Composite multi-layer non-woven material and preparation method and device thereof
Through the preparation method of multi-layer nonwoven materials, combined with high-pressure water spray treatment, the problem of reduced strength and flocculation of the cloth surface after the addition of wood pulp short fibers in the existing technology is solved, and high water absorption, fast water absorption, strength, fluffiness and softness are achieved. characteristics and reduce the flocculation rate and water usage.
Patent Information
- Application Number
- CN202410788992.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-19
AI Technical Summary
When short fibers such as wood pulp are added to existing nonwoven fabrics, the surface strength of the fabric is reduced and the flocculation changes, making it difficult to achieve the characteristics of high water absorption, fast water absorption, fluffiness and softness.
Using a multi-layer nonwoven material preparation method, multi-layer fiber web layers are formed through melt-blown, spun-bonded, mixed-blown and air-laid methods, and are treated with high-pressure water jets to enhance fiber entanglement and improve the breathability and breathability of the cloth surface. Moisture absorbing performance while reducing flocculation rate.
It has achieved high water absorption, quick water absorption, strong, fluffy and soft composite non-woven materials, reduced the flocculation rate, improved the strength and air permeability of the material, and the process uses less water and occupies a small area.
Smart Images

Figure CN118721949A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nonwoven fabrics, and in particular relates to a composite multi-layer nonwoven material and a preparation method and device thereof. Background Art
[0002] Nonwoven fabrics can be found everywhere in daily life and industrial production. From baby care to adult personal care, from face towels to skin care masks, from household wiping to car interior cleaning, from mobile phone cleaning to computer screen dust removal, to machine equipment and precision instrument cleaning, wiping materials made of nonwoven fabrics are everywhere and have become an indispensable part of life.
[0003] Although meltblown technology and spunbond technology have been vigorously developed in recent years, adding short fibers such as wood pulp into the equipment for non-woven fabric production still has disadvantages such as reduced fabric strength and increased linting. Summary of the invention
[0004] The purpose of the present invention is to provide a composite multi-layer nonwoven material and a preparation method and device thereof. The composite multi-layer nonwoven material obtained by the preparation method provided by the present invention has the characteristics of high water absorption, fast water absorption, high strength, fluffy fabric surface, soft hand feel and low linting rate.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a composite multi-layer nonwoven material, comprising the following steps:
[0007] Performing a first meltblowing and / or a first spunbonding on a first raw material to obtain a first web layer, wherein the first web layer comprises a plurality of stacked first meltblown webs and / or a plurality of first spunbonded webs, and the first raw material comprises a first polymer raw material;
[0008] An intermediate fiber web layer is prepared on the surface of the first fiber web layer, and the intermediate fiber web layer includes a plurality of stacked mixed-spray fiber webs and / or a plurality of air-laid fiber webs; the preparation method of the mixed-spray fiber web includes: performing a second melt-blowing on the second raw material, crushing the first water-absorbent fiber and then performing a first air-laying, and mixing the long fiber bundle obtained by the second melt-blowing and the short fiber bundle formed by the first air-laying to obtain the mixed-spray fiber web, and the second raw material includes a second polymer raw material; the preparation method of the air-laid fiber web includes: crushing the second water-absorbent fiber and then performing a second air-laying;
[0009] On the surface of the intermediate fiber web layer, the third raw material is subjected to a third meltblowing and / or a second spunbonding to form a second fiber web layer to obtain a semi-finished fiber web; the second fiber web layer comprises a plurality of stacked second meltblown fiber webs and / or a plurality of second spunbonded fiber webs, and the third raw material comprises a third polymer raw material;
[0010] Hot-rolling the semi-finished fiber web to obtain a hot-rolled fiber web; the first fiber web layer of the semi-finished fiber web forms the lower surface of the hot-rolled fiber web, and the second fiber web layer of the semi-finished fiber web forms the upper surface of the hot-rolled fiber web;
[0011] The hot-rolled fiber web is pre-wetted and then subjected to high-pressure water spraying to obtain a jacquard high-pressure water-sprayed fiber web, wherein the high-pressure water spraying includes sequentially performing flat-net forward spraying, drum reverse spraying, drum forward spraying and flat-net jacquard forward spraying, wherein the flat-net forward spraying is to spray water onto the upper surface of the hot-rolled fiber web, and simultaneously the lower surface is vacuumed; the drum reverse spraying is to spray water onto the lower surface of the hot-rolled fiber web on the rotating circumferential surface of the drum, and the drum forward spraying is to spray water onto the upper surface of the hot-rolled fiber web on the rotating circumferential surface of the drum; the flat-net jacquard forward spraying is to spray water onto the upper surface of the hot-rolled fiber web to form a jacquard pattern, and simultaneously the lower surface is vacuumed;
[0012] The jacquard high-pressure water-jet fiber web is dried and post-finished in sequence to obtain the composite multi-layer nonwoven material.
[0013] Preferably, the first melt-blowing further comprises spraying water or a first chemical additive aqueous solution on the long fiber bundle obtained by the first melt-blowing, the liquid volume of the first spraying is 0 to 180 L / h, and is not 0, and the first chemical additive in the first chemical additive aqueous solution accounts for 0.1 to 10% of the total mass of the composite multi-layer non-woven material;
[0014] The mixed spraying also includes spraying water or a second chemical additive aqueous solution on the mixed filament bundle formed by the short fiber bundle obtained by the first air-laid web and the long fiber bundle obtained by the second melt-blown, the liquid volume of the second spraying is 0 to 180 L / h, and is not 0, and the percentage of the second chemical additive in the second chemical additive aqueous solution to the total mass of the composite multi-layer non-woven material is 0.1 to 10%;
[0015] The second air-laid web further comprises spraying the staple fiber bundle obtained by the second air-laid web with a third water or a third chemical auxiliary agent aqueous solution, wherein the liquid volume of the third spray is 0 to 180 L / h and is not 0, and the third chemical auxiliary agent in the third chemical auxiliary agent aqueous solution accounts for 0.1 to 10% of the total mass of the composite multi-layer nonwoven material;
[0016] The third melt-blowing also includes a fourth spraying of water or a fourth chemical additive aqueous solution to the long fiber filament bundle obtained by the third melt-blowing, the liquid volume of the fourth spraying is 0 to 180 L / h and is not 0, and the fourth chemical additive in the fourth chemical additive aqueous solution accounts for 0.1 to 10% of the total mass of the composite multi-layer non-woven material.
[0017] Preferably, the mass of the first raw material in the first web layer accounts for 0.2-20% of the total mass of the composite multi-layer nonwoven material; the first raw material also includes a first functional masterbatch, and the mass of the first functional masterbatch in the first web layer accounts for 0.1-10% of the mass of the first polymer raw material;
[0018] When the intermediate fiber web layer includes a mixed spray fiber web, the second raw material in the intermediate fiber web layer accounts for 0.2-20% of the total mass of the composite multi-layer nonwoven material; the second raw material also includes a second functional masterbatch, and the mass of the second functional masterbatch in the intermediate fiber web layer accounts for 0.1-10% of the mass of the second polymer raw material;
[0019] The mass of the third raw material in the second web layer accounts for 0.2-20% of the total mass of the composite multi-layer nonwoven material; the second raw material also includes a third functional masterbatch, and the mass of the third functional masterbatch in the second web layer accounts for 0.1-10% of the mass of the third polymer raw material.
[0020] Preferably, the first polymer raw material, the second polymer raw material and the third polymer raw material independently include degradable or compostable thermoplastic fibers and / or thermoplastic polymer filaments; the degradable or compostable thermoplastic fibers include one or more of polylactic acid, polyhydroxyalkanoate, polycaprolactone, polyester amide and copolymers thereof, polyvinyl alcohol, polyvinyl alcohol derivatives, cellulose, cellulose derivatives, proteins, starch, starch derivatives, chitosan, chitosan derivatives, hemicellulose and hemicellulose derivatives; the material of the thermoplastic polymer filaments includes one or more of polyolefins, polyesters, polyhydroxyalkanoates and polyhydroxybutyrates; the thermoplastic polymer filaments include single components or double components, and the double components include one or more of sheath-core type, side-by-side type, trilobal type and orange segment type; the melt index of the thermoplastic polymer filaments ranges from 100 to 1500 g / 10 min;
[0021] The spinning temperatures of the first melt-blowing, the second melt-blowing and the third melt-blowing are independently 200° C. to 290° C.;
[0022] The diameter of the long fibers obtained by the first meltblowing, the first spunbonding, the second meltblowing, the third meltblowing and the second spunbonding is 5 to 20 μm, and the gram weight is 0.1 to 3.0 gsm.
[0023] Preferably, when the intermediate fiber web layer comprises a mixed spray fiber web, the mass of the first water-absorbent fibers in the intermediate fiber web layer accounts for 10 to 47.5% of the total mass of the composite multi-layer nonwoven material;
[0024] When the intermediate fiber web layer comprises an air-laid fiber web, the mass of the second water-absorbent fibers in the intermediate fiber web layer accounts for 10 to 47.5% of the total mass of the composite multi-layer nonwoven material;
[0025] The first absorbent fiber and the second absorbent fiber independently include wood pulp fiber and / or paper pulp fiber; the wood pulp fiber includes one or more of oak, poplar, birch, pine, spruce and fir; the paper pulp fiber includes one or more of straw pulp, reed pulp, sugarcane pulp, bamboo pulp, cotton pulp, hemp pulp and natural fiber rag pulp;
[0026] The length of the staple fibers obtained by the first air-laid web and the second air-laid web is 0.5 to 8 mm;
[0027] The first air-laid web and the second air-laid web are independently distributed and laid by a CD controllable ejector or laid by a forming head uniformly distributed along the width direction, and the forming head is a dust cage type or a flat screen type.
[0028] Preferably, the hot rolling setting temperature is 80-200°C, the speed is 0-1000m / min, and is not 0;
[0029] The pre-wetting water pressure is 0.1 to 5 MPa, preferably 0.5 to 4 MPa, more preferably 0.5 to 3 MPa;
[0030] The water pressure of the flat mesh type forward spray is 0.5 to 10 MPa, preferably 1 to 10 MPa, and more preferably 3 to 8 MPa;
[0031] The water pressure of the rotary drum reverse spray and the rotary drum forward spray is independently 1 to 15 MPa, preferably 3 to 15 MPa, and more preferably 5 to 12 MPa;
[0032] The water pressure of the flat mesh jacquard positive jet is 3 to 20 MPa, preferably 5 to 20 MPa, and more preferably 8 to 18 MPa;
[0033] The drying temperature is 90-130°C.
[0034] Preferably, the post-finishing comprises: one or more of spraying, roller coating and padding;
[0035] The chemical additives used in the post-finishing process include one or more of antibacterial agents, hydrophilic agents, softeners, softeners, strength agents, adhesives, silicones, wetting agents, latex and thermochromic colorant materials; the latex includes acrylic acid and / or ethylene vinyl acetate; the strength agent includes carboxymethyl cellulose and / or starch; the adhesive includes one or more of ethylene vinyl acetate, acrylic acid and other elastic adhesives.
[0036] The present invention provides a composite multi-layer nonwoven material prepared by the preparation method described in the above technical scheme, comprising a first layer structure, an intermediate layer structure and a second layer structure stacked in sequence; the first layer structure is formed by a plurality of first meltblown fiber webs and / or a plurality of first spunbond fiber webs; the intermediate layer structure is formed by a plurality of mixed-spray fiber webs and / or a plurality of air-laid fiber webs, and the second layer structure is formed by a plurality of second meltblown fiber webs and / or a plurality of second spunbond fiber webs.
[0037] The present invention provides a device used in the preparation method described in the above technical solution, comprising a web-forming curtain, a web-forming device arranged above the web-forming curtain, the web-forming device comprising a plurality of first melt-blowing devices and / or a plurality of spunbonding devices, and also comprising a plurality of mixed spray systems and / or a plurality of second grinding devices, the second grinding device comprising a second crusher and a second air-flow web-forming device; the mixed spray system comprising a plurality of second melt-blowing devices, a plurality of first grinding devices and a mixed spray forming box, the first grinding device comprising a first crusher and a first air-flow web-forming device;
[0038] A hot rolling device arranged downstream of the mesh forming curtain, a first mesh transport curtain arranged downstream of the hot rolling device, a pre-wetting device and a first high-pressure water spraying device arranged above the first mesh transport curtain, a first vacuum dehydration device arranged below the first mesh transport curtain, a second high-pressure water spraying device and a third high-pressure water spraying device arranged downstream of the first mesh transport curtain, a second mesh transport curtain arranged downstream of the second and third high-pressure water spraying devices, a jacquard high-pressure water spraying device arranged above the second mesh transport curtain, a second vacuum dehydration device arranged below the second mesh transport curtain, a drying device arranged downstream of the second mesh transport curtain, and a finishing device arranged downstream of the drying device.
[0039] Preferably, a first spray device is provided below the spinneret of the first melt-blowing device, a second spray device is provided below the discharge port of the mixed spray molding box, and a third spray device is provided below the second air-laid device;
[0040] The spinnerets of the first melt-blowing device and the second melt-blowing device include a first spinneret, a second spinneret or a third spinneret;
[0041] The first spinneret is provided with a single row of first spinneret holes, the first spinneret holes are inverted conical holes, the outer cone surface of the first spinneret holes is sleeved with first airflow drafting holes, the first airflow drafting holes are inverted conical holes and are coaxial with the first spinneret holes, the long fibers ejected from the first spinneret holes and the drafting gas ejected from the first airflow drafting holes converge at the apex, and the angle between the drafting gas and the long fibers is 30-70°;
[0042] The second spinneret is provided with a single row or multiple rows of second spinneret holes, the second spinneret holes are cylindrical holes, the outer circumference of the second spinneret holes is sleeved with second airflow drafting holes, the second airflow drafting holes are annular holes and are coaxial with the second spinneret holes;
[0043] The third spinneret is provided with a single row or multiple rows of third airflow drafting holes, the third airflow drafting holes are cylindrical holes, the outer peripheral surface of the third airflow drafting holes is sleeved with third spinneret holes, the third spinneret holes are annular holes and are coaxial with the third airflow drafting holes.
[0044] The present invention provides a method for preparing a composite multi-layer nonwoven material. The preparation method provided by the present invention obtains a multi-layer fiber mesh layer by melt-blowing, spunbonding, mixed spraying consisting of melt-blowing and air-laying, and a single air-laying, etc., which can enrich the types of fiber filaments in the fiber mesh layer, so that multiple fibers in the fiber layer can achieve functional compounding, and then the multi-layer fiber mesh layer is hot-rolled and shaped, and then high-pressure water spraying is performed. Compared with the prior art, the present invention does not affect the original characteristics of the fiber, does not damage the fiber, and also washes off the short fibers scattered on the surface of the fiber mesh, greatly reducing the fluffing rate, and the high-pressure water spraying step flushes the fiber mesh with high-pressure water, so that the fibers are more tightly entangled with each other, thereby enhancing the strength of the cloth; at the same time, due to the high-pressure water spraying, the micropores on the cloth surface are increased, thereby improving the fluffiness and air permeability of the cloth, and improving the high hygroscopicity and fast hygroscopicity of the fabric. Compared with water spunlace, the present invention uses a small number of water spunlace heads in the high-pressure water spraying method, occupies a small area, and uses less water. And because the traditional spunlace is to make the loose fibers entangled together better and play a role in reinforcement, the present invention uses high-pressure water spraying not only to make the fibers entangled together better, without the need for adhesive reinforcement, but also has wash-resistant performance, and also makes the product have excellent air permeability, high moisture absorption, fast moisture absorption performance, and can also make the fabric surface low in linting, low in linting, more fluffy, and softer in feel. In addition, the present invention also customizes different patterns according to customer needs through flat mesh jacquard positive spraying, so that the appearance of the non-woven fabric surface is varied.
[0045] Compared with the prior art, the method for preparing the composite multi-layer nonwoven material provided by the present invention has the following beneficial effects:
[0046] The present invention not only can give the material excellent instantaneous water absorption and rapid water absorption properties through the intermediate fiber web layer, but when the intermediate fiber web layer also includes a mixed spray fiber web, the long fibers obtained by the second melt-blown in the mixed spray fiber web can also play a certain supporting role, making the fabric fluffy and soft and improving the strength of the material. The high-pressure water spraying step greatly reduces the material's lint rate without destroying the original material properties, and further improves the material's strength, softness and fluffiness.
[0047] At the same time, compared with spunlace, the number of spunlace heads commonly used in the spunlace reinforcement process is 7-12, and the commonly used water pressure is 3-60Mpa. The water consumption of the spunlace non-woven production process is very large. Assuming that the output is 1 ton / day, about 50-60 tons of water are required per hour, making water the largest cost for spunlace non-woven fabric companies. The high-pressure water jet process of the present invention only consumes 1-2 tons of water to produce 1 ton of water-electret non-woven fabric. There are 4 spunlace heads and the water pressure is 0.1-15Mpa. Therefore, compared with traditional spunlace, the present invention uses fewer spunlace heads, lower water pressure, smaller footprint, and less water consumption. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 This is a schematic diagram of the structure of the device used in Example 1 of the present invention;
[0049] Figure 2 A schematic diagram of a device used in Example 2 of the present invention;
[0050] Figure 3 A schematic diagram of a device used in Example 3 of the present invention;
[0051] Figure 4 A schematic diagram of a device used in Example 4 of the present invention;
[0052] Figure 5 A schematic diagram of a device used in Example 5 of the present invention;
[0053] Figure 6 It is a cross-sectional view of a spinneret with multiple rows of holes in the present invention;
[0054] Figure 7 It is a front view of a spinneret with multiple rows of holes in the present invention;
[0055] Figure 8 It is a schematic cross-sectional view of a single spinneret hole in the present invention;
[0056] Fig. 9 This is a structural diagram of the mixed spray water absorption layer in the present invention;
[0057] Fig.10 This is a cross-sectional view of the melt-blown spinneret of the "slit air knife" in the present invention;
[0058] In the figure: 1 is a first melt-blowing device; 1-1 is a first melt-blowing raw material supply device; 1-2 is a first screw extruder; 1-3 is a first melt filtering device; 1-4 is a first spinning manifold; 1-5 is a first spinneret;
[0059] 2 is a second melt-blowing device; 2-1 is a second melt-blowing raw material supply device; 2-2 is a second screw extruder; 2-3 is a second melt filtering device; 2-4 is a second spinning manifold; 2-5 is a second spinneret;
[0060] 3 is a third melt-blowing device; 3-1 is a third melt-blowing raw material supply device; 3-2 is a third screw extruder; 3-3 is a third melt filtering device; 3-4 is a third spinning manifold; 3-5 is a third spinneret;
[0061] 4 is a fourth melt-blowing device; 4-1 is a fourth melt-blowing raw material supply device; 4-2 is a fourth screw extruder; 4-3 is a fourth melt filtering device; 4-4 is a fourth spinning manifold; 4-5 is a fourth spinneret;
[0062] 5 is a first grinding device; 5-1 is a first crusher; 5-2 is a first air-laid device;
[0063] 6 is the fifth melt-blowing device; 6-1 is the fifth melt-blowing raw material supply device; 6-2 is the fifth screw extruder; 6-3 is the fifth melt filtering device; 6-4 is the fifth spinning manifold; 6-5 is the fifth spinneret;
[0064] 7 is the sixth melt-blowing device; 7-1 is the fourth melt-blowing raw material supply device; 7-2 is the fourth screw extruder; 7-3 is the fourth melt filtering device; 7-4 is the fourth spinning manifold; 7-5 is the fourth spinneret;
[0065] 8 is a second grinding device; 8-1 is a second crusher; 8-2 is a second air-laid device;
[0066] 9 is a first spray mixing and forming box;
[0067] 10 is a second spray mixing and forming box;
[0068] 11-1 is the first spray device; 11-2 is the second spray device; 11-3 is the third spray device; 11-4 is the fourth spray device; 11-5 is the fifth spray device;
[0069] 12 is a first spunbond device; 12-1 is a first spunbond raw material supply device; 12-2 is a first spunbond screw extruder; 12-3 is a first spunbond spinning box; 12-4 is a first spunbond cooling device; 12-5 is a first spunbond traction device; 12-6 is a first spunbond separator;
[0070] 13 is a second spunbond device; 13-1 is a first spunbond raw material supply device; 13-2 is a first spunbond screw extruder; 13-3 is a first spunbond spinning box; 13-4 is a first spunbond cooling device; 13-5 is a first spunbond traction device; 13-6 is a first spunbond separator;
[0071] 14 is a first mixed spray system;
[0072] 15 is a second mixed spray system;
[0073] 16 is a hot rolling device; 17 is a roller pre-wetting device; 18 is a first high-pressure water spraying device; 19 is a first vacuum dehydration device; 20 is a first mesh conveying curtain; 21 is a second mesh conveying curtain; 22 is a second high-pressure water spraying device; 23 is a third high-pressure water spraying device; 24 is a conveying roller; 25 is a jacquard high-pressure water spraying device; 26 is a jacquard water spunlace machine roller; 27 is a second vacuum dehydration device; 28 is a drying device; 29 is a finishing device; 30 is a spinneret; 31 is a spinneret hole or an airflow drafting hole; 32 is an airflow drafting hole or a spinneret hole; 33 is a mixed spray water absorption layer; 34 is a short water absorption fiber; 35 is a melt-blown fiber; 36 is a "slit air knife" melt-blown type spinneret hole; 37 is a "slit air knife" melt-blown type airflow drafting hole; 38 is a mesh curtain; 39 is a suction wind device;
[0074] 40 is a third spunbond device; 40-1 is a first spunbond raw material supply device; 40-2 is a first spunbond screw extruder; 40-3 is a first spunbond spinning box; 40-4 is a first spunbond cooling device; 40-5 is a first spunbond traction device; 40-6 is a first spunbond separator;
[0075] 41 is the seventh melt-blowing device; 41-1 is the seventh melt-blowing raw material supply device; 41-2 is the seventh screw extruder; 41-3 is the seventh melt filtering device; 41-4 is the seventh spinning manifold; 41-5 is the seventh spinneret;
[0076] 42 is the fourth spunbond device; 42-1 is the first spunbond raw material supply device; 42-2 is the first spunbond screw extruder; 42-3 is the first spunbond spinning box; 42-4 is the first spunbond cooling device; 42-5 is the first spunbond traction device; 42-6 is the first spunbond wire separator. DETAILED DESCRIPTION
[0077] The present invention provides a method for preparing a composite multi-layer nonwoven material, comprising the following steps:
[0078] Performing a first meltblowing and / or a first spunbonding on a first raw material to obtain a first web layer, wherein the first web layer comprises a plurality of stacked first meltblown webs and / or a plurality of first spunbonded webs, and the first raw material comprises a first polymer raw material;
[0079] An intermediate fiber web layer is prepared on the surface of the first fiber web layer, and the intermediate fiber web layer includes a plurality of stacked mixed-spray fiber webs and / or a plurality of air-laid fiber webs; the preparation method of the mixed-spray fiber web includes: performing a second melt-blowing on the second raw material, crushing the first water-absorbent fiber and then performing a first air-laying, and mixing the long fiber bundle obtained by the second melt-blowing and the short fiber bundle formed by the first air-laying to obtain the mixed-spray fiber web, and the second raw material includes a second polymer raw material; the preparation method of the air-laid fiber web includes: crushing the second water-absorbent fiber and then performing a second air-laying;
[0080] On the surface of the intermediate fiber web layer, the third raw material is subjected to a third meltblowing and / or a second spunbonding to form a second fiber web layer to obtain a semi-finished fiber web; the second fiber web layer comprises a plurality of stacked second meltblown fiber webs and / or a plurality of second spunbonded fiber webs, and the third raw material comprises a third polymer raw material;
[0081] Hot-rolling the semi-finished fiber web to obtain a hot-rolled fiber web; the first fiber web layer of the semi-finished fiber web forms the lower surface of the hot-rolled fiber web, and the second fiber web layer of the semi-finished fiber web forms the upper surface of the hot-rolled fiber web;
[0082] The hot-rolled fiber web is pre-wetted and then subjected to high-pressure water spraying to obtain a jacquard high-pressure water-sprayed fiber web, wherein the high-pressure water spraying includes sequentially performing flat-net forward spraying, drum reverse spraying, drum forward spraying and flat-net jacquard forward spraying, wherein the flat-net forward spraying is to spray water onto the upper surface of the hot-rolled fiber web, and simultaneously the lower surface is vacuumed; the drum reverse spraying is to spray water onto the lower surface of the hot-rolled fiber web on the rotating circumferential surface of the drum, and the drum forward spraying is to spray water onto the upper surface of the hot-rolled fiber web on the rotating circumferential surface of the drum; the flat-net jacquard forward spraying is to spray water onto the upper surface of the hot-rolled fiber web to form a jacquard pattern, and simultaneously the lower surface is vacuumed;
[0083] The jacquard high-pressure water-jet fiber web is dried and post-finished in sequence to obtain the composite multi-layer nonwoven material.
[0084] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.
[0085] In the present invention, the total mass of the composite multilayer nonwoven material is the total mass of the polymer raw materials (two or three of the first polymer raw materials, the second polymer raw materials and the third polymer raw materials), the absorbent fibers (one or two of the first absorbent fibers and the second absorbent fibers), preferably also including chemical additives (at least one of the first chemical additive, the second chemical additive, the third chemical additive, the fourth chemical additive and the chemical additives used for post-finishing), preferably including functional masterbatch (any one of the first functional masterbatch, the second functional masterbatch and the third functional masterbatch). The sum of the mass percentages of the raw materials used in the composite multilayer nonwoven material is 100%.
[0086] The present invention performs a first meltblowing and / or a first spunbonding on the first raw material to obtain a first web layer, wherein the first web layer includes a plurality of stacked first meltblown webs and / or a plurality of first spunbonded webs, and the first raw material includes a first polymer raw material. In the present invention, the first web layer is also referred to as a "scrim" layer, which can reduce the shedding of short absorbent fibers in the middle web layer and reduce linting. The first polymer raw material preferably includes degradable or compostable thermoplastic fibers and / or thermoplastic polymer filaments; the degradable or compostable thermoplastic fibers include one or more of polylactic acid, polyhydroxyalkanoate, polycaprolactone, polyesteramide and copolymers thereof, polyvinyl alcohol, polyvinyl alcohol derivatives, cellulose, cellulose derivatives, proteins, starch, starch derivatives, chitosan, chitosan derivatives, hemicellulose and hemicellulose derivatives; the material of the thermoplastic polymer filaments includes one or more of polyolefins, polyesters, polyhydroxyalkanoates and polyhydroxybutyrates; the starch derivatives preferably include One or more of pregelatinized starch, acid-modified starch and oxidized starch; the chitosan derivative preferably includes one or more of chitosan oligosaccharides, chitosan quaternary ammonium salts, carboxymethyl chitosan and hydroxypropyl chitosan; the hemicellulose derivative preferably includes one or more of nonionic hemicellulose, anionic hemicellulose and cationic hemicellulose; the thermoplastic polymer filament preferably includes a single component or a two-component, and the two-component includes one or more of a sheath-core type, a parallel type, a trilobal type and an orange segment type; the melt index range of the thermoplastic polymer filament is preferably 100-1500g / 10min. The melt index range of the polymer material used in the first meltblowing is preferably 300-1000g / 10min, more preferably 400-800g / 10min, and further preferably 500-700g / 10min. The melt index range of the polymer material used in the first spunbond is preferably 10-100g / 10min, more preferably 10-60g / 10min, and further preferably 25-40g / 10min.
[0087] The mass of the first raw material in the first fiber web layer preferably accounts for 0.2-20% of the total mass of the composite multi-layer nonwoven material, more preferably 0.5-18%, and further preferably 5-15%; the first raw material also includes a first functional masterbatch, and the first functional masterbatch preferably includes one or more of a hydrophilic masterbatch, an elastic masterbatch, a degradable masterbatch, an antibacterial masterbatch, a cooling masterbatch, an antistatic masterbatch, and an anti-rust masterbatch. The mass of the first functional masterbatch in the first fiber web layer preferably accounts for 0.1-10% of the mass of the first polymer raw material, more preferably 0.5-5%, and further preferably 2-3%. The spinning temperature of the first meltblown is preferably 200°C to 290°C, more preferably 220-270°C, and further preferably 230-260°C. The hot air volume of the first meltblown is 800-2000Nm 3 / h. The first melt-blowing preferably also includes a first spray of water or a first chemical additive aqueous solution to the long fiber bundle obtained by the first melt-blowing. The first chemical additive aqueous solution preferably includes a first chemical additive and water, and the first chemical additive preferably includes one or more of an antibacterial agent, a hydrophilic agent, a softener, a softener, a strength agent, an adhesive, a silicone, a wetting agent, a latex and a thermochromic colorant material; the latex includes acrylic acid and / or ethylene vinyl acetate; the strength agent includes carboxymethyl cellulose and / or starch; the adhesive includes one or more of ethylene vinyl acetate, acrylic acid and other elastic adhesives. The first spray is a water mist formed by spraying water or chemical additives with a high-pressure small hole. The first spray volume is preferably 0-180L / h, more preferably 100-180L / h, and further preferably 120-150L / h, so that the spray can quickly adhere to the filaments and then dry. The percentage of the first chemical additive in the first chemical additive aqueous solution to the total mass of the composite multilayer nonwoven material is preferably 0.1-10%, more preferably 1-5%, and most preferably 1-3%. The diameter of the long fibers obtained by the first meltblowing is 5-20 μm, and the gram weight is 0.1-3.0 gsm. The diameter of the long fibers obtained by the first spunbond is 5-20 μm, and the gram weight is 0.1-3.0 gsm. The compositions of the plurality of first meltblown webs and / or the plurality of first spunbond webs are the same or different.
[0088] After obtaining the first web layer, the present invention prepares an intermediate web layer on the surface of the first web layer, and the intermediate web layer includes a plurality of stacked mixed-spray webs and / or a plurality of air-laid webs; the preparation method of the mixed-spray web includes: performing a second melt-blowing on the second raw material, crushing the first water-absorbent fiber and then performing a first air-laying, and mixing the long fiber bundle obtained by the second melt-blowing and the short fiber bundle formed by the first air-laying to obtain the mixed-spray web, and the second raw material includes a second polymer raw material; the preparation method of the air-laid web includes: crushing the second water-absorbent fiber and then performing a second air-laying. In the present invention, the first water-absorbent fiber preferably includes wood pulp fiber and / or paper pulp fiber; the wood pulp fiber includes one or more of oak, poplar, birch, pine, spruce and fir; the paper pulp fiber includes one or more of straw pulp, reed pulp, sugarcane pulp, bamboo pulp, cotton pulp, hemp pulp and natural fiber rag pulp. The mass of the first absorbent fiber in the intermediate fiber web layer accounts for a percentage of the total mass of the composite multi-layer nonwoven material of preferably 10 to 47.5%, more preferably 25-45%, and further preferably 30 to 45%. The pulverization is carried out in a grinding device. In the present invention, the first absorbent fiber is transported to the grinding device for pulverization via a transmission device. If it is a loose fiber such as cotton, it can be cut by a cutting device first and then pulverized by a grinding device, and the pulverized fibers are evenly distributed to various parts by air-laying. The first air-laying is preferably distributed and laid by a CD controllable ejector or by a forming head that is evenly distributed along the width direction for paving, and the forming head is a dust cage type or a flat screen type. The length of the short fibers obtained by the first air-laying is 0.5 to 8 mm. The second raw material comprises a second polymer raw material, and the second polymer raw material preferably comprises degradable or compostable thermoplastic fibers and / or thermoplastic polymer filaments; the degradable or compostable thermoplastic fibers comprise one or more of polylactic acid, polyhydroxyalkanoate, polycaprolactone, polyesteramide and copolymers thereof, polyvinyl alcohol, polyvinyl alcohol derivatives, cellulose, cellulose derivatives, proteins, starch, starch derivatives, chitosan, chitosan derivatives, hemicellulose and hemicellulose derivatives; the material of the thermoplastic polymer filaments comprises one or more of polyolefins, polyesters, polyhydroxyalkanoates and polyhydroxybutyrates; the starch derivatives comprise one or more of polyols, polyesters, polyhydroxyalkanoates and polyhydroxybutyrates; the The powder derivative preferably includes one or more of pregelatinized starch, acid-modified starch and oxidized starch; the chitosan derivative preferably includes one or more of chitosan oligosaccharides, chitosan quaternary ammonium salts, carboxymethyl chitosan and hydroxypropyl chitosan; the hemicellulose derivative preferably includes one or more of nonionic hemicellulose, anionic hemicellulose and cationic hemicellulose; the thermoplastic polymer filament preferably includes a single component or a two-component, and the two-component includes one or more of sheath-core type, parallel type, trilobal type and orange segment type; the melt index range of the thermoplastic polymer filament is preferably 100 to 1500 g / 10 min.The melt index range of the polymer material used in the second melt-blowing is preferably 300 to 1000 g / 10 min, more preferably 400 to 800 g / 10 min, and further preferably 500 to 700 g / 10 min.
[0089] In the present invention, the percentage of the second raw material in the intermediate fiber web layer to the total mass of the composite multi-layer nonwoven material is preferably 0.2-20%, more preferably 0.5-18%, and further preferably 5-15%; the second raw material of the second melt-blown preferably also includes a second functional masterbatch, and the second functional masterbatch preferably includes one or more of a hydrophilic masterbatch, an elastic masterbatch, a degradable masterbatch, an antibacterial masterbatch, a cooling masterbatch, an antistatic masterbatch and an anti-rust masterbatch. The mass of the second functional masterbatch in the intermediate fiber web layer accounts for 0.1-10% of the mass of the second polymer raw material, more preferably 0.5-5%, and further preferably 2-3%. The spinning temperature of the second melt-blown is preferably 200°C to 290°C, more preferably 220-270°C, and further preferably 230-260°C. The hot air volume of the second melt-blown is 800-2000Nm 3 / h. The mixed spraying also includes a second spray of water or a second chemical additive aqueous solution to the short fiber bundle obtained by the first air-laid web and the long fiber bundle obtained by the second melt-blown. The second spraying amount is preferably 0-180L / h, more preferably 100-180L / h, and further preferably 120-150L / h. The second spraying uses a high-pressure small hole spray to form a water mist of water or chemical additives, so that the spray can quickly adhere to the short fibers and filaments and then dry. The second chemical additive aqueous solution preferably includes a second chemical additive and water, and the second chemical additive preferably includes one or more of an antibacterial agent, a hydrophilic agent, a softener, a softener, a strength agent, an adhesive, a silicone, a wetting agent, a latex and a thermochromic colorant material; the latex includes acrylic acid and / or ethylene vinyl acetate; the strength agent includes carboxymethyl cellulose and / or starch; the adhesive includes one or more of ethylene vinyl acetate, acrylic acid and other elastic adhesives. The percentage of the second chemical additive in the second chemical additive aqueous solution to the total mass of the composite multilayer nonwoven material is preferably 0.1-10%, more preferably 1-5%, and most preferably 1-3%. The diameter of the long fiber obtained by the second melt-blowing is 5-20 μm and the gram weight is 0.1-3.0 gsm.
[0090] When the intermediate fiber web layer includes an air-laid fiber web, the preparation method of the air-laid fiber web includes: crushing the second water-absorbent short fibers and then air-laying them to obtain the air-laid fiber web. The second water-absorbent fibers preferably include wood pulp fibers and / or pulp fibers; the wood pulp fibers include one or more of oak, poplar, birch, pine, spruce and fir; the pulp fibers include one or more of straw pulp, reed pulp, sugarcane pulp, bamboo pulp, cotton pulp, hemp pulp and natural fiber rag pulp. The mass of the second water-absorbent fibers in the intermediate fiber web layer accounts for preferably 10-47.5% of the total mass of the composite multi-layer nonwoven material, more preferably 25-45%, and further preferably 30-45%. The crushing is carried out in a grinding device. In the present invention, the first water-absorbent fibers are transported to the grinding device for crushing via a transmission device. If it is for loose fibers such as cotton, it can be cut by a cutting device first and then crushed by a grinding device, and the crushed fibers are evenly distributed in various parts by air-laying. The second air-laid web is preferably laid by a CD controllable ejector or by a forming head that is evenly distributed along the width direction, and the forming head is a dust cage type or a flat screen type. The length of the short fibers obtained by the second air-laid web is 0.5 to 8 mm. The compositions of the plurality of mixed spray fiber webs are the same or different. The compositions of the plurality of air-laid fiber webs are the same or different.
[0091] The second air-laid web preferably further comprises a third spray of water or a third chemical additive aqueous solution to the staple fiber bundle obtained by the second air-laid web, and the third spraying amount is preferably 0-180L / h, more preferably 100-180L / h, and further preferably 120-150L / h. The third spray is a water mist formed by spraying water or chemical additives with high-pressure small holes, so that the spray can quickly adhere to the staple fibers and filaments and then dry. The third chemical additive aqueous solution preferably comprises a third chemical additive and water, and the third chemical additive preferably comprises one or more of an antibacterial agent, a hydrophilic agent, a softener, a softener, a strength agent, an adhesive, a silicone, a wetting agent, a latex and a thermochromic colorant material; the latex comprises acrylic acid and / or ethylene vinyl acetate; the strength agent comprises carboxymethyl cellulose and / or starch; the adhesive comprises one or more of ethylene vinyl acetate, acrylic acid and other elastic adhesives. The percentage of the third chemical additive in the second chemical additive aqueous solution to the total mass of the composite multi-layer nonwoven material is preferably 0.1-10%, more preferably 1-5%, and most preferably 1-3%.
[0092] After obtaining the intermediate web layer, the present invention performs a third meltblowing and / or a second spunbonding of the third raw material on the surface of the intermediate web layer to form a second web layer to obtain a semi-finished web; the second web layer includes a plurality of stacked second meltblown webs and / or a plurality of second spunbonded webs, and the third raw material includes a third polymer raw material. In the present invention, the second web layer is also called a "scrim" layer, which can reduce the shedding of short absorbent fibers in the intermediate web layer and reduce linting. The third polymer raw material preferably includes degradable or compostable thermoplastic fibers and / or thermoplastic polymer filaments; the degradable or compostable thermoplastic fibers include one or more of polylactic acid, polyhydroxyalkanoate, polycaprolactone, polyester amide and copolymers thereof, polyvinyl alcohol, polyvinyl alcohol derivatives, cellulose, cellulose derivatives, proteins, starch, starch derivatives, chitosan, chitosan derivatives, hemicellulose and hemicellulose derivatives; the material of the thermoplastic polymer filaments includes one or more of polyolefins, polyesters, polyhydroxyalkanoates and polyhydroxybutyrates; the starch derivatives preferably The invention discloses a kind of polymer filaments, which are preferably selected from the group consisting of pregelatinized starch, acid-modified starch and oxidized starch; the chitosan derivatives preferably include one or more of chitosan oligosaccharides, chitosan quaternary ammonium salts, carboxymethyl chitosan and hydroxypropyl chitosan; the hemicellulose derivatives preferably include one or more of nonionic hemicellulose, anionic hemicellulose and cationic hemicellulose; the polymer filaments include a single component or a double component, and the double component includes one or more of a sheath-core type, a parallel type, a trilobal type and an orange segment type; the melt index of the thermoplastic polymer filaments ranges from 100 to 1500 g / 10 min. The melt index of the polymer material used in the third melt-blowing is preferably in the range of 300 to 1000 g / 10 min, more preferably 400 to 800 g / 10 min, and further preferably 500 to 700 g / 10 min. The melt index of the polymer material used in the second spunbond is preferably in the range of 10 to 100 g / 10 min, more preferably 10 to 60 g / 10 min, and further preferably 25 to 40 g / 10 min.
[0093] The mass of the third raw material in the second fiber web layer preferably accounts for 0.2-20% of the total mass of the composite multi-layer nonwoven material, more preferably 0.5-18%, and further preferably 5-15%; the second raw material also includes a third functional masterbatch, and the third functional masterbatch preferably includes one or more of a hydrophilic masterbatch, an elastic masterbatch, a degradable masterbatch, an antibacterial masterbatch, a cooling masterbatch, an antistatic masterbatch, and an anti-rust masterbatch. The mass of the third functional masterbatch in the second fiber web layer preferably accounts for 0.1-10% of the mass of the third polymer raw material, more preferably 0.5-5%, and further preferably 2-3%. The spinning temperature of the third meltblown is preferably 200°C to 290°C, more preferably 220-270°C, and further preferably 230-260°C. The hot air volume of the third meltblown is 800-2000Nm 3 / h. The third melt-blowing preferably also includes a fourth spray of water or a fourth chemical additive aqueous solution to the long fiber bundle obtained by the third melt-blowing. The fourth spray is a water mist formed by spraying water or chemical additives with a high-pressure small hole, so that the spray can quickly adhere to the staple fibers and filaments and then dry. The fourth spray volume is preferably 0-180L / h, more preferably 100-180L / h, and further preferably 120-150L / h, so that the spray can quickly adhere to the filaments and then dry. The fourth chemical additive aqueous solution preferably includes a fourth chemical additive and water, and the fourth chemical additive preferably includes one or more of an antibacterial agent, a hydrophilic agent, a softener, a softener, a strength agent, an adhesive, a silicone, a wetting agent, a latex and a thermochromic colorant material; the latex includes acrylic acid and / or ethylene vinyl acetate; the strength agent includes carboxymethyl cellulose and / or starch; the adhesive includes one or more of ethylene vinyl acetate, acrylic acid and other elastic adhesives. The percentage of the fourth chemical additive in the fourth chemical additive aqueous solution to the total mass of the composite multilayer nonwoven material is preferably 0.1-10%, more preferably 1-5%, and most preferably 1-3%. The diameter of the long fibers obtained by the third meltblowing is 5-20 μm and the gram weight is 0.1-3.0 gsm. The diameter of the long fibers obtained by the second spunbond is 5-20 μm and the gram weight is 0.1-3.0 gsm. The compositions of the plurality of second meltblown webs and / or the plurality of second spunbond webs are the same or different.
[0094] After obtaining the semi-finished fiber web, the present invention hot-rolls the semi-finished fiber web to obtain a hot-rolled fiber web. In the present invention, hot-rolling and shaping uses a hot-rolling device to perform hot-rolling and shaping in a dotted or other geometric shape, wherein the rollers of the hot-rolling device have a self-heating function. The temperature of the hot-rolling and shaping is preferably 80 to 200°C, more preferably 90 to 150°C, and further preferably 90 to 110°C. The speed is preferably 0 to 1000 m / min, and is not 0, more preferably 100 to 1000 m / min, further preferably 200 to 600 m / min, and most preferably 300 to 500 m / min. The pattern of the hot pressing roller is arranged in convex lateral directions along the width.
[0095] After obtaining the hot-rolled fiber web, the present invention pre-wets the hot-rolled fiber web and then sprays it with high-pressure water to obtain a jacquard high-pressure water-sprayed fiber web. The high-pressure water spraying includes sequentially performing flat-net forward spraying, drum reverse spraying, drum forward spraying and flat-net jacquard forward spraying. The flat-net forward spraying is to spray water on the upper surface of the hot-rolled fiber web, and at the same time, the lower surface is vacuumed; the drum reverse spraying is to spray water on the lower surface of the hot-rolled fiber web on the rotating circumference of the drum; the drum forward spraying is to spray water on the upper surface of the hot-rolled fiber web on the rotating circumference of the drum; the flat-net jacquard forward spraying is to spray water on the upper surface of the hot-rolled fiber web to form a jacquard pattern, and at the same time, the lower surface is vacuumed. In the present invention, the hot-rolled hot-rolled fiber web after hot rolling can be transferred to the high-pressure water spraying equipment in an offline or online manner. The hot-rolled fiber web is adsorbed on the surface of the drum for transmission. The present invention dehydrates the hot-rolled fiber web by vacuuming. The water pressure of the pre-wetting is preferably 0.1-5MPa, more preferably 0.5-4MPa, and further preferably 0.5-3MPa. The water pressure of the flat mesh forward spray is preferably 0.5-10MPa, more preferably 1-10MPa, and further preferably 3-8MPa. The water pressure of the rotary drum reverse spray is preferably 1-15MPa, more preferably 3-15MPa, and further preferably 5-12MPa. The water pressure of the rotary drum forward spray is preferably 1-15MPa, more preferably 3-15MPa, and further preferably 5-12MPa. The water pressure of the flat mesh jacquard forward spray is 3-20MPa, preferably 5-20MPa, and further preferably 8-18MPa; the vacuum degree of the vacuum during the flat mesh forward spray is preferably 15000-40000Pa, more preferably 16000-37000Pa, and further preferably 25000-35000Pa. The vacuum degree of the jacquard water spraying is preferably 15000-40000 Pa, more preferably 16000-37000 Pa, and further preferably 25000-35000 Pa. During the pre-wetting, the flat mesh forward spraying, the rotary drum reverse spraying, the rotary drum forward spraying, and the flat mesh jacquard forward spraying, the water spray holes of the high-pressure water spraying equipment used spray multiple fine water jets vertically toward the fiber web. During the rotary drum reverse spraying and the rotary drum forward spraying, the hot rolled fiber web is adsorbed on the surface of the perforated drum.
[0096] In a specific embodiment of the present invention: the hot-rolled web after hot rolling can be transferred to the high-pressure water spraying device in an offline or online manner. First, the hot-rolled web is pre-wetted by the roller pre-wetting device, and the roller and the net conveying curtain clamp the hot-rolled web, compact the fluffy web, and remove the air in the web, so that the capillary effect on the fiber surface is enhanced, thereby enhancing the moisture absorption performance of the textile. This is also conducive to improving the air permeability of the composite multi-layer non-woven material. The hot-rolled web is transferred to the high-pressure water spraying area, and the water spray holes of the high-pressure water spraying equipment spray multiple fine water jets vertically to the web. After passing through the first high-pressure water spraying device, the hot-rolled web is adsorbed on the surface of the perforated roller and transferred to the second high-pressure water spraying device and the third high-pressure water spraying device. The perforated roller can adjust the tension of the cloth edge to prevent deviation, which is conducive to high-speed production of the machine, and the perforated roller is conducive to timely removing excess moisture from the cloth surface. Then it is transported to the top of the second net conveying curtain through the conveying roller. The hydroentanglement jacquard mechanism uses a high-pressure water spray device to copy the pattern on the jacquard mechanism drum onto the composite multi-layer nonwoven material on the high-speed cloth surface, and then removes excess water through a vacuum suction device;
[0097] After obtaining the jacquard high-pressure water-jet web, the present invention sequentially dries and post-finishes the jacquard high-pressure water-jet web to obtain the composite multi-layer nonwoven material. In the present invention, the drying is preferably hot air drying. The drying temperature is preferably 90 to 130°C, more preferably 90 to 150°C, and further preferably 100 to 130°C. The post-finishing treatment preferably includes: one or more of spraying, roller coating and padding; the chemical additives used in the post-finishing preferably include one or more of antibacterial agents, hydrophilic agents, softeners, softeners, strength agents, adhesives, silicones, wetting agents, latex and thermochromic colorant materials; the latex includes acrylic acid and / or ethylene vinyl acetate; the strength agent includes carboxymethyl cellulose and / or starch; the adhesive includes one or more of ethylene vinyl acetate, acrylic acid and other elastic adhesives.
[0098] The present invention provides a composite multi-layer nonwoven material prepared by the preparation method described in the above technical scheme, comprising a first layer structure, an intermediate layer structure and a second layer structure stacked in sequence; the first layer structure is formed by a plurality of first meltblown fiber webs and / or a plurality of first spunbond fiber webs; the intermediate layer structure is formed by a plurality of mixed-spray fiber webs and / or a plurality of air-laid fiber webs, and the second layer structure is formed by a plurality of second meltblown fiber webs and / or a plurality of second spunbond fiber webs.
[0099] The weight of the finished product is preferably 10 to 300 gsm.
[0100] The present invention provides a device used in the preparation method described in the above technical solution, comprising a web-forming curtain, a web-forming device arranged above the web-forming curtain, the web-forming device comprising a plurality of first melt-blowing devices and / or a plurality of spunbonding devices, and also comprising a plurality of mixed spray systems and / or a plurality of second grinding devices, the second grinding device comprising a second crusher and a second air-flow web-forming device; the mixed spray system comprising a plurality of second melt-blowing devices, a plurality of first grinding devices and a mixed spray forming box, the first grinding device comprising a first crusher and a first air-flow web-forming device;
[0101] A hot rolling device arranged downstream of the mesh forming curtain, a first mesh transport curtain arranged downstream of the hot rolling device, a pre-wetting device and a first high-pressure water spraying device arranged above the first mesh transport curtain, a first vacuum dehydration device arranged below the first mesh transport curtain, a second high-pressure water spraying device and a third high-pressure water spraying device arranged downstream of the first mesh transport curtain, a second mesh transport curtain arranged downstream of the second and third high-pressure water spraying devices, a jacquard high-pressure water spraying device arranged above the second mesh transport curtain, a second vacuum dehydration device arranged below the second mesh transport curtain, a drying device arranged downstream of the second mesh transport curtain, and a finishing device arranged downstream of the drying device.
[0102] In the present invention, the structure of the composite multi-layer nonwoven material prepared by the present invention may include at least three layers and / or at least four layers and / or at least five layers and / or multiple layers. The mixed spray system may be one or two or more groups, and the melt-blowing device may be opened only one or all; the spunbond / melt-blown devices on both sides may be one set on each side, or one side may not have one set or more sets on the other side.
[0103] In the present invention, the web-forming device above the web-forming curtain is provided with the number and arrangement order of a plurality of first melt-blowing devices, a plurality of spunbonding devices, a plurality of mixing spray systems and a plurality of second grinding devices according to the layer structure of the composite multi-layer nonwoven material.
[0104] In the present invention, a first spray device is provided below the spinneret of the first melt-blowing device, a second spray device is provided below the discharge port of the mixed spray molding box, and a third spray device is provided below the second air-laid device;
[0105] The spinnerets of the first melt-blowing device and the second melt-blowing device include a first spinneret, a second spinneret or a third spinneret;
[0106] like Fig.10As shown, a single row of first spinneret holes is provided on the first spinneret plate, the first spinneret holes are inverted conical holes, the outer conical surface of the first spinneret holes is sleeved with first airflow drafting holes, the first airflow drafting holes are inverted conical holes and are coaxial with the first spinneret holes, the long fibers ejected from the first spinneret holes and the drafting gas ejected from the first airflow drafting holes converge at the apex, and the angle between the drafting gas and the long fibers is 30-70°;
[0107] like Figure 6 , Figure 7 and Figure 8 As shown, a single row or multiple rows of second spinneret holes are arranged on the second spinneret plate, the second spinneret holes are cylindrical holes, the outer circumference of the second spinneret holes is sleeved with second airflow drafting holes, the second airflow drafting holes are annular holes and are coaxial with the second spinneret holes;
[0108] like Figure 6 , Figure 7 and Figure 8 As shown, the third spinneret is provided with a single row or multiple rows of third air flow stretching holes, the third air flow stretching holes are cylindrical holes, the outer peripheral surface of the third air flow stretching holes is sleeved with third spinneret holes, the third spinneret holes are annular holes and are coaxial with the third air flow stretching holes.
[0109] The operating temperature of the spinnerets of the first melt-blowing device and the second melt-blowing device is preferably 200°C to 290°C.
[0110] In the present invention, the configuration form of the first melt-blowing device and the second melt-blowing device can be a "slit air knife" melt-blowing type or a "coaxial" melt-blowing type. Fig.10 As shown, the "slit air knife" meltblown type is that two drafting gas flows converge to form a single airflow, and the drafting gas forms an angle of about 30-70° with the direction of the filament flow. When the polymer filaments leave the spinneret holes in the meltblown die, they are cooled and stretched by the air knife, and finally bonded to the mesh curtain. Each spinneret hole of the "coaxial" meltblown type has an annular fluid release hole around it, and the drafting gas can form an angle of less than 10° with the direction of the filament flow, so that the basically parallel airflows coaxially stretch the polymer melt. When the configuration form of the meltblown device is the "slit air knife" meltblown type, the spinneret is a single row of holes; when the configuration form of the meltblown device is the "coaxial" meltblown type, the spinneret can be a single row of holes or multiple rows of holes, and the multiple rows of holes spinneret include 2 rows, 3 rows, 4 rows or more rows.
[0111] In the present invention, the pre-wetting device is specifically a drum pre-wetting device.
[0112] In the present invention, when the second high-pressure water spray device and the third high-pressure water spray device spray water with high pressure on the obtained hot-rolled fiber web, the hot-rolled fiber web is adsorbed on the surface of the perforated roller and transmitted to the second high-pressure water spray device and the third high-pressure water spray device. The perforated roller can adjust the tension of the cloth edge to prevent deviation, which is beneficial to high-speed production of the machine, and the perforated roller is conducive to timely removal of excess moisture from the cloth surface.
[0113] In the present invention, the pressure of the high-pressure water spraying device is 60-250 Bar.
[0114] In the present invention, the drying device is preferably an oven, and the types of ovens include tunnel type, round screen type, and infrared heating type. Finally, the drying device is subjected to post-finishing by post-finishing equipment to give the wiping material certain functionality.
[0115] The present invention obtains a composite nonwoven fabric with high water absorption, fast water absorption, high strength, fluffy surface, soft hand feel and low linting rate by combining short fibers with polymers sprayed by melt-blowing / spunbond technology in the form of layering or mixed spraying and combining with a high-pressure water spraying process.
[0116] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0117] Example 1
[0118] This embodiment adopts Figure 1 The device shown is used to prepare composite multilayer nonwoven materials, such as Figure 1 The equipment shown includes: a first melt-blowing device, a first spraying device, a first mixed spraying system, the first mixed spraying system includes a third melt-blowing device, a first grinding device, a fourth melt-blowing device and a first mixed spraying forming box, a second spraying device, a second grinding device, a third spraying device, a first spunbonding device, a hot rolling device, a drum pre-wetting device, a first high-pressure water spraying device, a first vacuum dehydration device, a first mesh conveying curtain, a second mesh conveying curtain, a second high-pressure water spraying device, a third high-pressure water spraying device, a conveying roller, a jacquard high-pressure water spraying device, a jacquard water spunlace machine drum, a second vacuum dehydration device, a drying device, a finishing device, a mesh curtain and a suction air device;
[0119] Step 1: Using the first melt-blowing device, the two-component parallel polypropylene / polyester accounting for 6% of the total mass of the composite multi-layer non-woven material and the soft masterbatch are mixed, heated and melted, and then sprayed onto the mesh curtain to form a first melt-blown fiber web layer, wherein the soft masterbatch accounts for 1% of the mass of the two-component parallel polypropylene / polyester. The first spraying device is arranged in the first spinneret attachment of the first melt-blowing device to spray the hydrophilic additive accounting for 0.67% of the total mass of the composite multi-layer non-woven material with high-pressure small holes.
[0120] Step 2: Mix and heat the bi-component parallel polypropylene / polyester and water-absorbing masterbatch accounting for 12% of the total mass of the composite multi-layer non-woven material from the third melt-blown device and the fourth melt-blown device, wherein the water-absorbing masterbatch accounts for 2% of the mass of the bi-component parallel polypropylene / polyester, and transport the wood pulp fiber accounting for 50% of the total mass of the composite multi-layer non-woven material to the first grinding device through the transmission device for crushing, and distribute and lay the net through the CD controllable ejector, and the wood pulp fiber is finally mixed with the polymer material and the filament sprayed out by the high-temperature mixing of the water-absorbing masterbatch in the forming box to form a first mixed spray water-absorbing layer covering the first melt-blown fiber mesh layer. The first mixed spray system has a spray device, and the high-pressure small hole sprays the hydrophilic additive accounting for 0.67% of the total mass of the composite multi-layer non-woven material at 125L / h.
[0121] Step 3: The cotton pulp fibers accounting for 18% of the total mass of the composite multi-layer non-woven material crushed by the second grinding device are evenly distributed along the width direction for laying the net using a forming head, the forming head is a dust cage type, and a water-absorbing layer is formed to cover the mixed spray water-absorbing layer. The second grinding device is equipped with a spraying device, and a hydrophilic additive accounting for 0.67% of the total mass of the composite multi-layer non-woven material is sprayed at 125L / h with a high-pressure small hole.
[0122] Step 4: using a first spunbond device, mixing, heating and melting polypropylene accounting for 10% of the total mass of the composite multi-layer nonwoven material and spraying it onto the mesh curtain to form a first spunbond fiber web layer covering the water-absorbing layer.
[0123] Step 5: The meltblown fiber mesh layer, mixed spray water-absorbing layer, water-absorbing layer and spunbond fiber mesh layer formed by steps 1 to 4 are stacked on a mesh curtain and are subjected to hot rolling shaping in a geometric shape using a hot rolling mill at a temperature of 105°C to form a semi-finished product having two layers of spunbond and meltblown fiber mesh layers, and a mixed spray water-absorbing layer and a water-absorbing layer in the middle.
[0124] Step 6: Use a dot pattern to hot-roll and fix first, and then transfer the semi-finished product of step 5 to the high-pressure water spraying equipment by offline or online methods. First, pre-wet the semi-finished product of step 5 with a pre-wetting pressure of 0.5Mpa, and then transfer it to the first high-pressure water spraying device with a pressure of 8Mpa, the vacuum degree of the vacuum dehydration box is 25000pa, the pressure of the second high-pressure water spraying device is 12Mpa, and the pressure of the third high-pressure water spraying device is 11Mpa, and then it is transported to the top of the second mesh curtain through the conveying roller.
[0125] Step 7: The spunlace jacquard mechanism uses a high-pressure water spray device to copy the pattern on the jacquard mechanism drum onto the semi-finished product of step 6 on the high-speed cloth surface, wherein the pressure of the jacquard high-pressure water spray device is 15Mpa, and the vacuum degree of the vacuum dehydration box is 27000pa, forming a jacquard pattern on the surface of the semi-finished product of step 6.
[0126] Step 8: The semi-finished product of step 7 after dehydration is transferred to a hot air flow penetration oven by a mesh curtain, and the hot air drying temperature is 110°C. Finally, it is finished by a finishing equipment, and 2% antibacterial agent is used for finishing to enhance the antibacterial properties of the material, meet the special needs of consumers, and obtain a composite multi-layer non-woven material.
[0127] The composite multi-layer nonwoven material prepared in this embodiment is used to produce a 70gsm maternity pad. The composite material of this embodiment is composed of 4 fiber web layers, namely a first meltblown fiber web layer, a first mixed spray water-absorbing layer, a water-absorbing layer and a first spunbond fiber web layer. The meltblown polymer material used in the first meltblown device is a two-component parallel polypropylene / polyester with a melt index of 650g / 10min (LyondellBasell, London, UK), and a soft masterbatch (Dawn, China). The total mass of the soft masterbatch and the meltblown polymer material accounts for 6% of the total weight of the composite multi-layer nonwoven material prepared in this embodiment, and the soft masterbatch accounts for 1% of the polymer material in the first meltblown device; the polymer material used in the third and fourth meltblown devices is a two-component parallel polypropylene / polyester with a melt index of 650g / 10min. Ester (LyondellBasell, London, UK) and water-absorbing masterbatch (Dawn, China), the total mass of the water-absorbing masterbatch and the melt-blown polymer material used in the third melt-blowing device accounts for 6% of the total weight of the composite multi-layer non-woven material prepared in this embodiment, wherein the water-absorbing masterbatch used in the third melt-blowing device accounts for 2% of the polymer material in the third melt-blowing device; the total mass of the water-absorbing masterbatch and the melt-blown polymer material used in the fourth melt-blowing device accounts for 6% of the total weight of the composite multi-layer non-woven material prepared in this embodiment, wherein the water-absorbing masterbatch used in the fourth melt-blowing device accounts for 2% of the polymer material in the first melt-blowing device. A hydrophilic additive (Zhejiang Chuanghua Chemical) is used for spraying, and the hydrophilic additive accounts for 2% of the total weight. The first spunbond device uses polypropylene with a melt index of 35g / 10min (Zhejiang Jinchun Polymer Materials Co., Ltd.), and the spunbond polypropylene raw material accounts for 10% of the total weight. The raw material used for the short fiber in the first mixed spray water-absorbing layer is wood pulp (GP Company, USA), and wood pulp accounts for 50% of the total weight. The water-absorbing layer uses 18% cotton pulp (Manas Xiangyun Chemical Fiber Co., Ltd.), and 2% antibacterial agent (Zhejiang Chuanghua Chemical) is used in step eight.
[0128] Example 2
[0129] This embodiment adopts Figure 2 The device shown is used to prepare composite multilayer nonwoven materials, such as Figure 2The equipment shown includes: a first melt-blowing device, a first spraying device, a first mixed spraying system, the first mixed spraying system includes a third melt-blowing device, a first grinding device, a fourth melt-blowing device and a first mixed spraying molding box, a second spraying device, a second mixed spraying system, the second mixed spraying system includes a fifth melt-blowing device, a second grinding device, a sixth melt-blowing device and a first mixed spraying molding box, a third spraying device, a second melt-blowing device, a fourth spraying device, a hot rolling device, a drum pre-wetting device, a first high-pressure water spraying device, a first vacuum dehydration device, a first mesh conveying curtain, a second mesh conveying curtain, a second high-pressure water spraying device, a third high-pressure water spraying device, a conveying roller, a jacquard high-pressure water spraying device, a jacquard water spunlace machine drum, a second vacuum dehydration device, a drying device, a finishing device, a mesh curtain and a suction air device;
[0130] Step 1: Use the first melt-blowing device to mix and heat the polypropylene and hydrophilic soft masterbatch accounting for 8% of the total mass of the composite multi-layer non-woven material, and then spray them onto the mesh curtain to form the first melt-blown fiber mesh layer, wherein the hydrophilic soft masterbatch accounts for 3% of the mass of the polypropylene. The first spray device is arranged in the attachment of the first spinneret of the first melt-blowing device, and the high-pressure small hole sprays ultrapure water at 120L / h to cool the melt-blown filaments.
[0131] Step 2: Mix and heat the polypropylene and elastomer masterbatch of the third meltblown device, which is 6% of the total mass of the composite multi-layer nonwoven material, and melt them, wherein the elastomer masterbatch accounts for 2% of the mass of the polypropylene; Mix and heat the polypropylene elastomer masterbatch of the fourth meltblown device, which is 6% of the total mass of the composite multi-layer nonwoven material, and melt them, wherein the elastomer masterbatch accounts for 2% of the mass of the polypropylene. The wood pulp fiber raw material accounting for 28.5% of the total mass of the composite multi-layer nonwoven material is transported to the first grinding device through the transmission device for crushing, and is evenly distributed through the flat screen forming head. The wood pulp fiber is finally mixed with the filaments sprayed out by the high-temperature mixing of polypropylene and the water-absorbing masterbatch in the forming box to form a mixed spray water-absorbing layer covering the first meltblown fiber mesh layer.
[0132] Step 3: Mix and heat the polypropylene of the fifth melt-blown device, which is 6% of the total mass of the composite multi-layer non-woven material, with the elastomer masterbatch, wherein the elastomer masterbatch accounts for 2% of the mass of the polypropylene; Mix and heat the polypropylene of the sixth melt-blown device, which is 6% of the total mass of the composite multi-layer non-woven material, with the elastomer masterbatch, wherein the elastomer masterbatch accounts for 2% of the mass of the polypropylene. The wood pulp fiber raw material accounting for 28.5% of the total mass of the composite multi-layer non-woven material is transported to the second grinding device through the transmission device for crushing, and is evenly distributed through the flat screen forming head. The wood pulp fiber is finally mixed with the filaments sprayed out by the high-temperature mixing of the polypropylene water-absorbing masterbatch in the forming box to form a second mixed spray water-absorbing layer covering the first mixed spray water-absorbing layer.
[0133] Step 4: Using a second melt-blown device, 8% of the total mass of the composite multi-layer nonwoven material is mixed with hydrophilic soft masterbatch, heated and melted, and then sprayed onto the mesh curtain, wherein the hydrophilic soft masterbatch accounts for 3% of the mass of the polypropylene, to form a second melt-blown fiber mesh layer covering the second mixed spray water-absorbing layer. The first spray device is set in the fourth spinneret attachment of the second melt-blown device, and the high-pressure small hole sprays ultrapure water at 120L / h to cool the melt-blown filaments.
[0134] Step 5: The first meltblown web layer, the first mixed spray absorbent layer, the second mixed spray absorbent layer and the second meltblown web layer formed by steps 1 to 4 are stacked on a web curtain and are subjected to hot rolling shaping of a geometric shape using a hot rolling mill at a temperature of 103°C to form a semi-finished product having a spunbond web layer and a meltblown web layer as the upper and lower layers, respectively, and a mixed spray absorbent layer in the middle.
[0135] Step 6: Use the hot rolling mill to fix the non-woven fabric in a point shape, and then transfer the semi-finished product of step 5 to the high-pressure water spraying equipment offline or online. First, pre-wet the semi-finished product of step 5 at a pressure of 0.6Mpa, and then transfer it to the first high-pressure water spraying device at a pressure of 7Mpa, the vacuum degree of the vacuum dehydration box is 26000pa, the pressure of the second high-pressure water spraying device is 11.5Mpa, and the pressure of the third high-pressure water spraying device is 11.5Mpa, and then it is transported to the top of the second mesh curtain through the conveying roller.
[0136] Step 7: The spunlace jacquard mechanism uses a high-pressure water spray device to copy the pattern on the jacquard mechanism drum onto the semi-finished product of step 6 on the high-speed cloth surface, wherein the pressure of the jacquard high-pressure water spray device is 13Mpa, and the vacuum degree of the vacuum dehydration box is 25000pa, forming a jacquard pattern on the surface of the semi-finished product of step 6.
[0137] Step 8: The semi-finished product of step 7 after dehydration is transferred to a rotary screen oven by a screen curtain, and the hot air drying temperature is 100°C. Finally, it is finished by a finishing device, and a 3% hydrophilic additive is used for spray finishing to enhance the hygroscopicity of the material to obtain a composite multi-layer nonwoven material.
[0138] The composite multi-layer nonwoven material prepared in this embodiment is used to produce 70gsm disposable shirt fabric. The composite multi-layer nonwoven material of this embodiment is composed of 4 fiber mesh layers, namely the first melt-blown fiber mesh layer, the first mixed spray water-absorbing layer, the second mixed spray water-absorbing layer, and the second melt-blown fiber mesh spray layer. The third melt-blown device, the fourth melt-blown device, the fifth melt-blown device, and the sixth melt-blown device use polypropylene (LyondellBasell, London, UK) with a melt index of 650g / 10min and elastomer masterbatch (Dawn, China), wherein the elastomer masterbatch accounts for 2% of the mass of polypropylene, and the total mass of polypropylene and elastomer masterbatch in the third melt-blown device, the fourth melt-blown device, the fifth melt-blown device, and the sixth melt-blown device each accounts for 6% of the total weight of the composite multi-layer nonwoven material prepared in this embodiment; wherein the elastomer masterbatch accounts for 2% of the mass of polypropylene in the third melt-blown device, the fourth melt-blown device, the fifth melt-blown device, and the sixth melt-blown device;
[0139] The first melt-blowing device and the second melt-blowing device use 8% polypropylene with a melt index of 650g / 10min and hydrophilic soft masterbatch (Dawn, China), wherein the hydrophilic soft masterbatch accounts for 3% of the mass of polypropylene; the total mass of polypropylene and hydrophilic soft masterbatch in the first melt-blowing device and the second melt-blowing device each accounts for 8% of the total weight of the composite multi-layer nonwoven material prepared in this embodiment; wherein the hydrophilic soft masterbatch accounts for 3% of the mass of polypropylene in the first melt-blowing device and the second melt-blowing device;
[0140] The raw material used for the staple fibers is wood pulp (GP Company, USA), which accounts for 57% of the total weight, and the hydrophilic additive (Zhejiang Chuanhua Chemical) in step eight accounts for 3% of the total weight.
[0141] Example 3
[0142] This embodiment adopts Figure 3 The device shown is used to prepare composite multilayer nonwoven materials, such as Figure 3 The equipment shown includes: a second spunbond device, a first meltblown device, a first spray device, a first grinding device, a third spray device, a second meltblown device, a fourth spray device, a hot rolling device, a drum pre-wetting device, a first high-pressure water spray device, a first vacuum dehydration device, a first mesh conveying curtain, a second mesh conveying curtain, a second high-pressure water spray device, a third high-pressure water spray device, a conveying roller, a jacquard high-pressure water spray device, a jacquard water spunlace machine drum, a second vacuum dehydration device, a drying device, a finishing device, a mesh curtain and a suction air device;
[0143] Step 1: Use a second spunbond device to heat and melt the degradable polyester amide and hydrophilic soft masterbatch accounting for 12% of the total mass of the composite multi-layer non-woven material, and then spray them onto the mesh curtain, wherein the hydrophilic soft masterbatch accounts for 3% of the mass of the degradable polyester amide, to form a first spunbond fiber mesh layer.
[0144] Step 2: Use the first meltblown device to heat and melt the degradable polylactic acid and hydrophilic soft masterbatch accounting for 9% of the total mass of the composite multi-layer non-woven material, and then spray them onto the mesh curtain, wherein the hydrophilic soft masterbatch accounts for 3% of the mass of the degradable polyester amide, to form a first meltblown fiber web layer covering the first spunbond fiber web layer.
[0145] Step 3: transporting wood pulp fibers accounting for 68% of the total mass of the composite multi-layer nonwoven material to the first grinding device through a transmission device for crushing, and evenly distributing them through a flat screen forming head to form a water-absorbing layer which is layered on the first meltblown fiber web layer along the width direction.
[0146] Step 4: Use the third spray device to heat and melt the degradable polylactic acid and hydrophilic soft masterbatch accounting for 9% of the total mass of the composite multi-layer non-woven material, and spray them onto the mesh curtain, wherein the hydrophilic soft masterbatch accounts for 3% of the mass of the degradable polyester amide, to form a second melt-blown fiber web layer covering the water-absorbing layer.
[0147] Step 5: The first spunbond web layer, the first meltblown web layer, the water-absorbing layer, and the second meltblown web spray layer formed by steps 1 to 4 are stacked on a web curtain and are subjected to hot rolling shaping of a geometric shape using a hot rolling mill at a temperature of 105°C to form a semi-finished product having a spunbond web layer and a meltblown web layer as the upper and lower layers, respectively, and a water-absorbing layer and a first meltblown layer in the middle.
[0148] Step 6: Use a hot rolling mill to first fix the non-woven fabric in a point shape, and then transfer the semi-finished composite multi-layer non-woven material of step 5 to the high-pressure water spraying device in an offline or online manner. First, pre-wet the semi-finished composite multi-layer non-woven material of step 5 at a pre-wetting pressure of 0.5Mpa, and then transfer it to the first high-pressure water spraying device at a pressure of 7Mpa, the vacuum degree of the vacuum dehydration box is 26000pa, the pressure of the second high-pressure water spraying device is 12Mpa, and the pressure of the third high-pressure water spraying device is 12Mpa, and then it is transported to the top of the second mesh curtain through the conveying roller.
[0149] Step 7: The spunlace jacquard mechanism uses a high-pressure water spray device to copy the pattern on the jacquard mechanism drum onto the semi-finished product of step 6 on the high-speed cloth surface, wherein the pressure of the jacquard high-pressure water spray device is 15Mpa, and the vacuum degree of the vacuum dehydration box is 25000pa, forming a jacquard pattern on the surface of the semi-finished product of step 6.
[0150] Step 8: The semi-finished product of step 7 after dehydration is transferred to a rotary screen oven by a mesh curtain, and the hot air drying temperature is 102°C. Finally, it is finished by a finishing device. A 2% hydrophilic additive is used for roller coating to enhance the hygroscopicity of the material, thereby obtaining a composite multi-layer nonwoven material.
[0151] The composite multi-layer nonwoven material prepared in this embodiment is used to produce a 70gsm disposable biodegradable bath towel material. The composite material of this embodiment is composed of 4 fiber web layers, a first spunbond fiber web layer, a first meltblown fiber web layer, a water-absorbing layer, and a second meltblown fiber web spray layer. The first melt-blown device and the second melt-blown device use degradable polylactic acid (LyondellBasell, London, UK) with a melt index of 450g / 10min and a hydrophilic soft masterbatch (Dawn, China). The total mass of the hydrophilic soft masterbatch and the melt-blown degradable polylactic acid in the first melt-blown device and the second melt-blown device each accounts for 9% of the total weight of the composite multi-layer non-woven material prepared in this embodiment, wherein the hydrophilic soft masterbatch each accounts for 3% of the degradable polylactic acid in the first melt-blown device and the second melt-blown device; the second spunbond device uses a melt index of 45g / 10min, and the raw materials are degradable polylactic acid (LG, South Korea) and hydrophilic soft masterbatch accounting for 12% of the total weight of the composite multi-layer non-woven material prepared in this embodiment, and the hydrophilic soft masterbatch accounts for 3% of the degradable polylactic acid in the second spunbond device; the raw material used for the staple fiber is wood pulp (GP Company, the United States), and the wood pulp accounts for 68% of the total weight. The hydrophilic additive (Zhejiang Chuanhua Chemical) in step eight accounts for 2% of the total mass.
[0152] Example 4
[0153] This embodiment adopts Figure 4 The device shown is used to prepare composite multilayer nonwoven materials, such as Figure 4 The equipment shown includes: a second spunbond device, a third spunbond device, a first mixed spray system, the first mixed spray system includes a third melt-blown device, a first grinding device, a fourth melt-blown device and a first mixed spray molding box, a second spray device, a second melt-blown device, a fourth spray device, a seventh melt-blown device, a fifth spray device, a hot rolling device, a drum pre-wetting device, a first high-pressure water spray device, a first vacuum dehydration device, a first mesh curtain, a second mesh curtain, a second high-pressure water spray device, a third high-pressure water spray device, a conveying roller, a jacquard high-pressure water spray device, a jacquard water spunlace machine drum, a second vacuum dehydration device, a drying device, a finishing device, a mesh curtain and a suction air device;
[0154] Step 1: Using a second spunbond device, heat and melt the bicomponent polyester / polyamide masterbatch accounting for 12% of the total mass of the composite multi-layer nonwoven material and spray it onto the mesh curtain to form a first spunbond fiber web layer.
[0155] Step 2: Using a third spunbond device, heat and melt the bicomponent polyester / polyamide masterbatch accounting for 12% of the total mass of the composite multi-layer nonwoven material, and then spray it onto the mesh curtain to form a second spunbond fiber web layer.
[0156] Step three: The third and fourth melt-blown devices are respectively used to mix and melt 12% of the total mass of the composite multi-layer non-woven material with the reinforcing masterbatch, wherein the reinforcing masterbatch accounts for 1% of the mass of the polyester, and 26% of the wood pulp fiber raw materials are transported to the grinding device through a transmission device for crushing, and are evenly distributed through a flat screen forming head. The wood pulp fibers are finally mixed with the filaments sprayed out by the high-temperature mixture of polypropylene / polyester and the water-absorbing masterbatch in a forming box to form a first mixed spray water-absorbing layer covering the second spunbond web layer.
[0157] Step 4: Use a second meltblown device to mix 12% of the total mass of the composite multi-layer nonwoven material with the reinforcing masterbatch, heat and melt, and then spray it onto the mesh curtain, where the reinforcing masterbatch accounts for 1% of the mass of the polyester, to form a second meltblown fiber mesh layer covering the first mixed spray water-absorbing layer.
[0158] Step 5: Use the seventh meltblown device to mix the polyester accounting for 12% of the total mass of the composite multi-layer non-woven material with the reinforcing masterbatch, heat and melt, and then spray it onto the mesh curtain, wherein the reinforcing masterbatch accounts for 1% of the mass of the polyester, to form a third meltblown fiber web layer covering the second meltblown fiber web layer.
[0159] Step six: The first spunbond web layer, the second spunbond web layer, the first mixed spray absorbent layer, the second meltblown web spray layer, and the third meltblown web layer formed by steps one to five are stacked on a web curtain and are subjected to hot rolling shaping of geometric shapes using a hot rolling mill at a temperature of 100°C to form a semi-finished product having a spunbond web layer and a meltblown web layer as the upper and lower layers, respectively, and a second spunbond web layer, a first mixed spray absorbent layer, and a second meltblown layer in the middle.
[0160] Step 7: Use the hot rolling mill to fix the non-woven fabric in a point shape, and then transfer the semi-finished product of step 6 to the high-pressure water spraying equipment offline or online. First, pre-wet the semi-finished product of step 6 at a pressure of 0.6Mpa, and then transfer it to the first high-pressure water spraying device at a pressure of 7Mpa, the vacuum degree of the vacuum dehydration box is 24500pa, the pressure of the second high-pressure water spraying device is 10Mpa, and the pressure of the third high-pressure water spraying device is 10Mpa, and then it is transported to the top of the second mesh curtain through the conveying roller.
[0161] Step 8: The spunlace jacquard mechanism uses a high-pressure water spray device to copy the pattern on the jacquard mechanism drum onto the semi-finished product of step 7 on the high-speed cloth surface, wherein the pressure of the jacquard high-pressure water spray device is 12Mpa, and the vacuum degree of the vacuum dehydration box is 23000pa, forming a jacquard pattern on the surface of the semi-finished product of step 7.
[0162] Step nine: The semi-finished product of step eight after dehydration is transferred to a rotary screen oven by a mesh curtain, and the hot air drying temperature is 100°C. Finally, it is finished by a finishing device. A 2% antibacterial hydrophilic additive is used for spray finishing to enhance the antibacterial and hygroscopic properties of the material, meet the needs of consumers for the product, and obtain a composite multi-layer non-woven material.
[0163] The composite multilayer nonwoven material prepared in this embodiment is used to produce 70gsm disposable slipper materials. The composite material of this embodiment is composed of 5 fiber mesh layers, a first spunbond fiber mesh layer, a second spunbond fiber mesh layer, a first mixed spray water absorption layer, a second meltblown fiber mesh spray layer, and a third meltblown fiber mesh layer. The first and second spunbond devices use 12% bicomponent polyester / polyamide masterbatch (LyondellBasell, London, UK) with a melt index of 35g / 10min; the second meltblown device, the third meltblown device, the fourth meltblown device, and the seventh meltblown device use polyester (LyondellBasell, London, UK) and reinforcing masterbatch with a melt index of 650g / 10min, each accounting for 12% of the total weight of the composite multi-layer non-woven material prepared in this embodiment, wherein the reinforcing masterbatch each accounts for 1% of the mass of the polyester in the second meltblown device, the third meltblown device, the fourth meltblown device, and the seventh meltblown device; the raw material used for the staple fiber is wood pulp (GP Company, the United States), which accounts for 26% of the total weight; and the antibacterial hydrophilic additive (Zhejiang Chuanhua Chemical) in step nine accounts for 2% of the total mass.
[0164] Example 5
[0165] This embodiment adopts Figure 5 The device shown is used to prepare composite multilayer nonwoven materials, such as Figure 5 The equipment shown includes: a second spunbond device, a third spunbond device, a fourth spunbond device, a first mixed spray system, the first mixed spray system includes a third melt-blown device, a first grinding device, a fourth melt-blown device and a first mixed spray molding box, a second spray device, a second melt-blown device, a fourth spray device, a hot rolling device, a drum pre-wetting device, a first high-pressure water spray device, a first vacuum dehydration device, a first mesh conveying curtain, a second mesh conveying curtain, a second high-pressure water spray device, a third high-pressure water spray device, a conveying roller, a jacquard high-pressure water spray device, a jacquard water spunlace machine drum, a second vacuum dehydration device, a drying device, a finishing device, a mesh curtain and a suction air device;
[0166] Step 1: Using a second spunbond device, 10% of the total weight of the composite multi-layer nonwoven material is mixed with a reinforcing masterbatch, heated and melted, and then sprayed onto a mesh curtain, wherein the reinforcing masterbatch accounts for 1% of the weight of the polyester masterbatch, to form a first spunbond fiber mesh layer.
[0167] Step 2: Use a third spunbond device to mix 10% polyester and 1% reinforcing masterbatch of the total weight of the composite multi-layer nonwoven material, heat and melt them, and then spray them onto the mesh curtain, wherein the reinforcing masterbatch accounts for 1% of the weight of the polyester masterbatch, to form a second spunbond web layer covering the first spunbond web layer.
[0168] Step 3: Use the fourth spunbond device to mix and heat the polyester masterbatch accounting for 10% of the total mass of the composite multi-layer non-woven material with the reinforcing masterbatch, and then spray it onto the mesh curtain, wherein the reinforcing masterbatch accounts for 1% of the mass of the polyester masterbatch, to form a third spunbond fiber mesh layer covering the second spunbond fiber mesh layer.
[0169] Step 4: The third and fourth melt-blown devices are respectively used to mix, heat and melt the polyester masterbatch accounting for 9% of the total mass of the composite multi-layer non-woven material, and 40% of the rag pulp fiber raw materials are transported to the grinding device through the transmission device for crushing, and are evenly distributed through the flat screen forming head. The rag pulp fibers are finally mixed with the filaments sprayed out by the high-temperature mixture of polypropylene / polyester and the water-absorbing masterbatch in the forming box to form a first mixed spray water-absorbing layer covering the third spunbond fiber web layer.
[0170] Step 5: Using a second melt-blown device, the polyester masterbatch accounting for 9% of the total mass of the composite multi-layer nonwoven material is mixed, heated and melted, and then sprayed onto the mesh curtain to form a second melt-blown fiber mesh layer covering the first mixed spray water-absorbing layer.
[0171] Step six: The first spunbond web layer, the second spunbond web layer, the third spunbond web layer, the first mixed spray absorbent layer, and the second meltblown web spray layer formed by steps one to five are stacked on a web curtain and are subjected to hot rolling shaping of geometric shapes using a hot rolling mill at a temperature of 115°C to form a semi-finished product having a spunbond web layer and a meltblown web layer as the upper and lower layers, respectively, and a second spunbond web layer, a third spunbond web layer, and a first mixed spray absorbent layer in the middle.
[0172] Step 7: Use the hot rolling mill to fix the non-woven fabric in a point shape, and then the semi-finished product of step 6 can be transferred to the high-pressure water spraying equipment offline or online. First, the semi-finished product of step 6 is pre-wetted with a pre-wetting pressure of 1Mpa, and then transferred to the first high-pressure water spraying device with a pressure of 8Mpa, the vacuum degree of the vacuum dehydration box is 27000pa, the pressure of the second high-pressure water spraying device is 12Mpa, and the pressure of the third high-pressure water spraying device is 12Mpa, and then it is transported to the top of the second mesh curtain through the conveying roller.
[0173] Step 8: The spunlace jacquard mechanism uses a high-pressure water spray device to copy the pattern on the jacquard mechanism drum onto the semi-finished product of step 7 on the high-speed cloth surface, wherein the pressure of the jacquard high-pressure water spray device is 15Mpa, and the vacuum degree of the vacuum dehydration box is 26000pa, forming a jacquard pattern on the surface of the semi-finished product of step 7.
[0174] Step nine: The semi-finished product after dehydration is conveyed to the rotary screen oven by the conveying screen curtain, and the hot air drying temperature is 120℃. Finally, it is sprayed with 3% detergent through the finishing equipment, and then the material is cut into products of 6×6 cm in size and stacked into 5 layers. The upper and lower edges are hot-rolled at high temperature by about 0.5 cm so that the 5 layers are bonded together to meet the consumer's demand for the product and obtain a composite multi-layer non-woven material.
[0175] The composite multi-layer nonwoven material prepared in this embodiment is used to produce 70gsm disposable toilet cleaning brush material. The composite material of this embodiment is composed of 5 layers of fiber mesh layers. The second spunbond device, the third spunbond device and the fourth spunbond device use polyester (LyondellBasell, London, UK) with a melt index of 35g / 10min, each accounting for 10% of the total weight of the composite multi-layer nonwoven material prepared in this embodiment, and the reinforcing masterbatch (Dawn, China), wherein the reinforcing masterbatch each accounts for 1% of the mass of polyester in the second spunbond device, the third spunbond device and the fourth spunbond device; the second, third and fourth melt-blown devices use 9% polyester masterbatch (LyondellBasell, London, UK) with a melt index of 650g / 10min, and the raw material used for short fibers is recycled rag pulp, which accounts for 40% of the total weight, and the step nine cleaning agent (Zhejiang Chuanhua Chemical) accounts for 3% of the total mass.
[0176] Table 1 shows the performance test results of Examples 1 to 5 and a commercially available product (Mujin Diary Feather-Feathered Cotton Towel).
[0177] Table 1 Comparison of performance test results of composite nonwoven materials in Examples 1 to 5 on the market Mujin Diary Feather-Feathered Cotton Towel
[0178]
[0179] From Table 1, we can see that:
[0180] (1) Under the same gram weight conditions, the materials prepared in Examples 1-5 have a higher thickness (fluffiness) than commercially available products, which is about 55% higher. Since the middle layer of the embodiment includes a meltblown layer or a spunbond layer, the strength of the composite nonwoven material is improved by more than 50%, and a certain proportion of reinforcing masterbatch can be mixed into the raw materials. Therefore, Examples 4 and 5 can obtain better strength, which is 86% higher than the strength of the added product, thereby increasing the service life of the material.
[0181] (2) The present invention also provides a spraying device at the nozzle of the melt-blowing system and the mixed spraying system, and the hydrophilic additive is sprayed by the spraying device, so that the hydrophilic property of the non-woven fabric is greatly improved, and the water absorption performance is more than 50% higher than that of commercially available products.
[0182] It can be seen from the above embodiments that the present invention significantly reduces the flocculent coefficient by adding an online or offline high-pressure water spraying device, and greatly improves the air permeability, which is more than 1.2 times higher than that of commercially available products.
[0183] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing a composite multilayer nonwoven material, characterized in that: The following steps are involved: Performing a first meltblowing and / or a first spunbonding on a first raw material to obtain a first web layer, wherein the first web layer comprises a plurality of stacked first meltblown webs and / or a plurality of first spunbonded webs, and the first raw material comprises a first polymer raw material; Prepare an intermediate fiber web layer on the surface of the first fiber web layer, wherein the intermediate fiber web layer includes a plurality of stacked mixed-spray fiber webs and / or a plurality of air-laid fiber webs; The preparation method of the mixed-spray fiber web comprises: performing a second melt-blowing on a second raw material, performing a first air-laying after crushing the first water-absorbent fiber, and mixing and spraying the long fiber bundle obtained by the second melt-blowing and the short fiber bundle formed by the first air-laying to obtain the mixed-spray fiber web, wherein the second raw material comprises a second polymer raw material; the preparation method of the air-laid fiber web comprises: performing a second air-laying after crushing the second water-absorbent fiber; On the surface of the intermediate fiber web layer, the third raw material is subjected to a third meltblowing and / or a second spunbonding to form a second fiber web layer to obtain a semi-finished fiber web; the second fiber web layer comprises a plurality of stacked second meltblown fiber webs and / or a plurality of second spunbonded fiber webs, and the third raw material comprises a third polymer raw material; Hot-rolling the semi-finished fiber web to obtain a hot-rolled fiber web; the first fiber web layer of the semi-finished fiber web forms the lower surface of the hot-rolled fiber web, and the second fiber web layer of the semi-finished fiber web forms the upper surface of the hot-rolled fiber web; The hot-rolled fiber web is pre-wetted and then subjected to high-pressure water spraying to obtain a jacquard high-pressure water-sprayed fiber web, wherein the high-pressure water spraying includes sequentially performing flat-net forward spraying, drum reverse spraying, drum forward spraying and flat-net jacquard forward spraying, wherein the flat-net forward spraying is to spray water onto the upper surface of the hot-rolled fiber web, and simultaneously the lower surface is vacuumed; the drum reverse spraying is to spray water onto the lower surface of the hot-rolled fiber web on the rotating circumferential surface of the drum, and the drum forward spraying is to spray water onto the upper surface of the hot-rolled fiber web on the rotating circumferential surface of the drum; the flat-net jacquard forward spraying is to spray water onto the upper surface of the hot-rolled fiber web to form a jacquard pattern, and simultaneously the lower surface is vacuumed; The jacquard high-pressure water-jet fiber web is dried and post-finished in sequence to obtain the composite multi-layer nonwoven material.
2. The preparation method according to claim 1, characterized in that: The first melt-blowing further comprises spraying water or a first chemical additive aqueous solution to the long fiber bundle obtained by the first melt-blowing, the liquid volume of the first spraying is 0 to 180 L / h, and is not 0, and the first chemical additive in the first chemical additive aqueous solution accounts for 0.1 to 10% of the total mass of the composite multi-layer non-woven material; The mixed spraying also includes spraying water or a second chemical additive aqueous solution on the mixed filament bundle formed by the short fiber bundle obtained by the first air-laid web and the long fiber bundle obtained by the second melt-blown, the liquid volume of the second spraying is 0 to 180 L / h, and is not 0, and the percentage of the second chemical additive in the second chemical additive aqueous solution to the total mass of the composite multi-layer non-woven material is 0.1 to 10%; The second air-laid web further comprises spraying the staple fiber bundle obtained by the second air-laid web with a third water or a third chemical auxiliary agent aqueous solution, wherein the liquid volume of the third spray is 0 to 180 L / h and is not 0, and the third chemical auxiliary agent in the third chemical auxiliary agent aqueous solution accounts for 0.1 to 10% of the total mass of the composite multi-layer nonwoven material; The third melt-blowing also includes a fourth spraying of water or a fourth chemical additive aqueous solution to the long fiber filament bundle obtained by the third melt-blowing, the liquid volume of the fourth spraying is 0 to 180 L / h and is not 0, and the fourth chemical additive in the fourth chemical additive aqueous solution accounts for 0.1 to 10% of the total mass of the composite multi-layer non-woven material.
3. The preparation method according to claim 1, characterized in that: The mass of the first raw material in the first web layer accounts for 0.2-20% of the total mass of the composite multi-layer nonwoven material; the first raw material also includes a first functional masterbatch, and the mass of the first functional masterbatch in the first web layer accounts for 0.1-10% of the mass of the first polymer raw material; When the intermediate fiber web layer includes a mixed spray fiber web, the second raw material in the intermediate fiber web layer accounts for 0.2-20% of the total mass of the composite multi-layer nonwoven material; the second raw material also includes a second functional masterbatch, and the mass of the second functional masterbatch in the intermediate fiber web layer accounts for 0.1-10% of the mass of the second polymer raw material; The mass of the third raw material in the second web layer accounts for 0.2-20% of the total mass of the composite multi-layer nonwoven material; the second raw material also includes a third functional masterbatch, and the mass of the third functional masterbatch in the second web layer accounts for 0.1-10% of the mass of the third polymer raw material.
4. The preparation method according to claim 1 or 3, characterized in that: The first polymer raw material, the second polymer raw material and the third polymer raw material independently include degradable or compostable thermoplastic fibers and / or thermoplastic polymer filaments; the degradable or compostable thermoplastic fibers include one or more of polylactic acid, polyhydroxyalkanoate, polycaprolactone, polyesteramide and copolymers thereof, polyvinyl alcohol, polyvinyl alcohol derivatives, cellulose, cellulose derivatives, proteins, starch, starch derivatives, chitosan, chitosan derivatives, hemicellulose and hemicellulose derivatives; the material of the thermoplastic polymer filaments includes one or more of polyolefins, polyesters, polyhydroxyalkanoates and polyhydroxybutyrates; the thermoplastic polymer filaments include single components or double components, and the double components include one or more of sheath-core type, side-by-side type, trilobal type and orange segment type; the melt index of the thermoplastic polymer filaments ranges from 100 to 1500 g / 10 min; The spinning temperatures of the first melt-blowing, the second melt-blowing and the third melt-blowing are independently 200° C. to 290° C.; The diameter of the long fibers obtained by the first meltblowing, the first spunbonding, the second meltblowing, the third meltblowing and the second spunbonding is 5 to 20 μm, and the gram weight is 0.1 to 3.0 gsm.
5. The preparation method according to claim 1, characterized in that: When the intermediate fiber web layer includes a mixed spray fiber web, the mass of the first water-absorbent fibers in the intermediate fiber web layer accounts for 10 to 47.5% of the total mass of the composite multi-layer nonwoven material; When the intermediate fiber web layer comprises an air-laid fiber web, the mass of the second water-absorbent fibers in the intermediate fiber web layer accounts for 10 to 47.5% of the total mass of the composite multi-layer nonwoven material; The first absorbent fiber and the second absorbent fiber independently include wood pulp fiber and / or paper pulp fiber; the wood pulp fiber includes one or more of oak, poplar, birch, pine, spruce and fir; the paper pulp fiber includes one or more of straw pulp, reed pulp, sugarcane pulp, bamboo pulp, cotton pulp, hemp pulp and natural fiber rag pulp; The length of the staple fibers obtained by the first air-laid web and the second air-laid web is 0.5 to 8 mm; The first air-laid web and the second air-laid web are independently distributed and laid by a CD controllable ejector or laid by a forming head uniformly distributed along the width direction, and the forming head is a dust cage type or a flat screen type.
6. The preparation method according to claim 1, characterized in that: The hot rolling setting temperature is 80-200°C, and the speed is 0-1000m / min, and is not 0; The pre-wetting water pressure is 0.1-5 MPa; The water pressure of the flat net type positive spray is 0.5-10MPa; The water pressure of the rotary drum reverse spray and the rotary drum forward spray is independently 1 to 15 MPa; The water pressure of flat mesh jacquard positive spray is 3-20MPa; The drying temperature is 90-130°C.
7. The preparation method according to claim 1, characterized in that: The post-finishing comprises: one or more of spraying, roller coating and padding; The chemical additives used in the post-finishing process include one or more of antibacterial agents, hydrophilic agents, softeners, softeners, strength agents, adhesives, silicones, wetting agents, latex and thermochromic colorant materials; the latex includes acrylic acid and / or ethylene vinyl acetate; the strength agent includes carboxymethyl cellulose and / or starch; the adhesive includes one or more of ethylene vinyl acetate, acrylic acid and other elastic adhesives.
8. The composite multi-layer nonwoven material prepared by the preparation method according to any one of claims 1 to 7, characterized in that: It includes a first layer structure, an intermediate layer structure and a second layer structure which are stacked in sequence; the first layer structure is formed by a plurality of first meltblown fiber webs and / or a plurality of first spunbond fiber webs; the intermediate layer structure is formed by a plurality of mixed-spray fiber webs and / or a plurality of air-laid fiber webs, and the second layer structure is formed by a plurality of second meltblown fiber webs and / or a plurality of second spunbond fiber webs.
9. The device used in the preparation method according to any one of claims 1 to 7, characterized in that: It includes a web-forming curtain, a web-forming device arranged above the web-forming curtain, the web-forming device includes a plurality of first melt-blowing devices and / or a plurality of spunbonding devices, and also includes a plurality of mixed-spray systems and / or a plurality of second grinding devices, the second grinding device includes a second crusher and a second air-flow web-forming device; the mixed-spray system includes a plurality of second melt-blowing devices, a plurality of first grinding devices and a mixed-spray forming box, the first grinding device includes a first crusher and a first air-flow web-forming device; A hot rolling device arranged downstream of the mesh forming curtain, a first mesh transport curtain arranged downstream of the hot rolling device, a pre-wetting device and a first high-pressure water spraying device arranged above the first mesh transport curtain, a first vacuum dehydration device arranged below the first mesh transport curtain, a second high-pressure water spraying device and a third high-pressure water spraying device arranged downstream of the first mesh transport curtain, a second mesh transport curtain arranged downstream of the second and third high-pressure water spraying devices, a jacquard high-pressure water spraying device arranged above the second mesh transport curtain, a second vacuum dehydration device arranged below the second mesh transport curtain, a drying device arranged downstream of the second mesh transport curtain, and a finishing device arranged downstream of the drying device.
10. The device according to claim 9, characterized in that A first spray device is provided below the spinneret of the first melt-blowing device, a second spray device is provided below the discharge port of the mixed spray forming box, and a third spray device is provided below the second air-laid device; The spinnerets of the first melt-blowing device and the second melt-blowing device include a first spinneret, a second spinneret or a third spinneret; The first spinneret is provided with a single row of first spinneret holes, the first spinneret holes are inverted conical holes, the outer cone surface of the first spinneret holes is sleeved with first airflow drafting holes, the first airflow drafting holes are inverted conical holes and are coaxial with the first spinneret holes, the long fibers ejected from the first spinneret holes and the drafting gas ejected from the first airflow drafting holes converge at the apex, and the angle between the drafting gas and the long fibers is 30-70°; The second spinneret is provided with a single row or multiple rows of second spinneret holes, the second spinneret holes are cylindrical holes, the outer circumference of the second spinneret holes is sleeved with second airflow drafting holes, the second airflow drafting holes are annular holes and are coaxial with the second spinneret holes; The third spinneret is provided with a single row or multiple rows of third airflow drafting holes, the third airflow drafting holes are cylindrical holes, the outer peripheral surface of the third airflow drafting holes is sleeved with third spinneret holes, the third spinneret holes are annular holes and are coaxial with the third airflow drafting holes.
Citation Information
Patent Citations
Four-layer composite spunlace non-woven fabric and method for manufacturing same
CN106222887A
Wet spunlace composite material and production method thereof
CN108202515A
Infant wet tissue base fabric and production method thereof
CN111850820A
Method and device for preparing multi-layer composite non-woven fabric
CN116837536A
Cited By
Mixed spraying layer, non-woven composite material preparation device and non-woven composite material
CN119078317A
Hybrid spray layer, nonwoven composite manufacturing apparatus, and nonwoven composite
CN119078317B
Colorful non-woven material and preparation method thereof
CN121556222A