle of which is to use chitosan to reduce silver ions to silver nanoparticles to form chitosan silver nanoparticles (ChAgNPs); the prepared sample solution is transferred to a light-proof bottle for storage, and the obtained film colloid solution is coated on the substrate layer by a drop casting method and then solidified to form an antibacterial coating protective film.

[0012] Preferably, the mass concentration of the chitosan-glacial acetic acid solution is 1-10 g / L, the molar concentrations of the silver nitrate solution and the sodium hydroxide solution are 0.05-0.2 M, respectively; and the curing is performed by heating at 30-60° C. after solidification at room temperature.

[0013] The invention has the advantage that the chitosan-silver nanocomposite material is applied as an antibacterial coating on a mobile phone glass protective film and the coating is performed by a drop casting method, which is a simple and low-cost thin film coating deposition method. Different from spraying and dipping techniques, the drop casting method is a simple and more controllable coating technology, and is most suitable for thin solid films of small areas. In addition, AgNPs are the main antibacterial active particles, and their size is larger than that of silver ions, so that they can react with more molecules, thereby showing greater antibacterial activity. At present, the use of alcohol disinfection spray can be said to be the most popular method for disinfecting mobile phone screens, but its antibacterial properties are not embedded in the glass itself. On the contrary, what is reflected in the invention is that the antibacterial activity of the embedded coating is constant and effective, and its antibacterial effect is good.

[0014] Preferably, an ultra-thin bendable glass bonding jig used in step S4 comprises an operating panel, a clamping device and a fixing rod, wherein the fixing rods are symmetrically arranged on the side wall of the operating panel, an electric slide rail is arranged between the two fixing rods, an electric slider is arranged on the electric slide rail, the electric slide rail passes through the electric slider, the electric slider is linearly slidably connected to the electric slide rail, a connecting rod is arranged at the lower end of the electric slider, a fixing box is arranged at the lower end of the connecting rod, the clamping device comprises a bidirectional screw, a moving block and a clamping plate, the bidirectional screw passes through the fixing box, A motor is provided on one side wall of the fixed box, the bidirectional screw is connected to the output end of the motor, the moving blocks are symmetrically arranged on the bidirectional screw, the bidirectional screw passes through the moving block, and the bidirectional screw is provided with a positive thread and a negative thread, one of the moving blocks is threadedly connected to the positive thread, and the other moving block is threadedly connected to the negative thread, the fixed box is fitted and slidably connected to the moving block, a clamping plate is provided at the lower end of the moving block, an electric telescopic rod is provided on the inner side wall of one of the fixed rods, and a pressing plate is provided at one end of the electric telescopic rod.

[0015] Preferably, the upper wall of the operating panel is provided with symmetrical support rods, the upper end of the support rods is provided with a placing table, and the placing table is provided with anti-slip grooves; the inner wall of the clamping plate is provided with a limiting hole, and the limiting hole is provided with anti-slip silicone; the lower end of the operating panel is provided with a placing cabinet, and the placing cabinet is provided with a placing cavity, and the front side wall of the placing cabinet is provided with symmetrical fixed doors, and the fixed doors are adapted to the placing cavity.

[0016] Preferably, the fixed door is provided with a visual glass, and an inward-hook handle is provided at one end of the fixed door.

[0017] Preferably, universal wheels and brake devices are provided at the four corners of the bottom wall of the storage cabinet, and the universal wheels are adapted to the brake devices; and the motor is a servo motor.

[0018] The advantage of adopting the present invention is that the ultra-thin bendable glass bonding jig is provided with an electric slide rail and an electric slider. When the electric slide rail is started, the electric slider can be moved linearly thereon, which is convenient for driving the clamping plate to move, thereby driving the glass to move, and is convenient for accurate alignment and bonding. It is very convenient. A bidirectional screw and a moving block are provided. The motor output drives the bidirectional screw to rotate. The two moving blocks move with the rotation of the bidirectional screw, and can clamp and fix glass of different models and sizes. It is convenient to use, improve work efficiency, simple to operate, and increase the use effect. A limiting hole is provided, and the glass can be placed in the limiting hole. The distance between the two clamping plates is shortened, and the glass can be automatically bent to an appropriate amount to assist its use. A placing table is provided, which is convenient for placing objects and bonding the glass.

[0019] In summary, the present invention has the following beneficial effects: 1. An OLED panel lamination process based on ultra-thin glass, by adding a transparent protective film made of hybrid resin, a hybrid protective film that is stronger, more flexible and more transparent can be prepared; 2. An OLED panel lamination process based on ultra-thin glass, with the addition of a nano-flexible film substrate. The nano-flexible film is inexpensive, easy to obtain, process and manufacture. Using it as a flexible substrate has high transparency, high mechanical strength, and high overall product performance; 3. An OLED panel lamination process based on ultra-thin glass, which adds an antibacterial coating to the protective film, making it less likely to be contaminated by bacteria during the lamination process and the use of the film; 4. An OLED panel bonding process based on ultra-thin glass, in conjunction with the use of an ultra-thin bendable glass bonding fixture, is very convenient and can clamp and fix glass of different models and sizes, making it easy to use, improving work efficiency, being simple to operate, increasing the use effect, and making it convenient to place objects for bonding with the glass. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] FIG1 is a schematic diagram of an ultra-thin bendable glass bonding jig from a first viewing angle according to the present invention; FIG2 is a schematic diagram of the interior of a fixing box of an ultra-thin bendable glass laminating jig according to the present invention; In the figure: 1. operating panel; 2. fixing rod; 3. electric slide rail; 4. electric slide block; 5. connecting rod; 6. fixing box; 7. motor; 8. clamping plate; 9. electric telescopic rod; 10. pressing plate; 11. placing table; 12. supporting rod; 13. placing cabinet; 14. fixing door; 15. universal wheel; 16. bidirectional screw; 17. moving block. DETAILED DESCRIPTION

[0021] The following specific embodiments are merely explanations of the present invention and are not limitations of the present invention. After reading this specification, those skilled in the art may make modifications to the embodiments without any creative contribution as needed. However, such modifications are protected by the patent law as long as they are within the scope of the claims of the present invention. Example 1

[0022] Step S1: Preparation of protective film substrate layer: The protective film substrate layer is composed of a silicon substrate and a transparent protective film made of a hybrid resin. The preparation process of the hybrid resin transparent protective film is to prepare 50 parts by mass of 3-glycidoxypropyltrimethoxysilane and 50 parts by mass of 4,4'-methylenebiscyclohexylamine, mix them in a container, stir vigorously at 60°C for 5 hours for ring-opening reaction, and obtain a transparent viscous liquid resin film layer.

[0023] Step S2: Preparation of the protective film antibacterial protective coating: The protective film antibacterial protective coating is composed of a chitosan-silver nanocomposite film layer; the preparation process of the antibacterial coating chitosan-silver nanocomposite film layer is as follows: chitosan powder is added to a glacial acetic acid solution and stirred evenly to prepare a 1 g / L chitosan solution, 100 mL is taken and 1 mL of a 0.05 mol / L silver nitrate solution and 1 mL of a 0.05 mol / L sodium hydroxide solution are added respectively, and the mixture is stirred at 70°C to form a viscous chitosan-silver nanoparticle film solution, the prepared sample solution is transferred to a light-proof bottle for storage, the obtained film colloid solution is coated on the substrate layer by a drop casting method, and then solidified at room temperature and then heated at 50°C to cure to obtain an antibacterial coating protective film; there is also a nano-flexible film layer between the protective film substrate layer and the protective film antibacterial protective coating, and the thickness is 40 μm.

[0024] Step S3: attaching the release film: coating the antibacterial protective coating of step S2 on the protective film substrate layer of step S1, and attaching the release film after curing at room temperature.

[0025] Step S4: Machine film pasting: The protective film obtained by steps S1-S3 is pasted on the glass device. Example 2

[0026] Step S1: Preparation of protective film substrate layer: The protective film substrate layer is composed of a silicon substrate and a transparent protective film made of a hybrid resin. The preparation process of the hybrid resin transparent protective film is to prepare 80 parts by mass of 3-glycidoxypropyltrimethoxysilane and 20 parts by mass of 4,4'-methylenebiscyclohexylamine, mix them in a container, stir vigorously at 60°C for a ring-opening reaction for 5 hours, and obtain a transparent viscous liquid resin film layer.

[0027] Step S2: Preparation of the protective film antibacterial protective coating: The protective film antibacterial protective coating is composed of a chitosan-silver nanocomposite film layer; the preparation process of the antibacterial coating chitosan-silver nanocomposite film layer is as follows: chitosan powder is added to a glacial acetic acid solution and stirred evenly to prepare a 10 g / L chitosan solution, 100 mL is taken and added with 5 mL of 0.2 mol / L silver nitrate solution and 5 mL of 0.2 mol / L sodium hydroxide solution respectively, and stirred at 70°C to form a viscous chitosan-silver nanoparticle film solution, the prepared sample solution is transferred to a light-proof bottle for storage, the obtained film colloid solution is coated on the substrate layer by a drop casting method, and then solidified at room temperature and heated at 50°C to cure to obtain an antibacterial coating protective film; there is also a nano-flexible film layer between the protective film substrate layer and the protective film antibacterial protective coating, and the thickness is 80 μm.

[0028] Step S3: attaching the release film: coating the antibacterial protective coating of step S2 on the protective film substrate layer of step S1, and attaching the release film after curing at room temperature.

[0029] Step S4: Machine film pasting: The protective film obtained by steps S1-S3 is pasted on the glass device. Example 3

[0030] Step S1: Preparation of protective film substrate layer: The protective film substrate layer is composed of a silicon substrate and a transparent protective film made of a hybrid resin. The preparation process of the hybrid resin transparent protective film is to prepare 69.2 parts by mass of 3-glycidoxypropyltrimethoxysilane and 30.8 parts by mass of 4,4'-methylenebiscyclohexylamine, mix them in a container, stir vigorously at 80°C for 6 hours for ring-opening reaction, and obtain a transparent viscous liquid resin film layer.

[0031] Step S2: Preparation of the protective film antibacterial protective coating: The protective film antibacterial protective coating is composed of a chitosan-silver nanocomposite film layer; the preparation process of the antibacterial coating chitosan-silver nanocomposite film layer is as follows: chitosan powder is added to a glacial acetic acid solution and stirred evenly to prepare an 8 g / L chitosan solution, 100 mL is taken and 5 mL of 0.1 mol / L silver nitrate solution and 2 mL of 0.1 mol / L sodium hydroxide solution are added respectively, and stirred at 70°C to form a viscous chitosan-silver nanoparticle film solution, the prepared sample solution is transferred to a light-proof bottle for storage, the obtained film colloid solution is coated on the substrate layer by a drop casting method, and then solidified at room temperature and then heated at 45°C to cure to obtain an antibacterial coating protective film; there is also a nano-flexible film layer between the protective film substrate layer and the protective film antibacterial protective coating, and the thickness is 60 μm.

[0032] Step S3: attaching the release film: coating the antibacterial protective coating of step S2 on the protective film substrate layer of step S1, and attaching the release film after curing at room temperature.

[0033] Step S4: Machine film lamination: The protective film obtained from steps S1-S3 is laminated on the glass device, and an ultra-thin bendable glass lamination jig is used.

[0034] As shown in Figures 1 and 2, an ultra-thin bendable glass bonding jig comprises an operating panel 1, a clamping device and a fixed rod 2, wherein the fixed rod 2 is symmetrically arranged on the upper side wall of the operating panel 1, an electric slide rail 3 is arranged between the two fixed rods 2, an electric slider 4 is arranged on the electric slide rail 3, the electric slide rail 3 passes through the electric slider 4, the electric slider 4 is linearly slidably connected to the electric slide rail 3, a connecting rod 5 is arranged at the lower end of the electric slider 4, a fixing box 6 is arranged at the lower end of the connecting rod 5, the clamping device comprises a bidirectional screw 16, a moving block 17 and a clamping plate 8, the bidirectional screw 16 passes through the fixing box 6, a motor 7 is arranged on one side wall of the fixing box 6, the bidirectional screw 16 is connected to the output end of the motor 7, and the moving block 17 is symmetrically arranged on the bidirectional screw 16. On the screw 16, the bidirectional screw 16 passes through the moving block 17, and the bidirectional screw 16 is provided with a positive thread and a negative thread, one of the moving blocks 17 is threadedly connected to the positive thread, and the other moving block 17 is threadedly connected to the negative thread, the fixed box 6 is fitted and slidably connected to the moving block 17, and a clamping plate 8 is provided at the lower end of the moving block 17, one of the inner side walls of the fixed rods 2 is provided with an electric telescopic rod 9, and a pressing plate 10 is provided at one end of the electric telescopic rod 9, and a symmetrical support rod 12 is provided on the upper side wall of the operating panel 1, and a placing table 11 is provided on the upper end of the support rod 12, and anti-slip grooves are provided on the placing table 11, and a limiting hole is provided on the inner side wall of the clamping plate 8, and anti-slip silica gel is provided in the limiting hole.

[0035] During use, the glass is placed between the two clamping plates 8, the motor 7 is started, and the output of the motor 7 drives the bidirectional screw 16 to rotate. Since the positive thread and the negative thread are provided, the moving block 17 moves under the rotation of the bidirectional screw 16, and the two moving blocks 17 move in opposite directions. The fixed box 6 performs limit support, driving the clamping plate 8 to move, and the glass can be clamped. Then, the object to be bonded to the glass is placed on the placement table 11, and the electric slide rail 3 is started. The electric slider 4 moves linearly on the electric slide rail 3, driving the glass to move. Accurate alignment can be performed, and then the glass and the object are fitted together, and the electric telescopic rod 9 is started. The electric telescopic rod 9 is extended to drive the pressing plate 10 to move, and the pressing plate 10 is moved in contact with the glass. The pressing plate 10 has a built-in heating device, which can be fitted and fixed. When the glass needs to be bent, the two ends of the glass can be inserted into the limit holes, and the motor 7 is started. According to the above operation, the distance between the clamping plates 8 is reduced, which can assist the glass in bending. The connecting rod 5 is a liftable rod that can adjust the height distance between the glass and the object. It will not be elaborated in this article.

[0036] In actual use, it is necessary to conveniently place and store processed objects. In order to meet the above requirements, in this embodiment, a placement cabinet 13 is provided at the lower end of the operation panel 1, and a placement cavity is provided in the placement cabinet 13. The front side wall of the placement cabinet 13 is provided with symmetrical fixed doors 14, and the fixed doors 14 are adapted to the placement cavity.

[0037] In actual use, it is necessary to open or close the fixed door 14 conveniently. In order to meet the above requirement, in this embodiment, an inward-locking handle is provided at one end of the fixed door 14.

[0038] In actual use, it is necessary to conveniently observe the internal situation of the storage cabinet 13. In order to meet the above requirement, in this embodiment, the fixed door 14 is provided with a visual glass.

[0039] In actual use, it is necessary to conveniently move and stop the device to a suitable position. In order to meet the above requirements, in this embodiment, universal wheels 15 and brake devices are provided at the four corners of the bottom wall of the placement cabinet 13, and the universal wheels 15 are adapted to the brake devices. Example 4

[0040] Step S1: Preparation of protective film substrate layer: The protective film substrate layer is composed of a silicon substrate and a transparent protective film made of a hybrid resin. The preparation process of the hybrid resin transparent protective film is to prepare 60 parts by mass of 3-glycidoxypropyltrimethoxysilane and 40 parts by mass of 4,4'-methylenebiscyclohexylamine, mix them in a container, stir vigorously at 60°C for a ring-opening reaction for 5 hours, and obtain a transparent viscous liquid resin film layer.

[0041] Step S2: Preparation of the protective film antibacterial protective coating: The protective film antibacterial protective coating is composed of a chitosan-silver nanocomposite film layer; the preparation process of the antibacterial coating chitosan-silver nanocomposite film layer is as follows: chitosan powder is added to a glacial acetic acid solution and stirred evenly to prepare a 6 g / L chitosan solution, 100 mL is taken and 3 mL of a 0.15 mol / L silver nitrate solution and 4 mL of a 0.1 mol / L sodium hydroxide solution are added respectively, and the mixture is stirred at 70°C to form a viscous chitosan-silver nanoparticle film solution, the prepared sample solution is transferred to a light-proof bottle for storage, the obtained film colloid solution is coated on the substrate layer by a drop casting method, and then solidified at room temperature and then heated at 50°C to cure to obtain an antibacterial coating protective film; there is also a nano-flexible film layer between the protective film substrate layer and the protective film antibacterial protective coating, and the thickness is 70 μm.

[0042] Step S3: attaching the release film: coating the antibacterial protective coating of step S2 on the protective film substrate layer of step S1, and attaching the release film after curing at room temperature.

[0043] Step S4: machine film pasting: the protective film obtained by steps S1-S3 is pasted on the glass device. Example 5

[0044] Step S1: Preparation of protective film substrate layer: The protective film substrate layer is composed of a silicon substrate and a transparent protective film made of a hybrid resin. The preparation process of the hybrid resin transparent protective film is to prepare 56.8 parts by mass of 3-glycidoxypropyltrimethoxysilane and 43.2 parts by mass of 4,4'-methylenebiscyclohexylamine, mix them in a container, stir vigorously at 60°C for 5 hours for ring-opening reaction, and obtain a transparent viscous liquid resin film layer.

[0045] Step S2: Preparation of the protective film antibacterial protective coating: The protective film antibacterial protective coating is composed of a chitosan-silver nanocomposite film layer; the preparation process of the antibacterial coating chitosan-silver nanocomposite film layer is as follows: chitosan powder is added to a glacial acetic acid solution and stirred evenly to prepare a 4 g / L chitosan solution, 100 mL is taken and added with 4 mL of a 0.1 mol / L silver nitrate solution and 3 mL of a 0.15 mol / L sodium hydroxide solution, respectively, and stirred at 80°C to form a viscous chitosan-silver nanoparticle film solution, the prepared sample solution is transferred to a light-proof bottle for storage, the obtained film colloid solution is coated on the substrate layer by a drop casting method, and then solidified at room temperature and then heated at 50°C to cure to obtain an antibacterial coating protective film; there is also a nano-flexible film layer between the protective film substrate layer and the protective film antibacterial protective coating, with a thickness of 64.3 μm.

[0046] Step S3: attaching the release film: coating the antibacterial protective coating of step S2 on the protective film substrate layer of step S1, and attaching the release film after curing at room temperature.

[0047] Step S4: Machine film pasting: The protective film obtained by steps S1-S3 is pasted on the glass device. Example 6

[0048] Step S1: Preparation of protective film substrate layer: The protective film substrate layer is composed of a silicon substrate and a transparent protective film made of a hybrid resin. The preparation process of the hybrid resin transparent protective film is to prepare 75 parts by mass of 3-glycidoxypropyltrimethoxysilane and 25 parts by mass of 4,4'-methylenebiscyclohexylamine, mix them in a container, stir vigorously at 60°C for 5 hours for ring-opening reaction, and obtain a transparent viscous liquid resin film layer.

[0049] Step S2: Preparation of the protective film antibacterial protective coating: The protective film antibacterial protective coating is composed of a chitosan-silver nanocomposite film layer; the preparation process of the antibacterial coating chitosan-silver nanocomposite film layer is as follows: chitosan powder is added to a glacial acetic acid solution and stirred evenly to prepare a 7g / L chitosan solution, 100mL of which is added with 5mL of a 0.1mol / L silver nitrate solution and 2mL of a 0.1mol / L sodium hydroxide solution, respectively, and stirred at 80°C to form a viscous chitosan-silver nanoparticle film solution, the prepared sample solution is transferred to a light-proof bottle for storage, the obtained film colloid solution is coated on the substrate layer by a drop casting method, and then solidified at room temperature and then heated at 50°C to cure to obtain an antibacterial coating protective film; there is also a nano-flexible film layer between the protective film substrate layer and the protective film antibacterial protective coating, with a thickness of 55μm.

[0050] Step S3: attaching the release film: coating the antibacterial protective coating of step S2 on the protective film substrate layer of step S1, and attaching the release film after curing at room temperature.

[0051] Step S4: Machine film pasting: The protective film obtained by steps S1-S3 is pasted on the glass device. Comparative Example 1

[0052] Step S1: Preparation of the protective film substrate layer: The protective film substrate layer is composed of a silicon substrate.

[0053] Step S2: Preparation of the protective film antibacterial protective coating: The protective film antibacterial protective coating is composed of a chitosan-silver nanocomposite film layer; the preparation process of the antibacterial coating chitosan-silver nanocomposite film layer is as follows: chitosan powder is added to a glacial acetic acid solution and stirred evenly to prepare an 8 g / L chitosan solution, 100 mL is taken and 5 mL of 0.1 mol / L silver nitrate solution and 2 mL of 0.1 mol / L sodium hydroxide solution are added respectively, and stirred at 80°C to form a viscous chitosan-silver nanoparticle film solution, the prepared sample solution is transferred to a light-proof bottle for storage, the obtained film colloid solution is coated on the substrate layer by a drop casting method, and then solidified at room temperature and heated at 50°C to cure to obtain an antibacterial coating protective film; there is also a nano-flexible film layer between the protective film substrate layer and the protective film antibacterial protective coating, and the thickness is 60 μm.

[0054] Step S3: attaching the release film: coating the antibacterial protective coating of step S2 on the protective film substrate layer of step S1, and attaching the release film after curing at room temperature.

[0055] Step S4: Machine film pasting: The protective film obtained by steps S1-S3 is pasted on the glass device. Comparative Example 2

[0056] Step S1: Preparation of protective film substrate layer: The protective film substrate layer is composed of a silicon substrate and a transparent protective film made of a hybrid resin. The preparation process of the hybrid resin transparent protective film is to prepare 75 parts by mass of 3-glycidoxypropyltrimethoxysilane and 25 parts by mass of 4,4'-methylenebiscyclohexylamine, mix them in a container, stir vigorously at 60°C for 5 hours for ring-opening reaction, and obtain a transparent viscous liquid resin film layer.

[0057] Step S2: attaching the release film: attaching the release film after the protective film substrate layer is cured at room temperature.

[0058] Step S3: Machine film pasting: the protective film obtained by steps S1-S3 is pasted on the glass device. Comparative Example 3

[0059] Common ordinary membranes available in the market.

[0060] With respect to the film preparation processes of the embodiments and comparative examples, the present invention evaluates and compares the adhesion, peelability and antibacterial performance of the antibacterial coating colloid solution of the product film. The detection methods and results of each embodiment and comparative example are as follows: Adhesion test: Use a grid knife to test the adhesion of the cured glue on the PC film. If no peeling is observed under a magnifying glass, it is considered 5B; Peelability test: Apply glue evenly on one end of the PC template, cover it with an optical PET film, use a roller to mechanically roll it from the glued end to the other end, and then irradiate it under a UV lamp of 800mw / cm×cm for 2S before peeling off the PET film. The glue is distributed on the PET film and separated from the PC template. Check whether there is any residual glue on the PC template under a microscope, and check whether the optical pattern on the PET is complete; Antibacterial performance test: refer to WS / T 650-2019 test standard, antibacterial rate x calculation standard ; Among them, X—inhibition rate, %, A0—The amount of bacteria recovered in the positive control group, CFU / mL, A1——The amount of bacteria recovered in the test group, in CFU / mL, The result judgment standard is that if the inhibition rate is ≥50%~90%, it is judged to have an antibacterial effect; if the inhibition rate is ≥90%, it is judged to have a strong antibacterial effect.

[0061] The test results are shown in Table 1.

[0062] It can be seen from the test results that among Examples 1-6, Example 3 has the best product performance, excellent adhesion, a peelability grade of 5B, and an antibacterial rate of 94.8%, which can be judged to have a strong antibacterial effect, followed by Example 6, which shows that when the mass fraction of KH560 in the hybrid resin layer of the protective film substrate layer is 69.2 parts, the mass fraction of PACM is 30.8 parts or thereabouts, the thickness of the nano flexible film is 60 μm, the chitosan solution in the antibacterial protective coating is 8 g / L, the silver nitrate solution and the sodium hydroxide solution are 5 mL, 0.1 mol / L and 2 mL, 0.1 mol / L respectively, its adhesion, peelability and antibacterial performance are the best, and the flexural strength of the film is also high; in addition, Example 6 Example 3 also uses an ultra-thin bendable glass bonding jig in conjunction with the film bonding, so that the film is better bonded and its characteristics can be reflected to the greatest extent; compared with the comparative examples, whether no hybrid resin transparent protective layer is added in comparative example 1, no antibacterial protective coating and nano-flexible film are added in comparative example 2, or none of the three are added in comparative example 3, its adhesion, peelability and antibacterial performance are reduced to a certain extent, and it can be seen from comparative example 3 that when all three are added in the preparation process, the performance of the product is the worst; therefore, by adding a transparent protective film made of hybrid resin, a nano-flexible film substrate, an antibacterial coating of the protective film and using an ultra-thin bendable glass bonding jig, it is of great help to improve the quality of the film product.

Claims

1. An OLED panel bonding process based on ultra-thin glass, characterized in that Including the preparation of protective film and machine film application process, the specific steps are as follows: Step S1: Preparation of protective film substrate layer: The protective film substrate layer is composed of a silicon substrate and a transparent protective film made of a hybrid resin; Step S2: Preparation of the protective film antibacterial protective coating: The protective film antibacterial protective coating is composed of a chitosan-silver nanocomposite film layer; Step S3: attaching a release film: applying the antibacterial protective coating of step S2 to the protective film substrate layer of step S1, and attaching a release film after curing; Step S4: Machine film pasting: The protective film obtained by steps S1-S3 is pasted on the glass device.

2. The ultra-thin glass-based OLED panel bonding process according to claim 1, characterized in that: The hybrid resin in step S1 is made into a transparent protective film by synthesizing 3-glycidoxypropyltrimethoxysilane (KH560) and 4,4'-methylenebiscyclohexylamine (PACM) through a simple ring-opening reaction, wherein the preparation process is to prepare 50-80 parts by mass of 3-glycidoxypropyltrimethoxysilane and 20-50 parts by mass of 4,4'-methylenebiscyclohexylamine, mix them in a container, stir vigorously at 50-100°C, and perform a ring-opening reaction for 3-8 hours to obtain a transparent viscous liquid resin film layer.

3. The ultra-thin glass-based OLED panel bonding process according to claim 2, characterized in that: There is also a layer of nano flexible film between the protective film substrate layer and the protective film antibacterial protective coating layer, and the thickness is between 40-80 μm.

4. The ultra-thin glass-based OLED panel bonding process according to claim 1, characterized in that: The preparation process of the chitosan-silver nanocomposite film layer in step S2 is as follows: chitosan powder is added to glacial acetic acid solution and stirred evenly, 100 mL of the chitosan powder is added with 1-5 mL of silver nitrate solution and 1-5 mL of sodium hydroxide solution respectively, and stirred at 50-90° C. to form a viscous chitosan-silver nanoparticle film solution, the prepared sample solution is transferred to a light-proof bottle for storage, and the obtained film colloid solution is coated on the substrate layer by a drop casting method and then solidified to obtain an antibacterial coating protective film.

5. The ultra-thin glass-based OLED panel bonding process according to claim 4, characterized in that: The concentration of the glacial acetic acid solution is 1g / L. Chitosan and glacial acetic acid solution are prepared into chitosan-glacial acetic acid solution with a mass concentration of 1-10g / L. The molar concentrations of the silver nitrate solution and the sodium hydroxide solution are 0.05-0.2M respectively. The curing is performed by heating at 30-60°C after solidification at room temperature.

6. The ultra-thin glass-based OLED panel bonding process according to claim 1, characterized in that: In the film laminating process of step S4, an ultra-thin bendable glass laminating jig is used, comprising an operating panel (1), a clamping device and a fixing rod (2), characterized in that: the fixing rods (2) are symmetrically arranged on the upper side wall of the operating panel (1), an electric slide rail (3) is arranged between the two fixing rods (2), an electric slider (4) is arranged on the electric slide rail (3), the electric slide rail (3) passes through the electric slider (4), the electric slider (4) is linearly slidably connected to the electric slide rail (3), a connecting rod (5) is arranged at the lower end of the electric slider (4), a fixing box (6) is arranged at the lower end of the connecting rod (5), the clamping device comprises a bidirectional screw (16), a moving block (17) and a clamping plate (8), the bidirectional screw (16) passes through the fixing box (6), A motor (7) is disposed on one side wall of the fixed box (6), the bidirectional screw (16) is connected to the output end of the motor (7), the moving block (17) is symmetrically arranged on the bidirectional screw (16), the bidirectional screw (16) passes through the moving block (17), the bidirectional screw (16) is provided with a positive thread and a negative thread, one of the moving blocks (17) is threadedly connected to the positive thread, and the other moving block (17) is threadedly connected to the negative thread, the fixed box (6) and the moving block (17) are fitted and slidably connected, a clamping plate (8) is disposed at the lower end of the moving block (17), an electric telescopic rod (9) is disposed on the inner side wall of one of the fixed rods (2), and a pressing plate (10) is disposed at one end of the electric telescopic rod (9).

7. The ultra-thin glass-based OLED panel bonding process according to claim 6, characterized in that: The upper side wall of the operating panel (1) is provided with symmetrical support rods (12), the upper end of the support rods (12) is provided with a placement table (11), and the placement table (11) is provided with anti-slip grooves; the inner side wall of the clamping plate (8) is provided with a limit hole, and the limit hole is provided with anti-slip silica gel; the lower end of the operating panel (1) is provided with a placement cabinet (13), and the placement cabinet (13) is provided with a placement cavity, and the front side wall of the placement cabinet (13) is provided with symmetrical fixed doors (14), and the fixed doors (14) are adapted to the placement cavity.

8. The ultra-thin glass-based OLED panel bonding process according to claim 7, characterized in that: The fixed door (14) is provided with a visual glass, and one end of the fixed door (14) is provided with an inwardly buckled handle.

9. The ultra-thin glass-based OLED panel bonding process according to claim 8, characterized in that: Universal wheels (15) and a brake device are provided at the four corners of the bottom wall of the storage cabinet (13), and the universal wheels (15) are adapted to the brake device; and the motor (7) is a servo motor.

10. An OLED panel film based on ultra-thin glass, characterized in that According to an ultra-thin glass-based OLED panel laminating process as described in any one of claims 1-9, the thickness is between 100-200 μm, and can be applied to the field of ultra-thin glass film laminating.

Citation Information

Patent Citations

  • Flexible display panel and preparation method thereof and display device

    CN109994649A

  • Antibacterial protective film for OLED and preparation method of antibacterial protective film

    CN112143400A

  • Protection film of reinforcing aircraft surfaces chemical attack protection

    CN207724993U

  • High-precision glass sheet laminating equipment

    CN214989202U

  • Glass protective film attaching jig for glass attaching back plate

    CN215049715U