Process for producing aluminum hydroxide by taking aluminum ash disposal slag as raw material

By designing a process using aluminum ash disposal slag as raw material, using the mixing and high-temperature calcination of sodium carbonate and high-aluminum materials, combined with steps such as multi-stage heat exchange and carbon decomposition, we have solved the problem that aluminum elements in high-aluminum materials cannot directly produce aluminum hydroxide. solve the problem, achieve efficient recycling and optimal utilization of resources, and reduce production costs and alkali consumption.

CN118724034APending Publication Date: 2024-10-01SICHUAN TCL HAINENG ENVIRONMENTAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410790553.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The aluminum element in high-aluminum materials mainly exists in the form of inert a-alumina, and aluminum hydroxide cannot be produced through direct alkali dissolution, resulting in insufficient resource value.

Method used

A process for producing aluminum hydroxide using aluminum ash treatment slag as raw material is designed, including mixing dry high-aluminum materials with sodium carbonate, low-nitrogen combustion and calcination, multi-stage heat exchange, dissolution reaction, fine filtration, carbon decomposition, and filtration and washing. and evaporation crystallization and other steps to form an efficient carbon-alkali cycle process, reducing production consumption and alkali consumption.

Benefits of technology

It achieves efficient recovery of aluminum in high-aluminum materials, with an alumina dissolution rate of more than 90%, reducing production costs, converting slag materials into harmless building materials, and improving the purity and whiteness of aluminum hydroxide.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724034A_ABST
    Figure CN118724034A_ABST
Patent Text Reader

Abstract

The invention relates to a process for producing aluminum hydroxide by using aluminum ash disposal slag as a raw material, which comprises the following steps: S1, material preparation: uniformly mixing a dry high-aluminum material produced by aluminum ash production with sodium carbonate according to a mass ratio of 0.6-1.1; the high-aluminum material and sodium carbonate which are evenly mixed according to the proportion are subjected to high-temperature calcination, the material calcination temperature ranges from 1100 DEG C to 1150 DEG C, the phase is converted into regenerated aluminum oxide clinker, and a low-nitrogen combustor is adopted for calcination. And three procedures of raw material pre-homogenization stockpiling, ore grinding and high-pressure dissolution in normal aluminum oxide production are not needed, so that the production consumption is greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of chemical industry, in particular to a process for producing aluminum hydroxide using aluminum ash disposal slag as raw material. Background Art

[0002] Guangyuan's aluminum industry is one of the five characteristic industries identified by the Sichuan Provincial Party Committee and the Provincial Government. A large amount of aluminum ash slag is generated during the production process of electrolytic aluminum, recycled aluminum, aluminum processing and casting.

[0003] According to statistics, about 30-50kg of aluminum ash slag is discharged for every ton of aluminum produced and cast. There are many ash-producing enterprises in Guangyuan City. According to the plan, by 2030, the aluminum enterprises in Guangyuan Economic and Technological Development Zone alone will produce more than 100,000 tons of aluminum ash slag annually.

[0004] According to the aluminum content, aluminum ash can be divided into primary aluminum ash and secondary aluminum ash. Whether it is primary ash or secondary ash, its main components include metallic aluminum, aluminum oxide, aluminum nitride, aluminum carbide and a certain amount of sodium chloride, potassium chloride, fluoride and other salts and other small amounts of impurities such as iron, silicon, magnesium, titanium. The metallic aluminum content of secondary aluminum ash is lower than that of primary aluminum ash.

[0005] Aluminum ash and aluminum nitride react with water to produce ammonia, which pollutes the atmosphere. Fluoride salts and chloride salts dissolve in water and pollute natural water bodies and enter groundwater. Due to their obvious toxicity (I) and reactivity (R), direct discharge will cause irreversible pollution to the natural environment. The "National List of Hazardous Wastes" (2021 edition) includes aluminum ash, slag, and dust produced by electrolytic aluminum and recycled aluminum in the list of hazardous wastes.

[0006] In the wet treatment process, the denitrification and desalination process can effectively remove impurities such as nitrides, soluble chlorides and soluble fluorine in the aluminum ash to obtain harmless high-aluminum materials.

[0007] The high-aluminum material produced has an alumina content of more than 65% and a low silicon content. Judging from the aluminum content and the aluminum-silicon ratio, it is a high-quality aluminum resource. However, most of the aluminum element in the high-aluminum material exists in the form of inert a-alumina, and it is impossible to produce aluminum hydroxide by direct alkaline dissolution. Most of it enters the building materials industry, and the resource value is not fully utilized. Therefore, we propose a process for producing aluminum hydroxide using aluminum ash disposal slag as raw material. Summary of the invention

[0008] The purpose of the present invention is to overcome the shortcomings of the prior art, meet the actual needs, and provide a process for producing aluminum hydroxide using aluminum ash treatment slag as raw material, so as to solve the technical problem that most of the aluminum elements in the current high-aluminum materials exist in the form of inert α-alumina, and aluminum hydroxide cannot be produced by direct alkali dissolution. Most of the aluminum enters the building materials industry, and the resource value is not fully utilized.

[0009] In order to achieve the purpose of the present invention, the technical solution adopted by the present invention is: designing a process for producing aluminum hydroxide using aluminum ash disposal slag as raw material, comprising the following steps:

[0010] S1 batching: evenly mix the dry high-aluminum material produced by aluminum ash production with sodium carbonate, with the mass ratio of high-aluminum material to sodium carbonate being 0.6-1.1;

[0011] S2 Calcination: Calcine the high-aluminum material and sodium carbonate mixed in proportion at high temperature, the material calcination temperature is 1100°C-1150°C, the phase is converted into regenerated alumina clinker, and the calcination adopts a low-nitrogen burner;

[0012] The high-temperature clinker after calcination is subjected to multi-stage heat exchange with cold air, and the degree of high-aluminum clinker is reduced to below 100°C. The air is heated to 400-600°C. The heated hot air is used as a calcination combustion aid. The hot air temperature after calcination is 1100-1150°C. It is then subjected to multi-stage heat exchange with the S1 material, and the material is heated to 400-500°C. The hot air is cooled to 100-200°C and then the carbon dioxide is concentrated;

[0013] S3 leaching: high-aluminum clinker is mixed with washing liquid for dissolution reaction, the temperature is 85-95℃, the mass ratio of high-aluminum clinker to water is 1:2-1:4, and the mixture is stirred for 10-15min to fully dissolve the sodium aluminate in the high-aluminum clinker before entering the coarse filtration S4 process;

[0014] S4 coarse filtration: coarse filtration of the leached liquid to obtain a sodium aluminate solution, with a filtration accuracy of 80-150 meshes, and the coarse filtration is carried out by filter press, vacuum filtration or centrifuge, and the filter residue enters the S8 process for residue washing;

[0015] S5 fine filtration: fine filtration again through S4 sodium aluminate solution, with a filtration accuracy of 300-500 mesh, and the filtration form is one or more of precision filtration or cross-flow filtration. The semen enters the next level S6 carbon separation process for carbon dioxide decomposition, and the particulate material intercepted by the fine filtration returns to the S3 leaching process;

[0016] S6 Carbon fraction: The purified high-concentration CO2 gas from S9 is introduced into the refined filtrate produced by S5 to perform carbonation decomposition of sodium aluminate. The operating pressure is 0.1-0.3MPag, the temperature is 60-85°C, and the sodium aluminate is decomposed in the carbon fraction reaction tank with a residence time of 45-60min.

[0017] S7 filtration and washing: the slurry after carbon fractionation in S6 is filtered to separate aluminum hydroxide from the filtrate, the filtering form is one or more of a flat plate filter, a series of rotary drum filters or a horizontal belt filter, the filter cake is a wet-based multi-variety aluminum hydroxide, the filtrate is a sodium carbonate solution, and the filtrate enters the S10 evaporation and crystallization process;

[0018] S8 slag washing: the slag after coarse filtration in S4 contains alkalinity. After re-slurrying, filtration and washing, the slag no longer contains alkalinity and can be used as building material raw materials. The filtrate after filtration and washing is returned to the leaching process in S3;

[0019] S9 purification and concentration: The gas after the S2 calcination process is rich in CO2. The gas is subjected to dust removal, multi-stage cooling cycle spraying, and the gas after impurities are removed is purified gas. After gas purification, concentration and pressurization, it is used for carbonation decomposition. The pressurization is performed by a compressor, and the gas purification is performed by pressure swing adsorption. The exhaust gas temperature is 25-60°C, the exhaust pressure is 0.2-0.6Mpa.g, and the CO2 concentration is 35-40% v / v;

[0020] S10 evaporation and crystallization: the filtrate after S7 is a solution containing sodium carbonate, which is concentrated and crystallized by evaporation to produce wet-based sodium carbonate solid and evaporation condensate, which is used for washing and leaching process. The evaporator adopts one or both of energy-saving multi-effect evaporation or mechanical recompression evaporator;

[0021] S11 Carbon alkali drying: The wet sodium carbonate produced in S10 enters the dryer for drying. After drying, the moisture content of the sodium carbonate is less than 1%. After drying, the sodium carbonate returns to the batching S1 system. The drying temperature is 220-300°C. The drying adopts one or more of a vibrating fluidized bed, a disc dryer, and a rotary dryer.

[0022] Preferably, the S1 batching process measures the high-aluminum material, uses a spiral mixer as a mixing facility, and follows an analytical indicator of a Na:Al molar ratio of 1.05-1.1:1.

[0023] Preferably, the three processes of S2 calcination, S6 carbon separation, and S9 purification and concentration form a carbon dioxide cycle, which greatly reduces the purchase and supplement of carbon dioxide; the seven processes of S1 batching, S2 calcination, S3 leaching, S6 carbon separation, S7 filtration and washing, S10 evaporation and crystallization, and S11 carbon alkali drying form a carbon alkali cycle, which avoids the problems of the destination of carbon and alkali in seed decomposition, the problem of system alkali enrichment, and the problem of alkali supplementation in S1 batching.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1. The present invention uses aluminum ash treated slag (high-aluminum material) as raw material to produce aluminum hydroxide, which does not require the three processes of raw material pre-homogenization and storage, grinding, and high-pressure dissolution in normal alumina production, thereby greatly reducing production consumption; in the process of producing aluminum hydroxide using aluminum ash treated slag (high-aluminum material) as raw material, since the silicon dioxide content in the high-aluminum material is only 2-6%, the aluminum oxide content is 55-70%, the A / S is much higher than that of ordinary bauxite, and the alkali consumption is greatly reduced compared with ordinary alumina production; since the aluminum dissolved from alumina in sodium aluminate calcined at S2 high temperature is as high as more than 90%, the aluminum recovered from alumina is much higher than the aluminum oxide recovery rate (70-75%) of ordinary alumina production; the sodium aluminate calcined at S2 high temperature does not contain organic matter, thereby avoiding the influence of organic matter on the alumina system. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 is a process flow chart of the present invention; DETAILED DESCRIPTION

[0027] The present invention is further described below in conjunction with the accompanying drawings and embodiments:

[0028] Example 1: A process for producing aluminum hydroxide using aluminum ash treatment slag as raw material, see Figure 1 , including the following steps:

[0029] S1 batching: evenly mix the dry high-aluminum material produced by aluminum ash production with sodium carbonate, with the mass ratio of high-aluminum material to sodium carbonate being 0.6-1.1;

[0030] S2 Calcination: Calcine the high-aluminum material and sodium carbonate mixed in proportion at high temperature, the material calcination temperature is 1100°C-1150°C, the phase is converted into regenerated alumina clinker, and the calcination adopts a low-nitrogen burner;

[0031] The high-temperature clinker after calcination is subjected to multi-stage heat exchange with cold air, and the degree of high-aluminum clinker is reduced to below 100°C. The air is heated to 400-600°C. The heated hot air is used as a calcination combustion aid. The hot air temperature after calcination is 1100-1150°C. It is then subjected to multi-stage heat exchange with the S1 material, and the material is heated to 400-500°C. The hot air is cooled to 100-200°C and then the carbon dioxide is concentrated;

[0032] S3 leaching: high-aluminum clinker is mixed with washing liquid for dissolution reaction, the temperature is 85-95℃, the mass ratio of high-aluminum clinker to water is 1:2-1:4, and the mixture is stirred for 10-15min to fully dissolve the sodium aluminate in the high-aluminum clinker before entering the coarse filtration S4 process;

[0033] S4 coarse filtration: coarse filtration of the leached liquid to obtain a sodium aluminate solution, with a filtration accuracy of 80-150 meshes, and the coarse filtration is carried out by filter press, vacuum filtration or centrifuge, and the filter residue enters the S8 process for residue washing;

[0034] S5 fine filtration: fine filtration again through S4 sodium aluminate solution, with a filtration accuracy of 300-500 mesh, and the filtration form is one or more of precision filtration or cross-flow filtration. The semen enters the next level S6 carbon separation process for carbon dioxide decomposition, and the particulate material intercepted by the fine filtration returns to the S3 leaching process;

[0035] S6 Carbon fraction: The purified high-concentration CO2 gas from S9 is introduced into the refined filtrate produced by S5 to perform carbonation decomposition of sodium aluminate. The operating pressure is 0.1-0.3MPag, the temperature is 60-85°C, and the sodium aluminate is decomposed in the carbon fraction reaction tank with a residence time of 45-60min.

[0036] S7 filtration and washing: the slurry after carbon fractionation in S6 is filtered to separate aluminum hydroxide from the filtrate, the filtering form is one or more of a flat plate filter, a series of rotary drum filters or a horizontal belt filter, the filter cake is a wet-based multi-variety aluminum hydroxide, the filtrate is a sodium carbonate solution, and the filtrate enters the S10 evaporation and crystallization process;

[0037] S8 slag washing: the slag after coarse filtration in S4 contains alkalinity. After re-slurrying, filtration and washing, the slag no longer contains alkalinity and can be used as building material raw materials. The filtrate after filtration and washing is returned to the leaching process in S3;

[0038] S9 purification and concentration: The gas after the S2 calcination process is rich in CO2. The gas is subjected to dust removal, multi-stage cooling cycle spraying, and the gas after impurities are removed is purified gas. After gas purification, concentration and pressurization, it is used for carbonation decomposition. The pressurization is performed by a compressor, and the gas purification is performed by pressure swing adsorption. The exhaust gas temperature is 25-60°C, the exhaust pressure is 0.2-0.6Mpa.g, and the CO2 concentration is 35-40% v / v;

[0039] S10 evaporation and crystallization: the filtrate after S7 is a solution containing sodium carbonate, which is concentrated and crystallized by evaporation to produce wet-based sodium carbonate solid and evaporation condensate, which is used for washing and leaching process. The evaporator adopts one or both of energy-saving multi-effect evaporation or mechanical recompression evaporator;

[0040] S11 Carbon alkali drying: The wet sodium carbonate produced in S10 enters the dryer for drying. After drying, the moisture content of the sodium carbonate is less than 1%. After drying, the sodium carbonate returns to the batching S1 system. The drying temperature is 220-300°C. The drying adopts one or more of a vibrating fluidized bed, a disc dryer, and a rotary dryer.

[0041] For details, see Figure 1 In the S1 batching process, the high-aluminum material is measured, a spiral mixer is used as the mixing facility, and the Na:Al molar ratio is 1.05-1.1:1 according to the analytical index.

[0042] For further information, see Figure 1 The three processes of S2 calcination, S6 carbon separation, and S9 purification and concentration form a carbon dioxide cycle, which greatly reduces the purchase of carbon dioxide. The seven processes of S1 batching, S2 calcination, S3 leaching, S6 carbon separation, S7 filtration and washing, S10 evaporation and crystallization, and S11 carbon alkali drying form a carbon alkali cycle, which avoids the problems of the destination of carbon and alkali in seed decomposition, the problem of system alkali enrichment, and the problem of alkali supplementation in S1 batching.

[0043] The slag (high-aluminum material) produced from the treated aluminum ash has no harmful components and low impurity content. The aluminum hydroxide produced has good whiteness and high purity.

[0044] After testing, the main components of high-aluminum materials produced from aluminum ash are as follows:

[0045]

[0046] The aluminum hydroxide produced by the above process has an aluminum oxide dissolution rate of more than 90%.

[0047] The present invention has been experimentally studied and the process technology is very suitable for producing alumina using aluminum ash disposal slag (high aluminum material) as raw material. Compared with the traditional method of producing aluminum hydroxide using aluminum ore soil as raw material, the present invention reduces the high-pressure dissolution process and significantly reduces the production cost.

[0048] In addition, the components designed in the present invention are all universal standard parts or components known to technical personnel in this field. Their structures and principles can be known to technical personnel through technical manuals or through conventional experimental methods. They can be fully implemented by technical personnel in this field. Needless to say, the content protected by the present invention does not involve improvements to internal structures and methods.

[0049] The embodiments of the present invention disclose preferred embodiments, but are not limited thereto. A person skilled in the art can easily understand the spirit of the present invention based on the above embodiments and make different extensions and changes. However, as long as they do not deviate from the spirit of the present invention, they are all within the protection scope of the present invention.

Claims

1. A process for producing aluminum hydroxide using aluminum ash treatment slag as raw material, characterized in that: The following steps are involved: S1 batching: evenly mix the dry high-aluminum material produced by aluminum ash production with sodium carbonate, with the mass ratio of high-aluminum material to sodium carbonate being 0.6-1.1; S2 Calcination: Calcine the high-aluminum material and sodium carbonate mixed in proportion at high temperature, the material calcination temperature is 1100°C-1150°C, the phase is converted into regenerated alumina clinker, and the calcination adopts a low-nitrogen burner; The high-temperature clinker after calcination is subjected to multi-stage heat exchange with cold air, and the degree of high-aluminum clinker is reduced to below 100°C. The air is heated to 400-600°C. The heated hot air is used as a calcination combustion aid. The hot air temperature after calcination is 1100-1150°C. It is then subjected to multi-stage heat exchange with the S1 material, and the material is heated to 400-500°C. The hot air is cooled to 100-200°C and then the carbon dioxide is concentrated; S3 leaching: high-aluminum clinker is mixed with washing liquid for dissolution reaction, the temperature is 85-95℃, the mass ratio of high-aluminum clinker to water is 1:2-1:4, and the mixture is stirred for 10-15min to fully dissolve the sodium aluminate in the high-aluminum clinker before entering the coarse filtration S4 process; S4 coarse filtration: coarse filtration of the leached liquid to obtain a sodium aluminate solution, with a filtration accuracy of 80-150 meshes, and the coarse filtration is carried out by filter press, vacuum filtration or centrifuge, and the filter residue enters the S8 process for residue washing; S5 fine filtration: fine filtration again through S4 sodium aluminate solution, with a filtration accuracy of 300-500 mesh, and the filtration form is one or more of precision filtration or cross-flow filtration. The semen enters the next level S6 carbon separation process for carbon dioxide decomposition, and the particulate material intercepted by the fine filtration returns to the S3 leaching process; S6 Carbon fraction: The purified high-concentration CO2 gas from S9 is introduced into the refined filtrate produced by S5 to perform carbonation decomposition of sodium aluminate. The operating pressure is 0.1-0.3MPag, the temperature is 60-85°C, and the sodium aluminate is decomposed in the carbon fraction reaction tank with a residence time of 45-60min. S7 filtration and washing: the slurry after carbon fractionation in S6 is filtered to separate aluminum hydroxide from the filtrate, the filtering form is one or more of a flat plate filter, a series of rotary drum filters or a horizontal belt filter, the filter cake is a wet-based multi-variety aluminum hydroxide, the filtrate is a sodium carbonate solution, and the filtrate enters the S10 evaporation and crystallization process; S8 slag washing: the slag after coarse filtration in S4 contains alkalinity. After re-slurrying, filtration and washing, the slag no longer contains alkalinity and can be used as building material raw materials. The filtrate after filtration and washing is returned to the leaching process in S3; S9 purification and concentration: The gas after the S2 calcination process is rich in CO2. The gas is subjected to dust removal, multi-stage cooling cycle spraying, and the gas after impurities are removed is purified gas. After gas purification, concentration and pressurization, it is used for carbonation decomposition. The pressurization is performed by a compressor, and the gas purification is performed by pressure swing adsorption. The exhaust gas temperature is 25-60°C, the exhaust pressure is 0.2-0.6Mpa.g, and the CO2 concentration is 35-40% v / v; S10 evaporation and crystallization: the filtrate after S7 is a solution containing sodium carbonate, which is concentrated and crystallized by evaporation to produce wet-based sodium carbonate solid and evaporation condensate, which is used for washing and leaching process. The evaporator adopts one or both of energy-saving multi-effect evaporation or mechanical recompression evaporator; S11 Carbon alkali drying: The wet sodium carbonate produced in S10 enters the dryer for drying. After drying, the moisture content of the sodium carbonate is less than 1%. After drying, the sodium carbonate returns to the batching S1 system. The drying temperature is 220-300°C. The drying adopts one or more of a vibrating fluidized bed, a disc dryer, and a rotary dryer.

2. The process for producing aluminum hydroxide using aluminum ash treatment slag as raw material as claimed in claim 1, characterized in that: The S1 batching process measures the high-aluminum material, uses a spiral mixer as a mixing facility, and follows the analytical indicator of a Na:Al molar ratio of 1.05-1.1:

1.

3. The process for producing aluminum hydroxide using aluminum ash treatment slag as raw material as claimed in claim 1, characterized in that: The three processes of S2 calcination, S6 carbon separation, and S9 purification and concentration form a carbon dioxide cycle, which greatly reduces the purchase and supplement of carbon dioxide; the seven processes of S1 batching, S2 calcination, S3 leaching, S6 carbon separation, S7 filtration and washing, S10 evaporation and crystallization, and S11 carbon alkali drying form a carbon alkali cycle, which avoids the problems of the destination of carbon and alkali in seed decomposition, the problem of system alkali enrichment, and the problem of alkali supplementation in S1 batching.