Silicon-based mesoporous carbon / MOF (Metal Organic Framework) derived carbon / carbon nanotube composite electrode material for capacitive deionization as well as preparation and application of silicon-based mesoporous carbon / MOF derived carbon / carbon nanotube composite electrode material
The preparation of silicon-based mesoporous carbon/MOF-derived carbon/carbon nanotube composite electrode materials solves the ion blocking problem caused by the microporous structure of MOF materials, improves the adsorption performance and conductivity of the electrode, and achieves more efficient capacitance removal. Ion desalination effect.
Patent Information
- Application Number
- CN202410722333.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-05
AI Technical Summary
In the process of capacitive deionization seawater desalination, existing MOF materials are prone to clogging of ions due to their microporous structure, which reduces the effective pore size and adsorption efficiency. The electrode surface has insufficient wetting properties, which affects the adsorption, desorption and transmission of ions.
Using silicon-based mesoporous carbon/MOF-derived carbon/carbon nanotube composite electrode material, SBA-15 mesoporous carbon precursor was prepared through P123 and ethyl orthosilicate under acidic conditions, and combined with carbon nanotubes and hexahydrate zinc nitrate in the absence of Stir in water and methanol to form a silicon-based mesoporous carbon/MOF-derived carbon/carbon nanotube composite material. After step-wise calcination and nitric acid oxidation etching, a uniformly dispersed structure is formed to increase the pore size and specific surface area.
Significantly improves the ion adsorption active sites and hydrophilicity of the electrode material, increases the contact area between the solution and the electrode, avoids the agglomeration of carbon nanotubes, forms a three-dimensional structure, improves the conductivity of the electrode and the transmission channel of salt ions, Improved the adsorption performance of capacitive deionization.
Smart Images

Figure CN118723979A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of capacitive deionization and desalination, and in particular relates to a silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite electrode material for capacitive deionization and a preparation and application thereof. Background Art
[0002] In today's society where water resources are extremely scarce, metal-organic frameworks and their derivatives (MOFs) have been widely studied and applied to capacitive deionization (CDI) desalination technology, mainly due to their high specific surface area and ability to control pore size structure. However, the pore size of most MOF materials is microporous, which leads to the problem that ions are very easy to block the pores during the CDI adsorption process, resulting in a reduction in the effective pore size, a decrease in the adsorption efficiency after repeated use of the electrode, and the inability to regenerate the electrode. In response to this application defect of MOF materials, scientists have explored a variety of methods to improve this situation, among which increasing the sintering temperature and performing acid treatment is one method. A Chinese patent document (application number 201710504003.2) discloses a MOF structure porous carbon material, the preparation method of which includes: compounding a metal organic framework material on the surface of a carbon nanotube to form a carbonized precursor; heating the carbonized precursor to 700-1000°C in a protective atmosphere to obtain the MOF structure porous carbon material. The prepared material has the following defects: the wettability of the obtained electrode surface is insufficient, the contact area between the electrode and the solution to be adsorbed is small, which is not conducive to the adsorption and desorption of ions; the specific surface area of the composite electrode material is too small and the surface pore size is too large, which is not conducive to the transmission and storage of ions, resulting in poor adsorption performance of the electrode material. Summary of the invention
[0003] Research has found that Zn-MOF has too many microporous structures and a small average pore size, which will cause salt ions to block the pores during the adsorption process, resulting in a reduction in the effective pore size. To overcome this technical problem, the present invention provides a silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite electrode material for capacitive deionization and its preparation and application.
[0004] To achieve the purpose of the present invention, the technical solution adopted is: a method for preparing a silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite electrode material for capacitive deionization, characterized in that:
[0005] The method comprises the following steps: (1) preparing SBA-15 mesoporous carbon precursor by hydrothermal reaction of P123 and tetraethyl orthosilicate under acidic conditions;
[0006] (2) adding the SBA-15 mesoporous carbon precursor, carbon nanotubes and zinc nitrate hexahydrate in step (1) to anhydrous methanol in a certain mass ratio, stirring evenly and allowing sufficient adsorption to obtain solution A; adding a required amount of dimethylimidazole to anhydrous methanol to obtain solution B;
[0007] (3) adding the solution B in step (2) to the solution A, stirring until fully reacted, and then filtering to obtain a silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite material precursor;
[0008] (4) calcining the silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite material precursor in step (3) under inert atmosphere to obtain derived carbon, then oxidizing and etching the derived carbon with nitric acid, and vacuum drying to obtain a silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite electrode material;
[0009] The mass ratio of zinc in SBA-15 mesoporous carbon precursor, carbon nanotubes, and zinc nitrate is calculated to be 0.2-0.6: 0.15-0.3: 1.85-1.95;
[0010] In step (4), the high temperature calcination adopts a step-by-step calcination method, firstly raising the temperature to 500-550°C at a rate of 2-4°C / min, and calcining at this temperature for 4-5h; then continuing to raise the temperature to 950-1000°C at a rate of 5-8°C / min, and calcining at this temperature for 2-3h; the nitric acid concentration is 4-8M, the etching temperature is 90-100°C, and the reaction time is 4-6h.
[0011] The structure of the silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite electrode material for capacitive deionization prepared by the above method includes SBA mesoporous carbon, Zn-MOF-derived carbon attached to the SBA mesoporous carbon, and carbon nanotubes uniformly interspersed and connected in the gaps between the SBA mesoporous carbon and the Zn-MOF-derived carbon. The structure is formed by: uniformly dispersed SBA-15 mesoporous carbon precursor and carbon nanotubes in situ composite organic metal framework Zn-MOF, and then calcined and carbonized under the protection of an inert atmosphere;
[0012] The average pore size of the electrode material is 7.5-10 nm, and the specific surface area is ≥500 m 2 / g, pore volume 0.3~6cm 3 / g, equivalent series resistance ≤0.7Ω, water contact angle does not exceed 102°.
[0013] Furthermore, in step (2), the mass ratio of zinc to dimethylimidazole in zinc nitrate is 1:7.8-8.5.
[0014] Furthermore, in step (2), the stirring time is 6 to 8 hours;
[0015] Furthermore, in step (4), the high temperature calcination adopts a stepwise calcination method, which is divided into two stages of calcination process, wherein the calcination temperature of the first stage is 550°C, the heating rate is 2°C / min, and the calcination time is 4h; the calcination temperature of the second stage is 950°C, the heating rate is 5°C / min, and the calcination time is 2h;
[0016] An application of the silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite electrode material for capacitive deionization prepared by the above method includes the following steps: the silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite electrode material can be prepared into a CDI electrode by a general method.
[0017] For example, silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite-derived carbon, acetylene black and polytetrafluoroethylene emulsion (60wt%) (PTFE) are mixed in a mass ratio of 8:1:1, anhydrous ethanol is added dropwise until it becomes viscous, and after high-temperature mixing, a roller press is used to press it into a carbon film to obtain a CDI electrode.
[0018] Compared with the prior art, the present invention achieves the following beneficial effects:
[0019] 1) The present invention prepares silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite electrode materials by an in-situ growth method, which is simple and low-cost. After high-temperature carbonization, nitric acid is used for oxidation etching to effectively improve the pore structure, increase the ion adsorption active sites, and introduce oxygen-containing functional groups to improve the hydrophilicity of the carbon material (the water contact angle of the composite electrode material does not exceed 102°), increase the contact area between the solution and the electrode, and improve the adsorption effect of the electrode on salt ions.
[0020] 2) The silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite electrode material of the present invention adds an appropriate amount of carbon nanotubes, so that the carbon nanotubes are interspersed and connected between and inside the MOF crystals and the mesoporous carbon to form a three-dimensional structure, which can avoid the agglomeration of the carbon nanotubes, thereby improving the conductivity of the derived carbon material, facilitating the rapid transmission of ions, and having a good effect in capacitive deionization and desalination applications.
[0021] 3) The silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite electrode material of the present invention is prepared by introducing SBA-15 silicon-based mesoporous carbon with rich mesopore volume to prepare a precursor, and PCNT / SBA-derived carbon is prepared by a step-by-step temperature sintering process, so as to further improve the pore structure of the electrode material, realize more ion transmission channels and storage active sites, thereby further improving the adsorption performance of the MOF-based composite material in salt solution. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 is a scanning electron microscope image of the PCNT0.03 derived carbon in Example 1;
[0023] Figure 2 is a scanning electron microscope image of the PCNT / SBA0.02 derived carbon in Example 2;
[0024] Figure 3 is a scanning electron microscope image of the PCNT / SBA0.04 derived carbon in Example 3;
[0025] Figure 4 is a scanning electron microscope image of the PCNT / SBA0.06 derived carbon in Example 4;
[0026] Figure 5 is a transmission electron micrograph of the PCNT / SBA0.04 derived carbon in Example 3;
[0027] Figure 6 The XPS graphs of the PCNT, PCNT / SBA0.06, PCNT / SBA0.04 and PCNT / SBA0.02 derived carbon electrode materials and the fine spectrum of the PCNT / SBA0.04 derived carbon electrode material in Examples 1 to 4;
[0028] Figure 7 The XRD spectra of ZIF-8 / CNT0.03, ZCNT / SBA0.02, ZCNY / SBA0.04 and ZCNT / SBA0.06 precursors in Examples 1 to 4, and the XRD spectra of PCNT0.03, PCNT / SBA0.02, PCNT / SBA0.04 and PCNT / SBA0.06 derived carbon electrode materials;
[0029] Figure 8 The nitrogen adsorption-desorption isotherms and pore size distribution diagrams of the PCNT0.03, PCNT / SBA0.02, PCNT / SBA0.04 and PCNT / SBA0.06 derived carbon electrode materials in Examples 1 to 4;
[0030] Fig. 9 It is the Raman spectra of the PCNT0.03, PCNT / SBA0.02, PCNT / SBA0.04 and PCNT / SBA0.06 derived carbon electrode materials in Examples 1 to 4;
[0031] Fig.10 It is the water contact angle diagram of the PCNT0.03, PCNT / SBA0.02, PCNT / SBA0.04 and PCNT / SBA0.06 derived carbon electrode materials in Examples 1 to 4;
[0032] Fig.11It is a constant current charge-discharge diagram of the PCNT0.03, PCNT / SBA0.02, PCNT / SBA0.04 and PCNT / SBA0.06 derived carbon electrode materials in Examples 1 to 4 at a current density of 1 A / g, a voltage range of -1 to -0.2 V, and an electrolyte of 6 M KOH;
[0033] Fig.12 are AC impedance diagrams of PCNT0.03, PCNT / SBA0.02, PCNT / SBA0.04 and PCNT / SBA0.06 derived carbon electrode materials in Examples 1 to 4;
[0034] Fig.13 The CDI curves, electrosorption kinetic curves and Kim-Yoon curves of the PCNT0.03, PCNT / SBA0.02, PCNT / SBA0.04 and PCNT / SBA0.06 derived carbon electrode materials in Examples 1 to 4 at a working voltage of 1.2 V;
[0035] Fig.14 (a) CDI curve, (b) electrosorption kinetic curve, and (c) Kim-Yoon curve of the PCNT / SBA0.04 derived carbon electrode material at different voltages in Example 4; (d) electrosorption kinetic curve and (e) Kim-Yoon curve of the PCNT / SBA0.04 derived carbon electrode in NaCl solutions of different concentrations; adsorption-desorption cycle diagram of the PCNT / SBA0.04 derived carbon electrode at an operating voltage of 1.2 V and a 500 mg / L NaCl solution. DETAILED DESCRIPTION
[0036] In order to further understand the purpose, content and advantages of the present invention, the specific embodiments of the present invention are now described in detail as follows, but it is not limited to the following examples, and it is freely matched according to actual conditions. The endpoints and any values of the scope disclosed in this article are not limited to the precise scope and value. For numerical ranges, between the endpoint values of each scope, between the endpoint values of each scope and a separate point value, and between separate point values, one or more new numerical ranges can be combined with each other, and these numerical ranges should be considered as specifically disclosed in this article.
[0037] The present invention provides a preparation example of a dual MOF-derived porous carbon / nitrogen-sulfur co-doped graphene composite electrode material for capacitive deionization, comprising the following steps:
[0038] (1) SBA-15 mesoporous carbon precursor was prepared by hydrothermal reaction of P123 and tetraethyl orthosilicate under acidic conditions;
[0039] (2) adding the SBA-15 mesoporous carbon precursor, carbon nanotubes and zinc nitrate hexahydrate in step (1) to anhydrous methanol in a certain mass ratio, stirring evenly and allowing sufficient adsorption to obtain solution A; adding a required amount of dimethylimidazole to anhydrous methanol to obtain solution B;
[0040] (3) adding the solution B in step (2) to the solution A, stirring until fully reacted, and then filtering to obtain a silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite material precursor;
[0041] (4) calcining the silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite material precursor in step (3) under inert atmosphere to obtain derived carbon, then oxidizing and etching the derived carbon with nitric acid, and vacuum drying to obtain a silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite electrode material;
[0042] The mass ratio of zinc in SBA-15 mesoporous carbon precursor, carbon nanotubes, and zinc nitrate is calculated to be 0.2-0.6: 0.15-0.3: 1.85-1.95;
[0043] In step (4), the high temperature calcination adopts a step-by-step calcination method, firstly raising the temperature to 500-550°C at a rate of 2-4°C / min, and calcining at this temperature for 4-5h; then continuing to raise the temperature to 950-1000°C at a rate of 5-8°C / min, and calcining at this temperature for 2-3h; the nitric acid concentration is 4-8M, the etching temperature is 90-100°C, and the reaction time is 4-6h.
[0044] The structure of the silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite electrode material for capacitive deionization prepared by the above method includes SBA mesoporous carbon, Zn-MOF-derived carbon attached to the SBA mesoporous carbon, and carbon nanotubes uniformly interspersed and connected in the gaps between the SBA mesoporous carbon and the Zn-MOF-derived carbon. The average pore size of the obtained composite electrode material is 7.5-10nm, and the specific surface area is ≥500m 2 / g, pore volume 0.3~6cm 3 / g, equivalent series resistance ≤0.7Ω, water contact angle does not exceed 102°.
[0045] In a preferred embodiment, in order to efficiently obtain the SBA-15 mesoporous carbon precursor, a specific method for preparing the SBA-15 mesoporous carbon precursor is given, including: adding hydrochloric acid to the P123 aqueous solution, adding tetraethyl orthosilicate dropwise under heating conditions (the purpose of heating is to facilitate mixing, not exceeding the reaction temperature, preferably 40°C to 50°C), magnetically stirring for 4 to 6 hours, adding to an autoclave, hydrothermally reacting at 100 to 110°C for 10 to 12 hours, and then washing and drying to obtain the SBA-15 mesoporous carbon precursor.
[0046] In a more specific embodiment, the mass ratio of P123, ethyl orthosilicate, deionized water and concentrated hydrochloric acid is 1:1.96:26.25:4, and the mass concentration of concentrated hydrochloric acid is 36-38%.
[0047] In a preferred embodiment, the mass ratio of the SBA-15 mesoporous carbon precursor, carbon nanotubes, and zinc in the zinc nitrate in step (2) is calculated to be 0.3-0.5: 0.18-0.25: 1.85-1.95. Through this optimization, the specific surface area and pore size can be further optimized, while increasing the nitrogen content and reducing the equivalent series resistance value, providing the necessary conditions for further increasing the salt adsorption content of the electrode material.
[0048] The amount of dimethylimidazole used is generally aimed at consuming all zinc ions as much as possible to form an organic framework. From an economic point of view, in the above embodiment, the mass ratio of zinc to dimethylimidazole in zinc nitrate is 1:1.8-2.0.
[0049] The present invention is further described in detail below in conjunction with embodiments:
[0050] Embodiment 1:
[0051] Step 1: Weigh 200 mg of carbon nanotubes and 8.8 g of zinc nitrate hexahydrate, add them to 200 mL of methanol solution and stir for 30 min to obtain solution A. Add 15.4 g of dimethylimidazole to 200 mL of methanol to obtain solution B.
[0052] Step 2: quickly add the B solution in step 1 to the A solution, stir for 6 hours and then stand for 12 hours, collect the product by suction filtration, and vacuum dry it at 60° C. for 12 hours (drying reduces the humidity before calcination, reduces the risk of cracking the crucible and clogging the furnace ventilation pipe, and the vacuum drying temperature is generally 60-80° C. and the time is 12-15 hours) to obtain a ZnMOF / carbon nanotube precursor, denoted as ZCNT;
[0053] Step 3: The ZnMOF / carbon nanotube precursor obtained in step 2 was calcined at 950°C for 2h under argon protection with a heating rate of 5°C / min. The carbonized product was washed with 2M hydrochloric acid, filtered and washed to neutrality and dried. The obtained product was oxidized and etched by 6M nitric acid at 90°C for 4h, washed to neutrality, and dried in vacuum to obtain a Zn-MOF-derived carbon / carbon nanotube composite electrode material. According to the proportion of carbon nanotubes in the total mass (3%), the electrode material was recorded as PCNT0.03.
[0054] Through FE-SEM test, we can see that Figure 1PCNT0.03 derived carbon presents a polyhedral structure with a particle size of 100nm. It can be observed that carbon nanotubes are interspersed and connected between crystal particles with a relatively uniform distribution. In XPS analysis, PCNT0.03 derived carbon has three characteristic peaks of C1s, N1s and O1s at 284.8eV, 399.7eV and 531.8eV binding energies, and the peaks are relatively obvious. The nitrogen content is 18.9% and the oxygen content is 5.6%. In Raman test, the I of PCNT0.03 derived carbon is 1.34mm, 1.32mm and 1.6mm respectively. D / I G The value is 1.10, indicating a high degree of graphitization. In the nitrogen adsorption-desorption (BET) analysis, the nitrogen adsorption-desorption curve of the electrode material is a type IV curve. The pore size distribution diagram further confirms that the specific surface area of the derived carbon electrode material is 575.04 m 2 / g, pore volume 0.35cm 2 / g, the average pore size is 5.58nm. Further study on its electrochemical performance: The preparation method of the electrochemical working electrode is to ultrasonically disperse the electrode active material, conductive carbon black and polytetrafluoroethylene (binder) in an ultrasonic machine in a mass ratio of 8:1:1, and evenly coat the paste on graphite paper when the final form is a paste. The above sample is placed in a vacuum oven at 60°C for 6 hours and cooled to room temperature to obtain a test electrode. In the constant current charge and discharge (GCD) test, the current density is 1A / g, the voltage window is -1~-0.2V, the electrolyte is 6M KOH, the charge and discharge curve is symmetrically triangular, and the tested specific capacitance is 195.5F / g; in the alternating current impedance test (EIS) of the electrode material, the equivalent series resistance (Rs) value of the derived carbon electrode material is 0.726Ω; in the desalination performance test, the preparation method of the CDI electrode is: the electrode material, acetylene black and polytetrafluoroethylene emulsion (60wt%) (PTFE) are mixed according to a mass ratio of 8:1:1, anhydrous ethanol is added dropwise until it becomes viscous, and after high temperature mixing, a roller press is used to press it into a carbon film to obtain a CDI electrode. In the desalination performance test, the voltage applied to both ends of the electrode is 1.2V, the electrolyte is a 50ml volume, 500mg / L NaCl aqueous solution, and the electrical adsorption capacity of the derived carbon electrode material is 9.18mg / g.
[0055] Based on Example 1, only the amount of carbon nanotubes was adjusted to 100 mg, and the electrode material was recorded as PCNT0.02. Through FE-SEM testing, it can be observed that a small amount of CNT is compounded between Zn-MOF particles, and the PCNT0.02-derived carbon particles still maintain the same size as Zn-MOF;
[0056] The nitrogen content of PCNT0.02 derived carbon is 15.4%, which comes from the doping effect of organic ligands during high temperature cracking and the appropriate addition of carbon nanotubes. In the Raman test, the I D / I G The value is 1.08, and the degree of graphitization has decreased. In the nitrogen adsorption-desorption (BET) analysis, the nitrogen adsorption-desorption curve of the derived carbon electrode material is a type IV curve. The pore size distribution diagram further confirms that the specific surface area of the electrode material is 507.47 m 2 / g, pore volume 0.33cm 3 / g, the average pore size is 4.65nm. Further study of its electrochemical performance: in the constant current charge and discharge (GCD) test, the current density is 1A / g, the voltage window is -1~-0.2V, the electrolyte is 6M KOH, the charge and discharge curve is a symmetrical triangle shape, and the tested specific capacitance is 135.9F / g; in the alternating current impedance test (EIS) of the electrode material, the equivalent series resistance (Rs) value of the derived carbon electrode material is 0.734Ω; in the desalination performance test, the voltage applied across the electrode is 1.2V, the electrolyte is a 50ml, 500mg / L NaCl aqueous solution, and the electrical adsorption capacity of the derived carbon electrode material is 7.82mg / g.
[0057] Based on Example 1, only the amount of carbon nanotubes was adjusted to 300 mg, and the electrode material was recorded as PCNT0.04. Through FE-SEM testing, it can be observed that the morphology and structure of the PCNT0.04-derived carbon become disordered, and a large number of agglomerations occur; the nitrogen content of the PCNT0.02-derived carbon is 13.9%; in the Raman test, the I D / I G The value is 1.09, and the degree of graphitization has decreased. In the nitrogen adsorption-desorption (BET) analysis, the nitrogen adsorption-desorption curve of the electrode material is a type IV curve. The pore size distribution diagram further confirms that the specific surface area of the electrode material is 505.85 m 2 / g, pore volume 0.34cm 3 / g, the average pore size is 3.80nm. Further study of its electrochemical performance: in the constant current charge and discharge (GCD) test, the current density is 1A / g, the voltage window is -1~-0.2V, the electrolyte is 6M KOH, the charge and discharge curve is a symmetrical triangle shape, and the tested specific capacitance is 160.5F / g; in the alternating current impedance test (EIS) of the electrode material, the equivalent series resistance (Rs) value of the derived carbon electrode material is 0.728Ω; in the desalination performance test, the voltage applied across the electrode is 1.2V, the electrolyte is a 50ml, 500mg / L NaCl aqueous solution, and the electrical adsorption capacity of the derived carbon electrode material is 8.40mg / g.
[0058] Example 2
[0059] Step 1: Dissolve 4 g of P123 in 105 mL of deionized water and stir for 5 h to obtain solution A. Then weigh 20 mL of concentrated HCl (mass concentration of 36-38%) and add it to A to obtain solution B;
[0060] Step 2: Place solution B in step 1 in an oil bath at 40°C, add 9.1 mL of tetraethyl orthosilicate dropwise, react for 4 h with magnetic stirring, place in a hydrothermal kettle, react at 100°C for 24 h, filter and wash, place in a vacuum oven at 60°C and dry for 12 h to obtain a silicon-based mesoporous carbon precursor (denoted as SBA);
[0061] Step 3: Add 200 mg of the silicon-based mesoporous carbon precursor, 200 mg of carbon nanotubes and 8.8 g of zinc nitrate hexahydrate in step 2 to 200 mL of methanol and stir for 6 h to obtain solution C. Add 15.4 g of dimethylimidazole to 200 mL of methanol to obtain solution D;
[0062] Step 4: quickly add solution D in step 3 to solution C, stir for 12 hours and then stand, collect the product by suction filtration, and vacuum dry at 60° C. for 12 hours (drying reduces the humidity before calcination, reduces the risk of cracking the crucible and clogging the furnace ventilation pipe, and the vacuum drying temperature is generally 60-80° C. and the time is 12-15 hours) to obtain a silicon-based mesoporous carbon / Zn-MOF / carbon nanotube composite precursor, recorded as ZCNT / SBA0.02;
[0063] Step 5. The silicon-based mesoporous carbon / Zn-MOF / carbon nanotube composite precursor obtained in step 4 is first calcined at 550°C for 4 hours under argon protection, with a heating rate of 2°C / min; then the temperature is continued to be raised to 950°C for calcination for 2 hours, with a heating rate of 3°C / min. The carbonized product is washed with 2M hydrochloric acid, filtered, washed to neutrality and dried. The obtained product is oxidized and etched by 6M nitric acid at 90°C for 4 hours, washed to neutrality, and vacuum dried to obtain a silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite electrode material, recorded as PCNT / SBA0.02.
[0064] Through FE-SEM test, we can see that Figure 2, PCNT / SBA0.02 derived carbon presents a polyhedral structure, a large number of MOF derived carbon particles are attached to the surface of SBA mesoporous carbon, forming a core-shell structure, in the gap between the crystal and the mesoporous carbon, there are a large number of carbon nanotubes connected and interlaced; in the XPS spectrum, PCNT0.03 and PCNT / SBA0.02 derived carbon are found at 284.8eV, 399.7eV and 531.8eV binding energy of three characteristic peaks of C1s, N1s and O1s, and the peak shape is more obvious, which shows that the introduction of mesoporous carbon does not have a significant effect on Zn-MOF crystals, wherein the nitrogen content is 17.7%, and the oxygen content is 10.0%; in the XRD diagram, the main diffraction peak of the precursor is consistent with the diffraction peak position of the Zn-MOF precursor, which also shows that the addition of SBA mesoporous carbon does not cause too much change in the crystal surface of the precursor; in the Raman test, the I of PCNT / SBA0.02 D / I G The value is 1.07, indicating a high degree of graphitization. In the nitrogen adsorption-desorption (BET) analysis, the nitrogen adsorption-desorption curve of the electrode material is a type IV curve. The pore size distribution diagram further confirms that the specific surface area of the electrode material is 523.02 m 2 / g, pore volume 0.34cm 2 / g, the average pore size is 7.64nm. Further study of its electrochemical performance: in the constant current charge and discharge (GCD) test, the current density is 1A / g, the voltage window is -1~-0.2V, the electrolyte is 6M KOH, the charge and discharge curve is a symmetrical triangle shape, and the tested specific capacitance is 210.0F / g; in the alternating current impedance test (EIS) of the electrode material, the equivalent series resistance (Rs) value of the electrode material is 0.678Ω; in the desalination performance test, the voltage applied across the electrode is 1.2V, the electrolyte is a 50ml, 500mg / L NaCl aqueous solution, and the electrical adsorption capacity of the electrode material is 9.54mg / g.
[0065] Example 3
[0066] The main difference compared with Example 2 is that the amount of silicon-based mesoporous carbon (SBA) added in step three is 400 mg, and the remaining steps are the same as Example 2.
[0067] The product of this example is a silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite electrode material, which is denoted as PCNT / SBA0.04.
[0068] Through FE-SEM test, we can see that Figure 3Due to the increase of SBA content, the attachment of Zn-MOF crystals on the surface of mesoporous carbon becomes dispersed and no longer aggregates, which exposes more pores inside the mesoporous carbon, and carbon nanotubes are more evenly interspersed in the Zn-MOF crystals and mesoporous carbon, while connecting the gaps between the two; in the XPS spectrum, through the O1s fine spectrum of PCNT / SBA0.04, it can be found that the three characteristic peaks that appear correspond to three different forms of C=O, CO and OC=O, respectively. The appearance of these peaks indicates that oxygen-containing functional groups are successfully introduced into the surface of the material, which is beneficial to increase the hydrophilicity of the electrode surface. The nitrogen content is 14.9% and the oxygen content is 12.4%; in the XRD diagram, the main diffraction peaks of the precursor are consistent with the diffraction peaks of the ZIF-8 precursor, which also shows that the addition of SBA mesoporous carbon does not cause much change in the crystal surface of the precursor; in the Raman test, the I D / I G The value is 1.12, indicating a high degree of graphitization. In the nitrogen adsorption-desorption (BET) analysis, the nitrogen adsorption-desorption curve of the electrode material is a type IV curve. The pore size distribution diagram further confirms that the specific surface area of the electrode material is 590.06 m 2 / g, pore volume 0.36cm 2 / g, the average pore size is 8.77nm. Further study of its electrochemical performance: in the constant current charge and discharge (GCD) test, the current density is 0.5A / g, the voltage window is -1~-0.2V, the electrolyte is 6M KOH, the charge and discharge curve is a symmetrical triangle shape, and the tested specific capacitance is 235.0F / g; in the alternating current impedance test (EIS) of the electrode material, the equivalent series resistance (Rs) value of the electrode material is 0.654Ω; in the desalination performance test, the voltage applied across the electrode is 1.2V, the electrolyte is a 50ml, 500mg / L NaCl aqueous solution, and the electrical adsorption capacity of the electrode material is 10.25mg / g.
[0069] Example 4
[0070] The main difference compared with Example 2 is that the amount of silicon-based mesoporous carbon (SBA) added in step 3 is 600 mg, and the remaining steps are the same as Example 3.
[0071] The product of this example is a silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite electrode material, denoted as PCNT / SBA0.06.
[0072] Through FE-SEM test, we can see that Figure 4, when the SBA content increased to 0.6g, the number of Zn-MOF crystals on the surface of PCNT / SBA0.06 derived carbon decreased significantly, and the number of carbon nanotubes interlaced and linked inside the derived carbon also decreased significantly; in the XPS spectrum, when the SAB mesoporous carbon content increased to 0.6g, the nitrogen and oxygen contents of the PCNT / SBA0.06 derived carbon increased, the carbon content decreased to 67%, the nitrogen content was 15.1%, and the oxygen content was 17.8%; in the XRD diagram, the main diffraction peaks of the precursor were consistent with the diffraction peaks of the ZIF-8 precursor, which also shows that the addition of SBA mesoporous carbon did not cause much change in the crystal surface of the precursor; in the Raman test, the I D / I G The value is 1.08, indicating a high degree of graphitization. In the nitrogen adsorption-desorption (BET) analysis, the nitrogen adsorption-desorption curve of the electrode material is a type IV curve. The pore size distribution diagram further confirms that the specific surface area of the electrode material is 543.22 m 2 / g, pore volume 0.57cm 3 / g, the average pore size is 7.54nm. Further study of its electrochemical performance: in the constant current charge and discharge (GCD) test, the current density is 0.5A / g, the voltage window is -1~-0.2V, the electrolyte is 6M KOH, the charge and discharge curve is a symmetrical triangle shape, and the tested specific capacitance is 161.8F / g; in the alternating current impedance test (EIS) of the electrode material, the equivalent series resistance (Rs) value of the electrode material is 0.668Ω; in the desalination performance test, the voltage applied across the electrode is 1.2V, the electrolyte is a 50ml, 500mg / L NaCl aqueous solution, and the electrical adsorption capacity of the electrode material is 9.85mg / g.
[0073] The above description is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can use the technical solution and its concept of the present invention to replace or change them with equivalents within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
[0074] Table 1 Test results of the embodiment
[0075]
[0076] The present invention mixes silicon-based mesoporous carbon with a high specific surface and average pore size and a Zn MOF / carbon nanotube composite material with good hydrophilicity, and uses a step-by-step temperature sintering process to prepare PCNT / SBA derived carbon. The introduction of an appropriate amount of SBA mesoporous carbon does not affect the arrangement structure of Zn-MOF crystals and carbon nanotubes, but on the contrary effectively increases the average pore size of the derived carbon. The carbon nanotubes also intersperse between MOF crystals and between MOF and mesoporous carbon, playing a linking role, so that the carbon electrode material presents a three-dimensional structure. After step-by-step high-temperature pyrolysis and acid etching, more oxygen-containing groups are introduced while effectively expanding the pore size, improving the wettability of the electrode surface, and providing conditions for improving the electrical adsorption capacity and desalination efficiency of the electrode material.
Claims
1. A method for preparing a silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite electrode material for capacitive deionization, characterized in that: The following steps are involved: (1) SBA-15 mesoporous carbon precursor was prepared by hydrothermal reaction of P123 and tetraethyl orthosilicate under acidic conditions; (2) adding the SBA-15 mesoporous carbon precursor, carbon nanotubes and zinc nitrate hexahydrate in step (1) to anhydrous methanol in a certain mass ratio, stirring evenly and allowing sufficient adsorption to obtain solution A; adding a required amount of dimethylimidazole to anhydrous methanol to obtain solution B; (3) adding the solution B in step (2) to the solution A, stirring until fully reacted, and then filtering to obtain a silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite material precursor; (4) calcining the silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite material precursor in step (3) under inert atmosphere to obtain derived carbon, then oxidizing and etching the derived carbon with nitric acid, and vacuum drying to obtain a silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite electrode material; The mass ratio of zinc in SBA-15 mesoporous carbon precursor, carbon nanotubes, and zinc nitrate is calculated to be 0.2-0.6: 0.15-0.3: 1.85-1.95; In step (4), the high temperature calcination adopts a step-by-step calcination method, firstly raising the temperature to 500-550°C at a rate of 2-4°C / min, and calcining at this temperature for 4-5h; then continuing to raise the temperature to 950-1000°C at a rate of 5-8°C / min, and calcining at this temperature for 2-3h; the nitric acid concentration is 4-8M, the etching temperature is 90-100°C, and the reaction time is 4-6h.
2. The method for preparing the silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite electrode material for capacitive deionization according to claim 1, characterized in that: The specific steps of step (1) include adding hydrochloric acid to the P123 aqueous solution, adding tetraethyl orthosilicate dropwise under heating conditions, magnetically stirring for 4 to 6 hours, adding to an autoclave, hydrothermally reacting at 100 to 110° C. for 10 to 12 hours, and then washing and drying to obtain an SBA-15 mesoporous carbon precursor.
3. The method for preparing the silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite electrode material for capacitive deionization according to claim 1, characterized in that: In step (2), the mass ratio of SBA-15 mesoporous carbon precursor, carbon nanotubes, and zinc in zinc nitrate is calculated to be 0.3-0.5: 0.18-0.25: 1.85-1.
95.
4. The method for preparing the silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite electrode material for capacitive deionization according to claim 1, characterized in that: In step (2), the stirring time of solution A is 6 to 8 hours.
5. The method for preparing the silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite electrode material for capacitive deionization according to claim 1, characterized in that: The stirring time in step (3) is 10 to 12 hours.
6. A composite electrode material, characterized in that: It is prepared according to the method for preparing a silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite electrode material for capacitive deionization according to any one of claims 1 to 5.
7. Use of the composite electrode material according to claim 6 in capacitive deionization and desalination, characterized in that: The invention comprises preparing a CDI electrode from a silicon-based mesoporous carbon / MOF-derived carbon / carbon nanotube composite electrode material.
Citation Information
Patent Citations
Preparation and application of carbon nanotube / MOF derivative porous carbon composite electrode material
CN109354137A
Preparation method of carbon micron cage encapsulated carbon nanotube wave-absorbing material
CN114835106A