Chromium slag utilization method
Through ball milling of chromium slag and sodium-containing alkaline substances and low-temperature oxidation roasting, combined with water leaching and crystallization methods, the problem of low chromium extraction rate and incomplete resource utilization of chromium slag was solved, and efficient chromium resource utilization and no waste water, The waste-free process improves the industrial purity and economic benefits of the product.
Patent Information
- Application Number
- CN202410783876.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-18
AI Technical Summary
In the existing technology, the chromium extraction rate of chromium residue is low, resource utilization is incomplete, product economic benefits are low, and there are problems of insufficient chromium reduction and chromium pollution.
By ball milling chromium slag and sodium-containing alkaline substances, low-temperature oxidation roasting, combined with water leaching and crystallization methods, sodium chromate is separated and extracted, avoiding the chromium reduction step in the traditional crystallization method, and achieving efficient extraction of chromium and separation of sodium phosphate. .
It improves the extraction rate and resource utilization rate of chromium, realizes a wastewater-free and waste-residue-free process, solves the problems of chromium resource waste and environmental pollution, and improves the industrial purity and economic benefits of the product.
Smart Images

Figure BDA0004898018420000061 
Figure BDA0004898018420000071 
Figure HDA0004898018430000011
Abstract
Description
Technical Field
[0001] The invention belongs to the field of solid waste resource utilization in the battery industry, and specifically relates to a method for utilizing chromium slag. Background Art
[0002] In the battery industry, nickel salts are produced by using nickel-iron alloy process. The impurity removal process of this process will produce a large amount of by-product high-phosphorus iron-chromium slag, referred to as chromium slag. Since chromium slag is the residue generated by the smelting process, the valuable metals and impurities are recombined and distributed in the slag forming process to form a stable compound mixed with each other. The main components of the chromium slag are compounds composed of metal cations such as iron, nickel, and chromium and phosphorus-containing anions. For example, phosphorus is generally mixed with one or more of orthophosphate, hypophosphite, phosphite, metaphosphate, polyphosphate or pyrophosphate. The compound composition of chromium slag is very complex. Conventional ore sorting is difficult to achieve the purification of various compounds in chromium slag or the extraction of valuable elements (iron, phosphorus, nickel, chromium). Therefore, although the content of iron phosphate and valuable elements in chromium slag is very high, it is difficult to utilize it as a resource. It has been stored as hazardous waste for a long time, or landfilled after solidification or stabilization; it not only occupies a large amount of land, but also has a high environmental risk.
[0003] At present, the calcium-free roasting method can oxidize the chromium in the iron-chromium slag under alkaline and high temperature conditions, convert the low-valent chromium into hexavalent chromium and then extract it. However, this method mainly destroys the iron-chromium spinel structure by high-temperature roasting greater than 1000°C, but this method is not suitable for application to the high-phosphorus iron-chromium slag, because the high-phosphorus iron-chromium slag will melt at 900°C or above, making the subsequent leaching and extraction more difficult. And this technology also has the defects of chromium encapsulation, poor mass transfer effect and low chromium extraction rate (generally below 80%) due to the small proportion of chromium and insufficient contact between chromium and alkali, as well as the difficulty in separating and purifying sodium phosphate and sodium chromate. In addition, the chromium extracted by this method currently uses the traditional crystallization method to precipitate chromium salts and reduce the chromium therein. The process has the problem of insufficient chromium reduction, low chromium reduction efficiency, and the generation of chromium slag again, resulting in waste of chromium resources, new chromium pollution, incomplete resource utilization, low product economic benefits, and limited application fields. Summary of the invention
[0004] In view of the problems of low chromium extraction rate, incomplete resource utilization of chromium slag, low economic benefits of products, etc. in the above-mentioned prior art, the present invention will provide a method for utilizing chromium slag, which has a high chromium extraction rate in the chromium slag and converts all the chromium into sodium chromate, and the chromium slag is completely utilized as a resource, and no wastewater or waste slag is generated during the process.
[0005] To achieve the above purpose, the following technical solutions are specifically included:
[0006] A method for utilizing chromium slag comprises the following steps:
[0007] (1) ball-milling chromium slag and sodium-containing alkaline substances to obtain a mixture;
[0008] (2) calcining the mixture to obtain a calcined product; the calcining temperature is 650-800° C.;
[0009] (3) immersing the roasted product in water to obtain iron ore and leaching solution after solid-liquid separation;
[0010] (4) crystallizing the leachate to obtain sodium phosphate and a separated liquid after solid-liquid separation;
[0011] (5) Evaporating and crystallizing the separated liquid to obtain sodium chromate.
[0012] In the method of the present invention, chromium slag and sodium-containing alkaline substances are mixed and ball-milled to change the crystal phase structure of the chromium slag, which can improve the oxidation efficiency of chromium during roasting; then a low-temperature oxidation roasting method is used to achieve crystal transformation, so that the main phase material releases chromium ions after crystal transformation, and the chromium ions are exposed to an alkaline environment during the crystal transformation process to fully oxidize, thereby improving the oxidation rate of chromium. The ball milling combined with the low-temperature oxidation roasting solves the problems of insufficient oxidation caused by chromium wrapping, low mass transfer between chromium and alkaline substances, and incomplete contact in the calcium-free roasting method, thereby increasing the extraction rate of chromium; the method of the present invention also separates sodium phosphate and sodium chromate by a crystallization method based on solubility differences, instead of reducing chromium after crystallization in the traditional method, thereby avoiding the problem of insufficient chromium reduction and the generation of chromium slag again.
[0013] Preferably, in step (1), the sodium-containing alkaline substance includes at least one of sodium hydroxide, sodium carbonate and sodium bicarbonate.
[0014] Preferably, in step (1), the chromium slag comprises the following components in percentage by mass: 1%-5% chromium, 30%-35% iron, and 15%-20% phosphorus.
[0015] The method of the present invention is more suitable for the above-mentioned chromium slag with high iron and phosphorus content.
[0016] Preferably, in step (1), the mass ratio of the chromium slag to the sodium-containing alkaline substance is 1:(0.8-1.3).
[0017] Preferably, in step (1), the ball milling time is 30-150 min.
[0018] Preferably, in step (2), the calcination temperature is 700-750°C.
[0019] Preferably, in step (2), the calcination time is 180-270 min.
[0020] Preferably, in step (3), the number of immersions is 1-3 times, the temperature of each immersion is selected from 50-95° C., and the time of each immersion is selected from 60-240 min.
[0021] Preferably, in step (3), the mass ratio of the roasted product to water is 1:(1-3).
[0022] Preferably, in step (4), the crystallization temperature is 20-30°C.
[0023] At the above cooling temperature, it can be ensured that no sodium chromate is precipitated, and what is precipitated is sodium phosphate.
[0024] Preferably, in step (5), the evaporation temperature is 80-90°C, and the crystallization temperature is 15-25°C.
[0025] Considering the high solubility of sodium chromate, in order to separate and purify sodium chromate, the density of the sodium chromate solution obtained after evaporation is 1.8-2.0g / cm 3 , combined with a crystallization temperature of 15-25°C, industrial purity sodium chromate can be obtained. In addition, the distilled water produced by evaporation and cooling crystallization is collected and used for subsequent leaching of roasted materials, realizing water recycling.
[0026] Compared with the prior art, the present invention has the following beneficial effects: the present invention fully extracts Cr and P from the chromium slag through the steps of mixed grinding, low-temperature roasting and crystal transformation, water immersion, crystallization, separation and the like of chromium slag and sodium-containing alkaline substances, and separates and prepares phosphate, sodium chromate and industrial iron ore products, thereby realizing full resource utilization of the valuable elements in the chromium slag, solving the environmental pollution problem of chromium slag in the nickel salt process of nickel-iron alloy production, solving the defects of chromium encapsulation, poor mass transfer effect and low chromium extraction rate, low chromium reduction efficiency, introduction of new impurities, waste of chromium resources, new chromium pollution, and difficulty in separating and purifying sodium phosphate and sodium chromate in the traditional calcium-free roasting process due to the small proportion of chromium and insufficient contact between chromium and alkali. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 Flow chart of the method for utilizing chromium slag of the present invention.
[0028] Figure 2 The XRD spectra of the mixture in step (1) of Comparative Example 1 and Examples 1-3 and the chromium slag are shown.
[0029] Figure 3 The local XRD spectra of the mixture in step (1) of Comparative Example 1 and Examples 1-3 and the chromium slag.
[0030] Figure 4 The XRD spectra of the calcined product and chromium slag in step (2) in Examples 1 and 4-6.
[0031] Figure 1-4 The chromium slag, chromium slag original sample, and chromium slag original slag involved in the invention are all represented as raw materials in the following embodiments and comparative examples: chromium slag (dry slag), and the chromium slag used in all embodiments and comparative examples is the same. DETAILED DESCRIPTION
[0032] In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention will be further described below through specific examples. The test methods used in the examples and / or comparative examples are conventional methods unless otherwise specified; the materials, reagents, etc. used can be obtained from commercial channels unless otherwise specified.
[0033] The chromium slag used below is a by-product high-phosphorus ferrochromium slag collected from the impurity removal process of producing nickel salts by the nickel-iron alloy process in the battery industry. There are no special requirements and it can be purchased on the market or collected by itself. The chromium slag used in the following embodiments and comparative examples has the same source, and the chromium slag includes the following components in percentage by mass: 1%-5% chromium, 30%-35% iron, and 15%-20% phosphorus.
[0034] Example 1
[0035] A method for utilizing chromium slag, the specific process is as follows Figure 1 As shown, the specific steps include:
[0036] (1) 50 g of chromium slag (dry slag) and 50 g of sodium carbonate were ball-milled in a ball mill for 150 min. After ball-milling, the solid was sieved through a 250-mesh sieve to obtain a mixture;
[0037] (2) calcining the mixture in a box-type muffle furnace under air atmosphere at 750° C. for 240 min to obtain a calcined product;
[0038] (3) Leaching the roasted product with pure water at a solid-liquid ratio of 1:2 at 80°C for 150 minutes, separating the solid and the liquid to obtain a leachate and a filter residue; repeating the above immersion conditions twice, combining the leachates, and drying the filtered solid to obtain industrial iron ore;
[0039] (4) placing the leachate obtained in step (3) in a crystallizer. Since the temperature of the leachate is relatively high, the leachate needs to be cooled to 25° C. for crystallization. After the crystallization is completed, centrifugation is performed to obtain sodium phosphate solid and separated liquid. The dried sodium phosphate solid meets the standard of "Industrial Trisodium Phosphate HG / T 2517";
[0040] (5) placing the separated liquid obtained in step (4) in an evaporator and evaporating it at 85° C., and the distilled water generated in this process is returned to the leaching stage, so that no wastewater or solid waste is generated in the whole process of the chromium slag process; the liquid remaining after evaporation is a sodium chromate solution, and the density of the sodium chromate solution is 1.9 g / cm3 The sodium chromate solution is then cooled to 18°C for crystallization. After drying, the sample is solid sodium chromate, which meets the standard of "Industrial Sodium Chromate HG / T 4312".
[0041] Example 2
[0042] The difference between this embodiment and embodiment 1 is that in step (1), the ball milling time is 30 minutes.
[0043] Example 3
[0044] The difference between this embodiment and embodiment 1 is that in step (1), the ball milling time is 90 minutes.
[0045] Example 4
[0046] The difference between this embodiment and embodiment 1 is that in step (2), the calcination temperature is 650°C.
[0047] Example 5
[0048] The difference between this embodiment and embodiment 1 is that in step (2), the calcination temperature is 700°C.
[0049] Example 6
[0050] The difference between this embodiment and embodiment 1 is that in step (2), the calcination temperature is 800°C.
[0051] Example 7
[0052] A method for utilizing chromium slag specifically comprises the following steps:
[0053] (1) 50 g of chromium slag (dry slag) and 40 g of sodium carbonate were ball-milled in a ball mill for 150 min. After ball-milling, the solid was sieved through a 250-mesh sieve to obtain a mixture;
[0054] (2) calcining the mixture in a box-type muffle furnace under air atmosphere at 750° C. for 270 min to obtain a calcined product;
[0055] (3) Leaching the roasted product with pure water at a solid-liquid ratio of 1:3 at 95°C for 120 minutes, separating the solid and the liquid to obtain a leachate and a filter residue; repeating the above-mentioned immersion conditions twice, combining the leachates, and drying the filtered solid to obtain industrial iron ore;
[0056] (4) placing the leachate obtained in step (3) in a crystallizer, cooling and crystallizing at 20° C., and after the crystallization is completed, centrifuging to obtain sodium phosphate solid and separated liquid, wherein the dried sodium phosphate solid meets the standard of "Industrial Trisodium Phosphate HG / T 2517";
[0057] (5) placing the separated liquid obtained in step (4) in an evaporator and evaporating it at 90° C., and the distilled water generated in the process is returned to the leaching stage, so that no wastewater or solid waste is generated in the whole process of the chromium slag process; the liquid remaining after evaporation is a sodium chromate solution, and the density of the sodium chromate solution is 1.9 g / cm 3 The sodium chromate solution is then placed at room temperature of 25°C for cooling and crystallization. After drying, the sample is solid sodium chromate, which meets the standard of "Industrial Sodium Chromate HG / T 4312".
[0058] Example 8
[0059] A method for utilizing chromium slag specifically comprises the following steps:
[0060] (1) 50 g of chromium slag (dry slag) and 65 g of sodium carbonate were ball-milled in a ball mill for 120 min. After ball-milling, the solid was sieved through a 250-mesh sieve to obtain a mixture;
[0061] (2) calcining the mixture in a box-type muffle furnace under air atmosphere at 750° C. for 180 min to obtain a calcined product;
[0062] (3) Leaching the roasted product with pure water at a solid-liquid ratio of 1:3 at 50°C for 240 minutes, separating the solid and the liquid to obtain a leachate and a filter residue; repeating the above immersion conditions twice, combining the leachates, and drying the filtered solid to obtain industrial iron ore;
[0063] (4) placing the leachate obtained in step (3) in a crystallizer, cooling and crystallizing at 30° C., and after the crystallization is completed, centrifuging to obtain sodium phosphate solid and separated liquid, wherein the dried sodium phosphate solid meets the standard of “Industrial Trisodium Phosphate HG / T 2517”;
[0064] (5) placing the separated liquid obtained in step (4) in an evaporator and evaporating it at 85° C., and the distilled water generated in this process is returned to the leaching stage, so that no wastewater or solid waste is generated in the whole process of the chromium slag process; the liquid remaining after evaporation is a sodium chromate solution, and the density of the sodium chromate solution is 1.9 g / cm 3 The sodium chromate solution is then placed at room temperature of 15°C for cooling and crystallization. After drying, the sample is solid sodium chromate, which meets the standard of "Industrial Sodium Chromate HG / T 4312".
[0065] Comparative Example 1
[0066] The difference between this comparative example and Example 1 is that the ball milling in the ball mill in step (1) is not performed, and in this comparative example, the mixture of chromium slag and sodium carbonate is subjected to steps (2) to (5).
[0067] Comparative Example 2
[0068] The difference between this comparative example and Example 1 is that in step (2), the calcination temperature is 900°C.
[0069] The chromium slag becomes molten and chromium and phosphorus cannot be effectively leached.
[0070] Comparative Example 3
[0071] The difference between this comparative example and Example 1 is that in step (2), the calcination temperature is 600°C.
[0072] The chromium slag, the mixture obtained in step (1) and the roasted product obtained in step (2) are characterized by XRD, and the chromium and phosphorus contents in the leaching solution of step (3) are measured by ICP to calculate the leaching rates of chromium and phosphorus.
[0073] Table 1
[0074]
[0075]
[0076] In the method of the present invention, the chromium slag is roasted (low-temperature oxidation roasting) in air and alkaline conditions, and the substances in the chromium slag undergo a crystal phase transformation, wherein the chromium element is oxidized, and the chromium element and the phosphorus element in the chromium slag exist in the form of sodium chromate and sodium phosphate. Since these two sodium salts are soluble in water, both can be effectively leached during the water immersion process; and in the method of the present invention, before the low-temperature oxidation roasting, the chromium slag and the sodium-containing alkaline substance are mixed and ball-milled to pre-change the crystal phase structure of the chromium slag, which can further improve the oxidation efficiency of chromium during low-temperature oxidation roasting and further improve the leaching rate of chromium and phosphorus.
[0077] From the attached Figure 2-3 It can be seen from the XRD diagram that as the grinding time increases, the mineral phase of the chromium slag does not change, but the diffraction peak gradually broadens, and the microstructure of the chromium slag crystal changes. As the grinding time increases, the main peak of the mixed ground sample shifts to the left compared to the original chromium slag sample. Partial oxidation may occur in the mixed phase, causing the sample surface to break and resulting in grain size reduction. From Table 1, it can be seen that compared with the non-grinding roasting in Comparative Example 1, the grinding in Examples 2-4 helps the leaching of chromium and phosphorus. Grinding for 150 minutes before roasting allows the elements in the chromium slag to be fully utilized, which is helpful for the next step of cooling crystallization.
[0078] From the attached Figure 4As shown in Table 1, the main phase of the original chromium slag is Fe5(PO4)4(OH)3·2H2O. In the present invention, the chromium slag is ground with sodium carbonate and then solid-phase calcined to release chromium ions after crystal transformation. With the increase of temperature, only the ferric oxide crystal form is transformed at 650°C and 700°C, but not the trisodium phosphate crystal form. Under this condition, the leaching rate is low because the chromium ions are not completely released into the alkaline environment. Combined with Comparative Example 3, it can be seen that the calcination temperature should not be lower than 650°C. With the increase of temperature, the main phase of the chromium slag is gradually transformed into ferric oxide and trisodium phosphate at 750°C and 800°C, so that the chromium can be completely released into the alkaline environment to improve the oxidation rate of chromium. Compared with the mixed slag calcined at 750°C and 800°C in Example 1, there are more impurities, which is not conducive to the leaching of chromium. Combined with Comparative Example 2, it can be seen that the calcination temperature should not be too high. If the temperature is too high, the chromium slag will melt, making the chromium slag more tightly wrapped, making it more difficult to leach chromium and phosphorus, and it is impossible to effectively leach chromium and phosphorus.
[0079] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for utilizing chromium slag, characterized in that: The steps include: (1) ball-milling chromium slag and sodium-containing alkaline substances to obtain a mixture; (2) calcining the mixture to obtain a calcined product; the calcining temperature is 650-800° C.; (3) immersing the roasted product in water to obtain iron ore and leaching solution after solid-liquid separation; (4) crystallizing the leachate to obtain sodium phosphate and a separated liquid after solid-liquid separation; (5) Evaporating and crystallizing the separated liquid to obtain sodium chromate.
2. The method for utilizing chromium slag according to claim 1, characterized in that: In step (1), the ball milling time is 30-150 minutes; the chromium slag comprises the following components in percentage by weight: 1%-5% chromium, 30%-35% iron, and 15%-20% phosphorus.
3. The method for utilizing chromium slag according to claim 1, characterized in that: In step (2), the calcination temperature is 700-750°C.
4. The method for utilizing chromium slag according to claim 1, characterized in that: In step (2), the calcination time is 180-270 min.
5. The method for utilizing chromium slag according to claim 1, characterized in that: In step (1), the sodium-containing alkaline substance includes at least one of sodium hydroxide, sodium carbonate, and sodium bicarbonate.
6. The method for utilizing chromium slag according to claim 1, characterized in that: In step (1), the mass ratio of the chromium slag to the sodium-containing alkaline substance is 1:(0.8-1.3).
7. The method for utilizing chromium slag according to claim 1, characterized in that: In step (3), the number of immersions is 1-3 times, the temperature of each immersion is selected from 50-95° C., and the time of each immersion is selected from 60-240 min.
8. The method for utilizing chromium slag according to claim 1, characterized in that: In step (3), the mass ratio of the roasted product to water is 1:(1-3).
9. The method for utilizing chromium slag according to claim 1, characterized in that: In step (4), the crystallization temperature is 20-30°C.
10. The method for utilizing chromium slag according to claim 1, characterized in that: In step (5), the evaporation temperature is 80-90°C, and the crystallization temperature is 15-25°C.
Citation Information
Patent Citations
Method for recovering vanadium and chromium from vanadium and chromium-containing slag
CN102586612A
Method for extracting chromium from high-chromium-content calcium-chromium slag
CN106381394A
Method for preparing mica iron oxide by using chromium-containing iron slag which is the by-product of chromium salt wet process
CN108128810A