Compound, ion exchange membrane and preparation method and application thereof

By introducing metal-organic polyhedron and cerium ion complexes into the ion exchange membrane to form a three-dimensional structure to improve conductivity and barrier properties, the problem that the ion exchange membrane is susceptible to free radical attacks in the existing technology is solved, and higher chemical properties are achieved. stability and electrochemical performance.

CN118725488APending Publication Date: 2024-10-01STATE POWER INVESTMENT CORP HYDROGEN ENERGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410707698.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-03
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing ion exchange membranes are susceptible to hydroxyl radical attack in fuel cells, leading to performance degradation and shortened lifetime, and current solutions such as impregnating cerium ion solutions or doping cerium-based metal salts/metal oxide methods reduce proton transport capabilities and conductivity, and poor compatibility, resulting in reduced electrochemical performance.

Method used

Using a composite of metal-organic polyhedron and ion exchange resin, the three-dimensional structure formed by the assembly of cerium ions and organic ligands improves the conductivity and barrier properties, enhances mechanical properties and electrochemical properties, and serves as the coordination center of the metal-organic polyhedron. Quencher of hydroxyl radicals to improve chemical stability.

Benefits of technology

Significantly improves the chemical stability, resistance to free radical attack and electrochemical performance of the ion exchange membrane, extends the service life of the battery, improves the conductivity and mechanical properties, avoids cross-linking contact between cerium ions and resin, and enhances interaction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725488A_ABST
    Figure CN118725488A_ABST
Patent Text Reader

Abstract

The invention discloses a compound, an ion exchange membrane and a preparation method and application thereof, the compound comprises ion exchange resin and a metal organic polyhedron, and the metal organic polyhedron comprises cerium ions and an organic ligand. According to the invention, the metal organic polyhedron has good solubility in a solvent, is in a monomolecular state in a solution or a polymer, and has better performance than nano metal salt, and the three-dimensional structure of the metal organic polyhedron is beneficial to proton conduction, prolongs the transmission path of gas and small organic molecules, and can improve the conductivity and barrier property of the compound; the mechanical performance and the electrochemical performance are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of ion exchange membranes, and in particular to a composite, an ion exchange membrane, and a preparation method and application thereof. Background Art

[0002] Ion exchange membranes can be divided into fuel cell proton exchange membranes, chlor-alkali industrial membranes, flow battery membranes, water electrolysis hydrogen production proton exchange membranes, separation membranes, etc. according to different usage scenarios. Among them, perfluorosulfonic acid resin (PFSA) ion exchange membranes are widely used due to their excellent chemical stability. However, after circulating in the battery for a period of time, the performance will decay due to the attack of various free radicals, and even cause battery damage. Taking fuel cells as an example, fuel cells are composed of many key components. The decay of other components such as catalysts and gas diffusion layers generally only leads to a decrease in battery performance, but the damage of proton exchange membranes will directly lead to the mixing of cathode and anode reaction gases, causing direct battery failure and even safety accidents. Therefore, as the core component of fuel cells, the mass transfer performance and chemical stability of proton exchange membranes are closely related to the performance of fuel cells. It is crucial to develop ion exchange membranes with high performance and high durability.

[0003] During the operation of the fuel cell, the ion exchange membrane is susceptible to attack by hydroxyl radicals, i.e., chemical degradation of the PFSA ionomer. It is generally believed that free radicals are generated by oxidation induction, such as hydroxyl (HO·), hydrogen peroxide (OOH·), and hydrogen (H·). Such free radicals mainly cause membrane cleavage due to incomplete redox reaction on the cathode side or gas penetration through the PEM, resulting in degradation of membrane performance and even perforation, leading to battery failure. Therefore, it is necessary to improve the chemical durability of the ion exchange membrane to overcome the performance degradation and shortened life caused by hydroxyl radical attack.

[0004] At present, free radical attack on ion exchange membranes can be alleviated by adding free radical quenchers, for example, the ion exchange membrane is impregnated with cerium ion solution or doped with cerium-based metal salts / metal oxides to improve chemical durability. However, the method of impregnating cerium ion solution or doping with cerium-based metal salts / metal oxides is simple, but it will lead to a significant decrease in the proton transport capacity of the ion exchange membrane, reduce conductivity, and sacrifice electrochemical performance. Cerium-based metal salts / metal oxides have poor compatibility with polymers, are unevenly dispersed in polymers, will produce agglomeration, and the doping amount is limited.

[0005] Metal-organic polyhedra (MOP) are nanocages with specific spatial structure formed by assembling metal ion clusters and building blocks with coordination functional groups. Compared with metal-organic frameworks (MOFs), MOPs also have the advantages of regular pores, adjustable pore size, high porosity, etc., and also have the advantages of structural design that MOFs do not have. Summary of the invention

[0006] The present invention is based on the inventors' discovery and understanding of the following facts and problems: At present, free radical attack on ion exchange membranes can be alleviated by adding free radical quenchers. However, the method of impregnating cerium ion solution or doping cerium-based metal salts / metal oxides is simple, but will lead to a significant decrease in the proton transport capacity of the ion exchange membrane, reduce conductivity, and sacrifice electrochemical performance. In addition, cerium-based metal salts / metal oxides have poor compatibility with polymers, are unevenly dispersed in polymers, will produce agglomerations, and the doping amount is limited.

[0007] The present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, the embodiments of the present invention provide a composite, an ion exchange membrane, and a preparation method and application thereof. The metal organic polyhedron has good solubility in a solvent, is in a single molecule state in a solution or a polymer, and has better performance than nano metal salts. The three-dimensional structure of the metal organic polyhedron is conducive to the conduction of protons and extends the transmission path of gases and organic small molecules, which can improve the conductivity and barrier properties of the composite, and enhance the mechanical properties and electrochemical properties.

[0008] The embodiment of the present invention provides a composite, comprising: an ion exchange resin and a metal organic polyhedron, wherein the metal organic polyhedron comprises cerium ions and an organic ligand, and the structural formula of the organic ligand is shown in formula (1):

[0009]

[0010] Wherein, Z in formula (1) is selected from the following structures:

[0011]

[0012]

[0013] Advantages and technical effects of the composite of the embodiment of the present invention: the composite includes an ion exchange resin and a metal organic polyhedron, the metal organic polyhedron has a special spatial structure, has good solubility in a solvent, can overcome the problem of uneven dispersion of cerium-based metal salts and metal oxides in the resin, the metal organic polyhedron is in a single molecule state in the solution, can be doped with the resin at the molecular level, and can enhance the interaction between the resin matrix, and the performance is better than that of nano cerium salt. The cage of the metal organic polyhedron has a spatial structure of a specific size and an internal channel of a special cavity, which can allow a certain amount of small molecules to pass through, can adjust the ion transfer site and the sulfonate arrangement, and improve the electrochemical performance. The three-dimensional structure in the metal organic polyhedron is conducive to the conduction of protons, and extends the transmission path of gases and organic small molecules, which can improve the conductivity and barrier properties of the material, and enhance the mechanical properties and electrochemical properties. The metal organic polyhedron of the present invention has structural diversity and controllable and adjustable structure, has great advantages in constructing proton transfer, and has broad application prospects. Introducing cerium ions into the composite in the form of metal organic polyhedrons can effectively avoid cross-linking contact between cerium ions and ionic groups of ion exchange polymers, such as sulfonic acid functional groups. The coordination center of the metal organic polyhedron is the cerium ion, which can act as a hydroxyl radical quencher, significantly improving the chemical stability, chemical durability and resistance to free radical attack of the composite.

[0014] In some embodiments, the topological structure of the metal-organic polyhedron is a three-dimensional structure;

[0015] And / or, the unit cell volume of the metal organic polyhedron is

[0016] and / or, the composite comprises 95% to 99.99% ion exchange resin and 0.01% to 5% metal organic polyhedron, by mass;

[0017] And / or, the ion exchange resin comprises at least one of perfluorosulfonic acid resin, perfluorosulfonimide resin, polyacid side chain perfluoro resin, sulfonated polytrifluorostyrene, sulfonated polysulfone, sulfonated polyethersulfone, sulfonated polyetheretherketone, sulfonated polyaryletherketone, sulfonated polyarylethernitrile, sulfonated polyphosphazene, sulfonated polyphenylene oxide, sulfonated polybenzonitrile, sulfonated polyimide or sulfonated polybenzimidazole;

[0018] And / or, the cerium ions include Ce 4+ .

[0019] The embodiment of the present invention provides a method for preparing a composite, comprising: dispersing an ion exchange resin and a metal organic polyhedron in a solvent to obtain a dispersion, and then drying the dispersion to obtain a composite. In the embodiment of the present invention, the process is simple, easy to operate, and has high production efficiency, and is easy to be widely used in industrial production.

[0020] In some embodiments, the dispersion temperature is 10 to 240°C;

[0021] And / or, the dispersion time is 0.1 to 24 hours;

[0022] And / or, the drying temperature is 20-180°C.

[0023] An embodiment of the present invention provides an ion exchange membrane, comprising: the composite material described in the embodiment of the present invention or a composite material prepared by the preparation method described in the embodiment of the present invention.

[0024] In the embodiment of the present invention, the ion exchange membrane has all the advantages of the composite material, which will not be described in detail here. The metal organic polyhedron has good solubility, can enhance the interaction between the ion exchange resin matrix, and thus has excellent film processing properties. The introduction of cerium ions through the metal nodes of the metal organic polyhedron can quench the free radicals generated during the operation of the ion exchange membrane, reduce the attack on the ion exchange membrane, and thus improve its mechanical properties. The introduction of metal organic polyhedron into the ion exchange membrane effectively improves the chemical stability, chemical durability, resistance to free radical attack, mechanical properties and electrochemical properties of the ion exchange membrane, thereby improving the comprehensive performance of the ion exchange membrane.

[0025] In some embodiments, comprising 95% to 99.99% ion exchange resin and 0.01% to 5% metal organic polyhedron, by mass;

[0026] And / or, the thickness of the ion exchange membrane is 4 to 50 μm;

[0027] and / or, the ion exchange capacity of the ion exchange membrane is 0.1 to 4.2 mmol / g;

[0028] And / or, the ion exchange membrane comprises a reinforced membrane.

[0029] The present invention provides a method for preparing an ion exchange membrane, comprising the following steps:

[0030] (1) dispersing an ion exchange resin and a metal organic polyhedron in a solvent to obtain a dispersion;

[0031] (2) The dispersion is molded and then dried to obtain an ion exchange membrane.

[0032] In the embodiments of the present invention, the prepared ion exchange membrane has good flatness, uniform thickness distribution, simple process, convenient operation, high production efficiency, and is convenient for wide application in industrial production.

[0033] In some embodiments, in step (1), the dispersion temperature is 10 to 240°C;

[0034] And / or, in the step (1), the dispersion time is 0.1 to 24 hours;

[0035] And / or, in the step (2), the forming comprises at least one of casting, pouring or coating;

[0036] And / or, the step (2) further comprises a reinforced membrane, wherein the dispersion is loaded on the reinforced membrane and then dried to obtain an ion exchange membrane;

[0037] And / or, in the step (2), the drying temperature is 20 to 180°C.

[0038] The embodiment of the present invention provides an application of a composite or ion exchange membrane, which is used for at least one of batteries, chlor-alkali industry, water electrolysis hydrogen production, capacitors, electrodialysis, sensors, desalination membranes, ultrafiltration membranes, microfiltration membranes, fabrics, and protective equipment. In the embodiment of the present invention, all the advantages of the composite and ion exchange membrane are possessed, which will not be repeated here.

[0039] In some embodiments, at least one of the following is used for proton exchange membranes for fuel cells, liquid flow battery membranes, polyelectrolyte membranes for the chlor-alkali industry, proton exchange membranes for water electrolysis to produce hydrogen, acidic primary battery membranes, lithium battery membranes, polyelectrolytes in supercapacitors, and electrodialysis membranes for metal recovery.

[0040] The embodiment of the present invention provides a fuel cell, comprising the composite or the ion exchange membrane described in the embodiment of the present invention. The embodiment of the present invention has all the advantages of the metal organic polyhedron, composite and ion exchange membrane, which will not be described in detail here. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 is a cross-sectional view of PEM-1 in Example 1 of the present invention. DETAILED DESCRIPTION

[0042] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to be used to explain the present invention, but should not be understood as limiting the present invention.

[0043] In this article, the term "metal-organic polyhedron", also known as "metal-organic cage" or "metal-organic cage compound", etc., can also be called "coordination polymer" or "coordination compound".

[0044] A composite according to an embodiment of the present invention comprises: an ion exchange resin and a metal organic polyhedron, wherein the metal organic polyhedron comprises cerium ions and an organic ligand, and the structural formula of the organic ligand is shown in formula (1):

[0045]

[0046] Wherein, Z in formula (1) is selected from the following structures:

[0047]

[0048] The composite of the embodiment of the present invention comprises an ion exchange resin and a metal organic polyhedron. The metal organic polyhedron has a special spatial structure and good solubility in a solvent. It can overcome the problem of uneven dispersion of cerium-based metal salts and metal oxides in the resin. The metal organic polyhedron is in a single molecule state in the solution, can be doped with the resin at the molecular level, and can enhance the interaction between the resin matrix, and has better performance than nano cerium salts. The cage of the metal organic polyhedron has a spatial structure of a specific size and an internal channel of a special cavity, which can allow a certain amount of small molecules to pass through, can adjust the ion transfer site and the sulfonate arrangement, and improve the electrochemical performance. The three-dimensional structure in the metal organic polyhedron is conducive to the conduction of protons, and prolongs the transmission path of gas and organic small molecules, can improve the conductivity and barrier properties of the material, and enhance the mechanical properties and electrochemical properties. The metal organic polyhedron of the present invention has structural diversity and controllable and adjustable structure, has great advantages in constructing proton transfer, and has broad application prospects. Introducing cerium ions into the composite in the form of metal organic polyhedrons can effectively avoid cross-linking contact between cerium ions and ionic groups of ion exchange polymers, such as sulfonic acid functional groups. The coordination center of the metal organic polyhedron is a cerium ion, which can act as a hydroxyl radical quencher and significantly improve the chemical stability, chemical durability and resistance to free radical attack of the composite.

[0049] In the embodiments of the present invention, the composite can also be used to prepare coatings, hydrogels and adhesives for porous membranes such as desalination membranes (nanofiltration membranes) and ultrafiltration / microfiltration membranes, as well as various fabrics and protective equipment in the fields of surgical gloves, protective clothing, sterile sheets, etc., and has a wide range of applications.

[0050] In some embodiments, the cerium ions include Ce 4+ In the embodiment of the present invention, the cerium ion is tetravalent.

[0051] In some embodiments, the topological structure of the metal organic polyhedron is a spatial three-dimensional structure; optionally, the metal organic polyhedron is a solid material. In the embodiments of the present invention, the organic ligands and cerium ions form a three-dimensional structure after coordination, which has a higher quenching efficiency for hydroxyl radicals, and the special spatial structure of the three-dimensional structure can enhance proton transfer and improve conductivity.

[0052] In some embodiments, Z is selected from the structures in Table 1:

[0053] Table 1

[0054]

[0055]

[0056] In some embodiments, the unit cell volume of the metal organic polyhedron is Specifically, for example, Preferably, In the embodiments of the present invention, the unit cell volume is a common parameter for describing the structural characteristics of metal organic polyhedrons, which is further beneficial to improving the electrical conductivity and barrier properties of the composite, and enhancing the mechanical properties and electrochemical properties.

[0057] In some embodiments, the method for preparing the metal organic polyhedron includes: dispersing a metal salt and an organic ligand in a solvent, and reacting to obtain the metal organic polyhedron;

[0058] Optionally, the metal salt is a cerium salt, and preferably, the cerium salt includes at least one of cerium nitrate hexahydrate, cerium trifluoromethanesulfonate, cerium sulfate, cerium chloride, cerium acetate, and cerium acetylacetonate;

[0059] Optionally, the molar ratio of the metal salt to the organic ligand is 1:1 to 1.5 (specifically, for example, 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5);

[0060] Optionally, the solvent includes at least one of acetonitrile, N,N dimethylformamide (DMF), dimethyl sulfoxide (DMSO), methanol, and ethanol;

[0061] Optionally, the metal salt and the organic ligand are dispersed in a solvent and stirred; the reaction temperature is 80-120°C, specifically, for example, 80°C, 90°C, 100°C, 110°C, 120°C; the reaction time is 12-24h, specifically, for example, 12h, 18h, 24h; the reaction is carried out under an inert atmosphere, preferably, the inert atmosphere is nitrogen; after the reaction, the mixture is cooled to room temperature, impurities after the reaction are filtered out, and metal organic polyhedrons are obtained.

[0062] In some embodiments, taking Z as a carbazole derivative group as an example, the preparation method of the carbazole derivative-based organic ligand is as follows:

[0063]

[0064] The method for preparing the carbazole derivative-based organic ligand comprises the following steps:

[0065] (1) Synthesis of Structural Formula 2

[0066] 20 mL of dry DMSO was added to a round-bottom flask, and 0.167 g of carbazole (1 mmol) and 100 μL of 4-fluoroacetophenone (0.83 mmol) were weighed and dissolved. After that, 7 g of anhydrous sodium carbonate and 150 mg of copper powder were added, and the temperature was slowly raised to 140°C for 72 hours. After the reaction was completed, the mixture was cooled to room temperature, extracted three times with 100 mL of ethyl acetate, and then washed with saturated brine three times. Finally, the organic phases were combined, dried with anhydrous sodium sulfate, and the solvent was removed by vacuum distillation to obtain a crude product, which was then purified with a silica gel column to obtain a light yellow solid structure 2.

[0067] (2) Synthesis of Structural Formula 3

[0068] Under water bath conditions, 57 mg of dichloromethane solution of structure 2 (0.19 mmol) was added dropwise to a flask containing 0.134 g AlCl3 (1 mmol) and acetyl chloride (7.25 mL). After 4 hours of reaction at room temperature, the reaction was completed. The mixture was extracted with dichloromethane several times, washed with sodium hydroxide solution and saturated saline solution several times, the dichloromethane organic phase was combined, dried with anhydrous sodium sulfate, filtered, and the crude product was purified by chromatography to obtain structure 3.

[0069] (3) Synthesis of Structural Formula 4

[0070] In an ice-water bath, 3 mL of liquid bromine was added to a flask containing 7 g of sodium hydroxide and 30 mL of deionized water, and the mixture was reacted at room temperature for two hours. Then, the 1,4-dioxane solution of structural formula 3 was slowly added, and the mixture was reacted at 50° for 3 hours. After the reaction, hydrochloric acid and sodium hypobromite were added in an ice-water bath, and the pH was adjusted to 1. The white structural formula 4 was obtained by recrystallization.

[0071] (4) Synthesis of Structural Formula 5

[0072] 20 mL of concentrated sulfuric acid was added dropwise to a methanol solution containing 0.375 g of structure 4, and the mixture was refluxed overnight. After the reaction was completed, the mixture was filtered and washed with water for several times to obtain structure 5.

[0073] (5) Synthesis of Structural Formula 6

[0074] 10 mL of 98% hydrazine hydrate and 50 mL of ethanol were added dropwise to a solution containing 2.98 g of the structural formula 5, and the mixture was refluxed overnight. After the reaction was completed, the mixture was washed with methanol for several times to obtain the structural formula 6.

[0075] (6) Synthesis of Structural Formula 7

[0076] 0.83 g of structure 6 and 0.88 g of salicylaldehyde (7.2 mmol) were weighed into a 100 mL flask, and 50 mL of methanol was added and stirred. Glacial acetic acid was added dropwise as a catalyst, and the reaction was carried out for 24 hours. After the reaction was completed, it was washed with methanol several times to obtain a yellow solid of structure 7, i.e., a carbazole derivative-based organic ligand.

[0077] The synthesis of the carbazole derivative-based ligand cerium-based metal organic polyhedron comprises the following steps:

[0078] Take 0.729 g (0.01 mmol) of structure 7 in a 50 mL beaker, add DMF solution to completely dissolve it, add 0.3 mmol of KOH 16.8 mg, and then add 43.4 mg of cerium nitrate hexahydrate, react overnight, filter after the reaction is completed, and slowly diffuse ether into the solution to obtain black block crystals, which are cerium-based metal organic polyhedrons.

[0079] In some embodiments, the composite comprises 95% to 99.99% (specifically, for example, 95%, 96%, 97%, 98%, 98.5%, 99%, 99.5%, 99.8%, 99.9%, 99.95%, 99.99%) of ion exchange resin and 0.01% to 5% (specifically, for example, 0.01%, 0.05%, 0.1%, 0.2%, 0.5%, 1%, 1.5%, 2%, 3%, 4%, 5%) of metal organic polyhedron, by mass.

[0080] In some embodiments, the ion exchange resin comprises at least one of perfluorosulfonic acid resin, perfluorosulfonimide resin, polyacid side chain perfluoro resin, sulfonated polytrifluorostyrene, sulfonated polysulfone, sulfonated polyethersulfone, sulfonated polyetheretherketone, sulfonated polyaryletherketone, sulfonated polyarylethernitrile, sulfonated polyphosphazene, sulfonated polyphenylene oxide, sulfonated polybenzonitrile, sulfonated polyimide or sulfonated polybenzimidazole; preferably, the ion exchange resin comprises at least one of perfluorosulfonic acid resin, perfluorosulfonimide resin, polyacid side chain perfluoro resin, sulfonated polytrifluorostyrene, sulfonated polyetheretherketone, sulfonated polyaryletherketone and sulfonated polyarylethernitrile; more preferably, the ion exchange resin comprises perfluorosulfonic acid resin;

[0081] Optionally, according to different cations, the perfluorosulfonic acid resin includes an acid-type perfluorosulfonic acid resin, an alkali metal-type perfluorosulfonic acid resin or other cationic perfluorosulfonic acid resin;

[0082] Wherein, the general structural formula of the acid-type perfluorosulfonic acid resin is:

[0083]

[0084] In the formula, m=0-6, n=2-5; x determines the ion exchange equivalent (EW) of the acid-type perfluorosulfonic acid resin, and y determines the molecular weight of the acid-type perfluorosulfonic acid resin;

[0085] The general structural formula of the alkali metal perfluorosulfonic acid resin or other cationic perfluorosulfonic acid resin is:

[0086]

[0087] In the formula, m=0-6, n=2-5, M is selected from at least one of lithium, sodium, potassium, rubidium, cesium or other cations; the other cations include at least one of ammonium ion, alkaline earth metal ion, iron ion, vanadium ion, titanium ion, cobalt ion, chromium ion, nickel ion, copper ion, aluminum ion, silver ion, zinc ion, manganese ion and tin ion; x determines the EW of the resin, and y determines the molecular weight of the resin.

[0088] A method for preparing a composite according to an embodiment of the present invention comprises: dispersing an ion exchange resin and a metal organic polyhedron in a solvent to obtain a dispersion, and then drying the dispersion to obtain a composite. In the embodiment of the present invention, the process is simple, easy to operate, and has high production efficiency, and is easy to be widely used in industrial production.

[0089] In some embodiments, the dispersion temperature is 10-240°C, specifically, for example, 10°C, 20°C, 25°C, 30°C, 50°C, 100°C, 200°C, 240°C; and / or the dispersion pressure is normal pressure to 20MPa, specifically, for example, normal pressure, 0.2MPa, 0.5MPa, 1MPa, 5MPa, 10MPa, 20MPa; and / or the dispersion time is 0.1-24h, specifically, for example, 0.1h, 0.5h, 1h, 6h, 12h, 24h.

[0090] In some embodiments, the solvent includes at least one of water, a high boiling point organic solvent, tetrahydrofuran, and a lower aliphatic alcohol; the high boiling point organic solvent includes at least one of ethylene glycol, propylene glycol, glycerol, DMF, DMAC, DMSO, hexamethylphosphoramide, and NMP; the lower aliphatic alcohol includes at least one of methanol, ethanol, isopropanol, and n-propanol.

[0091] In some embodiments, the ion exchange resin and the metal organic polyhedron are dispersed in a solvent, and after dispersion, a redispersion treatment is performed to obtain a dispersion; wherein the redispersion treatment includes at least one of stirring, shaking or ultrasound.

[0092] In some embodiments, the drying temperature is 20-180°C, specifically, for example, 20°C, 30°C, 50°C, 80°C, 100°C, 180°C.

[0093] An ion exchange membrane according to an embodiment of the present invention comprises: the composite according to an embodiment of the present invention or a composite prepared by the preparation method according to an embodiment of the present invention.

[0094] In the embodiment of the present invention, the ion exchange membrane has all the advantages of the composite material, which will not be described in detail here. The metal organic polyhedron has good solubility, can enhance the interaction between the ion exchange resin matrix, and thus has excellent film processing properties. The introduction of cerium ions through the metal nodes of the metal organic polyhedron can quench the free radicals generated during the operation of the ion exchange membrane, reduce the attack on the ion exchange membrane, and thus improve its mechanical properties. The introduction of metal organic polyhedron into the ion exchange membrane effectively improves the chemical stability, chemical durability, resistance to free radical attack, mechanical properties and electrochemical properties of the ion exchange membrane, thereby improving the comprehensive performance of the ion exchange membrane.

[0095] In some embodiments, the method comprises 95% to 99.99% (specifically, for example, 95%, 96%, 97%, 98%, 98.5%, 99%, 99.5%, 99.8%, 99.9%, 99.95%, 99.99%) of ion exchange resin and 0.01% to 5% (specifically, for example, 0.01%, 0.05%, 0.1%, 0.2%, 0.5%, 1%, 1.5%, 2%, 3%, 4%, 5%) of metal organic polyhedron, by mass.

[0096] In some embodiments, the ion exchange membrane has a thickness of 4 to 50 μm, specifically, for example, 4 μm, 5 μm, 10 μm, 20 μm, 30 μm, 50 μm; and / or the ion exchange capacity of the ion exchange membrane is 0.1 to 4.2 mmol / g, specifically, for example, 0.1 mmol / g, 1 mmol / g, 2 mmol / g, 3 mmol / g, 4 mmol / g, 4.2 mmol / g.

[0097] In some embodiments, the ion exchange membrane includes a reinforced membrane; preferably, the reinforced membrane is a porous membrane; the thickness of the reinforced membrane is 4 to 20 μm, specifically, for example, 4 μm, 5 μm, 10 μm, 20 μm; optionally, the reinforced membrane or its material includes at least one of porous PEEK mesh, ePTFE membrane, polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene copolymer, tetrafluoroethylene-propylene copolymer, ethylene-tetrafluoroethylene copolymer, tetrafluoroethylene-hexafluoropropylene-ethylene copolymer, polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, vinylidene fluoride-tetrafluoroethylene-hexafluoropropylene copolymer, and polyvinyl fluoride, preferably polytetrafluoroethylene.

[0098] A method for preparing an ion exchange membrane according to an embodiment of the present invention comprises the following steps:

[0099] (1) dispersing an ion exchange resin and a metal organic polyhedron in a solvent to obtain a dispersion;

[0100] (2) The dispersion is molded and then dried to obtain an ion exchange membrane.

[0101] In the embodiment of the present invention, the prepared ion exchange membrane has good flatness, uniform thickness distribution, simple process, easy operation, high production efficiency, and is easy to be widely used in industrial production. In addition, the dispersion in the preparation process can also be used to prepare coatings, hydrogels and adhesives for porous membranes such as desalination membranes (nanofiltration membranes), ultrafiltration membranes and microfiltration membranes, as well as various fabrics and protective equipment in the fields of surgical gloves, protective clothing, sterile sheets, etc.

[0102] In some embodiments, in the step (1), the dispersion temperature is 10 to 240°C, specifically, for example, 10°C, 20°C, 25°C, 30°C, 50°C, 100°C, 200°C, 240°C; and / or, in the step (1), the dispersion pressure is normal pressure to 20MPa, specifically, for example, normal pressure, 0.2MPa, 0.5MPa, 1MPa, 5MPa, 10MPa, 20MPa; and / or, in the step (1), the dispersion time is 0.1 to 24h, specifically, for example, 0.1h, 0.5h, 1h, 6h, 12h, 24h.

[0103] In some embodiments, in step (1), the solvent includes at least one of water, a high boiling point organic solvent, tetrahydrofuran, and a lower aliphatic alcohol; the high boiling point organic solvent includes at least one of ethylene glycol, propylene glycol, glycerol, DMF, DMAC, DMSO, hexamethylphosphoramide, and NMP; and the lower aliphatic alcohol includes at least one of methanol, ethanol, isopropanol, and n-propanol.

[0104] In some embodiments, in step (1), the ion exchange resin and the metal organic polyhedron are dispersed in a solvent, and after dispersion, a re-dispersion treatment is performed to obtain a dispersion; wherein the re-dispersion treatment includes at least one of stirring, shaking or ultrasound;

[0105] And / or, in the step (2), the forming comprises at least one of casting, pouring or coating;

[0106] And / or, the step (2) further comprises a reinforced membrane, wherein the dispersion is loaded on the reinforced membrane (on one side or both sides), and then dried to obtain an ion exchange membrane; the loading method comprises at least one of infiltration, blade coating, and slit coating;

[0107] And / or, in step (2), the drying temperature is 20-180°C, specifically, for example, 20°C, 30°C, 50°C, 80°C, 100°C, 180°C.

[0108] The application of a composite or ion exchange membrane in an embodiment of the present invention is used for at least one of batteries, chlor-alkali industry, water electrolysis hydrogen production, capacitors, electrodialysis, sensors, desalination membranes, ultrafiltration membranes, microfiltration membranes, fabrics, and protective equipment. In the embodiment of the present invention, all the advantages of the composite and ion exchange membrane are possessed, which will not be repeated here.

[0109] In some embodiments, at least one of the following is used for proton exchange membranes for fuel cells, liquid flow battery membranes, polyelectrolyte membranes for the chlor-alkali industry, proton exchange membranes for water electrolysis to produce hydrogen, acidic primary battery membranes, lithium battery membranes, polyelectrolytes in supercapacitors, and electrodialysis membranes for metal recovery.

[0110] A fuel cell according to an embodiment of the present invention comprises the composite or the ion exchange membrane according to an embodiment of the present invention. In the embodiment of the present invention, all advantages of the metal organic polyhedron, composite and ion exchange membrane are possessed, which will not be described in detail here.

[0111] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.

[0112] The cerium salts and compounds used in the examples of the present invention are from chemical reagent suppliers such as Aladdin, Macklin Reagent, Beide Pharmaceuticals, and Leyan Reagent. Perfluorosulfonic acid resins are from Chemours, 3M, and Solvay. Other solvents are common chemical reagents.

[0113] The test methods for conductivity, EW, IEC, tensile strength, elastic modulus, tensile strain at break, gas permeability, water absorption and swelling rate refer to "Proton Exchange Membrane Fuel Cell Part 3: Proton Exchange Membrane Test Methods". Among them, the test conditions for conductivity are 80℃ and relative humidity 95%.

[0114] Example 1: Preparation of Ce-based Metal-organic Polyhedron / Perfluorosulfonic Acid Resin Ion Exchange Membrane PEM-1 Where Z is a Carbazole Derivative

[0115] In the organic ligand of the cerium-based metal organic polyhedron, Z is a carbazole derivative group, and the cerium ion is Ce 4+ The single crystal structure analysis of the cerium-based metal organic polyhedron found that the carbazole derivative Ce-based crystal [6+6] structure has a window area of The cavity volume is The distance between the two cerium ions is

[0116] 10g of perfluorosulfonic acid resin (3M800 resin 3M Company, EW 800g / mol) and 20mg of metal organic polyhedron were dispersed in a solvent to obtain a dispersion liquid. The dispersion temperature was 120°C, the pressure was 2MPa, and the time was 12h. The perfluorosulfonic acid resin and the metal organic polyhedron were uniformly dissolved in a mixed solvent of propylene glycol:DMF:water with a volume ratio of 3:1:1 by stirring. It was configured into a mixed solution with a solid content of 15% and a viscosity of 40mPa·s.

[0117] Turn on the scraper and set the coating speed to 25cm / min, the scraper height to 11μm, place the A4-sized Daicel PET base film on the scraper, add 10mL of the above mixed solution, start the equipment to scrape the resin solution evenly, then cut the polytetrafluoroethylene membrane (ePTFE) to A4 size and cover it on the solution, wait for 5 minutes at room temperature to allow the solution to completely soak the ePTFE membrane. Reset the scraper height to 8μm, continue to add 8mL of the mixed solution at the same scraper speed, scrape once more, and place it in an oven at 160℃ for 10 minutes to remove the solvent, and obtain the ion exchange membrane PEM-1. Figure 1 is a cross-sectional view of PEM-1.

[0118] Example 2: Preparation of Ce-based Metal-organic Polyhedron / Perfluorosulfonic Acid Resin Ion Exchange Membrane PEM-2 Where Z is Phenyl

[0119] In the organic ligand of the cerium-based metal organic polyhedron, Z is a phenyl group, and the cerium ion is Ce 4+ The single crystal structure analysis of the cerium-based metal organic polyhedron found that the phenyl Ce-based crystal structure has a window area of Cavity volume The distance between two cerium ions

[0120] The preparation method is the same as that of Example 1, except that the metal-organic polyhedron uses a cerium-based metal-organic polyhedron in which Z is a phenyl group, to obtain an ion exchange membrane PEM-2.

[0121] Example 3: Preparation of Cerium-based Metal-organic Polyhedron / Perfluorosulfonic Acid Resin Ion Exchange Membrane PEM-3 Where Z is Triazine

[0122] In the organic ligand of the cerium-based metal organic polyhedron, Z is a triazine group, and the cerium ion is Ce 4+ The single crystal structure analysis of the cerium-based metal organic polyhedron found that the triazine Ce-based crystal structure has a window area of Cavity volume The distance between two cerium ions

[0123] The preparation method is the same as that of Example 1, except that the metal organic polyhedron adopts a cerium-based metal organic polyhedron in which Z is a triazine group, to obtain an ion exchange membrane PEM-3.

[0124] Example 4: Preparation of Cerium-based Metal-organic Polyhedron / Perfluorosulfonic Acid Resin Ion Exchange Membrane PEM-4 Where Z is Nitrogen

[0125] In the organic ligand of the cerium-based metal organic polyhedron, Z is a nitrogen group, and the cerium ion is Ce 4+ The single crystal structure analysis of the cerium-based metal organic polyhedron found that the nitrogen-based Ce-based crystal structure has a window area of Cavity volume The distance between two cerium ions

[0126] The preparation method is the same as that of Example 1, except that the metal-organic polyhedron adopts a cerium-based metal-organic polyhedron in which Z is a nitrogen group, to obtain an ion exchange membrane PEM-4.

[0127] Example 5: Preparation of Cerium-based Metal-organic Polyhedron / Perfluorosulfonic Acid Resin Ion Exchange Membrane PEM-5 Where Z is Meta-triphenyl Group

[0128] In the organic ligand of the cerium-based metal organic polyhedron, Z is a triphenyl group, and the cerium ion is Ce 4+ The single crystal structure analysis of the cerium-based metal organic polyhedron found that the meta-triphenylene Ce-based crystal structure has a window area of Cavity volume The distance between two cerium ions

[0129] The preparation method is the same as that of Example 1, except that the metal organic polyhedron adopts a cerium-based metal organic polyhedron in which Z is a triphenyl group as the main body, to obtain an ion exchange membrane PEM-5.

[0130] Example 6: Preparation of Cerium-based Metal-organic Polyhedron / Perfluorosulfonic Acid Resin Ion Exchange Membrane PEM-6 Where Z is Triphenylamine

[0131] In the organic ligand of the cerium-based metal organic polyhedron, Z is a triphenylamine group, and the cerium ion is Ce 4+ The single crystal structure analysis of the cerium-based metal organic polyhedron found that the triphenylamine Ce-based crystal structure has a window area of Cavity volume The distance between two cerium ions

[0132] The preparation method is the same as that of Example 1, except that the metal-organic polyhedron adopts a cerium-based metal-organic polyhedron in which Z is a triphenylamine group, to obtain an ion exchange membrane PEM-6.

[0133] Example 7: Preparation of Ce-based Metal-organic Polyhedron / Perfluorosulfonic Acid Resin Ion Exchange Membrane PEM-7 Where Z is 2,4,6-Triphenylazine

[0134] In the organic ligand of the cerium-based metal organic polyhedron, Z is a 2,4,6-triphenylazine group, and the cerium ion is Ce 4+ The single crystal structure analysis of the cerium-based metal organic polyhedron found that the 2,4,6-triphenyloxazine Ce-based crystal structure has a window area of Cavity volume The distance between two cerium ions

[0135] The preparation method is the same as that of Example 1, except that the metal organic polyhedron uses a cerium-based metal organic polyhedron in which Z is a 2,4,6 triphenylazine group to obtain an ion exchange membrane PEM-7.

[0136] Example 8: Preparation of Cerium-based Metal-organic Polyhedron / Perfluorosulfonic Acid Resin Ion Exchange Membrane PEM-8 Where Z is Fluorenyl

[0137] In the organic ligand of the cerium-based metal organic polyhedron, Z is a fluorene group, and the cerium ion is Ce 4+ The single crystal structure analysis of the cerium-based metal organic polyhedron found that the fluorene Ce-based crystal structure has a window area of Cavity volume The distance between two cerium ions

[0138] The preparation method is the same as that of Example 1, except that the metal organic polyhedron adopts a cerium-based metal organic polyhedron in which Z is a fluorene group, to obtain an ion exchange membrane PEM-8.

[0139] Example 9: Preparation of Ce-based Metal-organic Polyhedron / Perfluorosulfonic Acid Resin Ion Exchange Membrane PEM-9 Where Z is 1,3,5-Triphenylsulfonate Sodium Benzene

[0140] In the organic ligand of the cerium-based metal organic polyhedron, Z is 1,3,5-triphenylsulfonate sodium benzene, and the cerium ion is Ce 4+ The single crystal structure analysis of the cerium-based metal organic polyhedron found that the 1,3,5-triphenylsulfonate phenyl Ce-based crystal structure has a window area of Cavity volume The distance between two cerium ions

[0141] The preparation method is the same as that of Example 1, except that the metal organic polyhedron uses a cerium-based metal organic polyhedron in which Z is 1,3,5-triphenylsulfonate sodium-based benzene to obtain an ion exchange membrane PEM-9.

[0142] Example 10: Preparation of Ce-based Metal-organic Polyhedron / Perfluorosulfonic Acid Resin Ion Exchange Membrane PEM-10 Where Z is a 10-phenylnaphthalene Derivative

[0143] In the organic ligand of the cerium-based metal organic polyhedron, Z is a phenylnaphthalene derivative, and the cerium ion is Ce 4+ The single crystal structure analysis of the cerium-based metal organic polyhedron found that the phenylnaphthalene derivative Ce-based crystal structure has a window area of Cavity volume The distance between two cerium ions

[0144] The preparation method is the same as that of Example 1, except that the metal organic polyhedron uses a cerium-based metal organic polyhedron in which Z is a 10-phenylnaphthalene derivative, to obtain an ion exchange membrane PEM-10.

[0145] Example 11: Preparation of Ce-based Metal-organic Polyhedron / Perfluorosulfonic Acid Resin Ion Exchange Membrane Where Z is a Carbazole Derivative

[0146] The preparation method is the same as that of Example 1, except that the added amounts of the carbazole derivative-based cerium-based metal organic polyhedron are 1 mg, 5 mg, and 10 mg, respectively, to obtain ion exchange membranes PEM-11, PEM-12, and PEM-13, respectively.

[0147] Comparative Example 1: Preparation of ion exchange membrane D-PEM-1 without adding metal organic polyhedron

[0148] The preparation method is the same as that of Example 1, except that no metal organic polyhedron is added to obtain an ion exchange membrane D-PEM-1.

[0149] Table 2

[0150]

[0151] Free radical resistance of ion exchange membrane: The ion exchange membrane was immersed in Fenton's reagent at 80°C for 8 hours, and the mass loss and conductivity decay before and after immersion were compared. Preparation of Fenton's reagent: 0.1 mL of Fe with a molar concentration of 0.01 mol / L was added to 50 mL of 3% H2O2 solution. 2+The solution is the Fenton reagent, which is prepared and used immediately. The smaller the mass loss percentage of the ion exchange membrane after Fenton reagent treatment, the better the durability; the smaller the conductivity decay, the better the free radical resistance.

[0152] The ion exchange membranes prepared in Examples 1-10 and Comparative Example 1 were treated with Fenton's reagent. The mass loss after treatment is shown in Table 3.

[0153] Table 3

[0154]

[0155]

[0156] It can be seen from the data in Table 3 that, compared with Comparative Example 1, after doping with the cerium-based metal organic polyhedron compound, the free radical durability of the ion exchange membrane is significantly improved, and the mass loss of the ion exchange membrane is significantly reduced. Better free radical durability can enable it to have better safety and reliability in long-term operation.

[0157] The IEC, water absorption rate and mass loss of the ion exchange membranes after treatment with Fenton's reagent of the ion exchange membranes prepared in Example 1, Example 11 and Comparative Example 1 were tested. The results are shown in Table 4.

[0158] Table 4

[0159]

[0160] It can be seen from the data in Table 4 that after Example 11 is doped with a small amount of cerium-based metal organic polyhedron compound, the IEC and water absorption rate of the ion exchange membrane change little, and the free radical durability is improved; even the ion exchange membrane PEM-11 with a cerium-based metal organic polyhedron content of about 0.01% has a significantly reduced mass loss compared with D-PEM-1.

[0161] Table 5

[0162]

[0163]

[0164] It can be seen from the data in Table 5 that the electrochemical performance of the ion exchange membrane containing the cerium-based metal organic polyhedron has been greatly improved.

[0165] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0166] Although the above embodiments have been shown and described, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. Changes, modifications, substitutions and variations of the above embodiments by those of ordinary skill in the art are all within the scope of protection of the present invention.

Claims

1. A composite, It is characterized in that include: Ion exchange resin and metal organic polyhedron, the metal organic polyhedron includes cerium ions and organic ligands, and the structural formula of the organic ligand is shown in formula (1): Wherein, Z in formula (1) is selected from the following structures:

2. The complex according to claim 1, It is characterized in that The topological structure of the metal-organic polyhedron is a spatial three-dimensional structure; And / or, the unit cell volume of the metal organic polyhedron is and / or, the composite comprises 95% to 99.99% ion exchange resin and 0.01% to 5% metal organic polyhedron, by mass; And / or, the ion exchange resin comprises at least one of perfluorosulfonic acid resin, perfluorosulfonimide resin, polyacid side chain perfluoro resin, sulfonated polytrifluorostyrene, sulfonated polysulfone, sulfonated polyethersulfone, sulfonated polyetheretherketone, sulfonated polyaryletherketone, sulfonated polyarylethernitrile, sulfonated polyphosphazene, sulfonated polyphenylene oxide, sulfonated polybenzonitrile, sulfonated polyimide or sulfonated polybenzimidazole; And / or, the cerium ions include Ce 4+ .

3. A method for preparing the composite according to claim 1 or 2, It is characterized in that include: The ion exchange resin and the metal organic polyhedron are dispersed in a solvent to obtain a dispersion liquid, and then the dispersion liquid is dried to obtain a composite.

4. The method for preparing the composite according to claim 3, It is characterized in that The dispersion temperature is 10 to 240°C; And / or, the dispersion time is 0.1 to 24 hours; And / or, the drying temperature is 20-180°C.

5. An ion exchange membrane, It is characterized in that include: The complex according to claim 1 or 2 or the complex prepared by the preparation method according to claim 3 or 4.

6. The ion exchange membrane according to claim 5, It is characterized in that comprising 95% to 99.99% of ion exchange resin and 0.01% to 5% of metal organic polyhedron, by mass; And / or, the thickness of the ion exchange membrane is 4 to 50 μm; and / or, the ion exchange capacity of the ion exchange membrane is 0.1 to 4.2 mmol / g; And / or, the ion exchange membrane comprises a reinforced membrane.

7. A method for preparing the ion exchange membrane according to claim 5 or 6, It is characterized in that The following steps are involved: (1) dispersing an ion exchange resin and a metal organic polyhedron in a solvent to obtain a dispersion; (2) The dispersion is molded and then dried to obtain an ion exchange membrane.

8. The method for preparing the composite according to claim 7, It is characterized in that In the step (1), the dispersion temperature is 10 to 240°C; And / or, in the step (1), the dispersion time is 0.1 to 24 hours; And / or, in the step (2), the forming comprises at least one of casting, pouring or coating; And / or, the step (2) further comprises a reinforced membrane, wherein the dispersion is loaded on the reinforced membrane and then dried to obtain an ion exchange membrane; And / or, in the step (2), the drying temperature is 20 to 180°C.

9. Use of the composite according to claim 1 or 2 or the ion exchange membrane according to claim 5 or 6, It is characterized in that Used in at least one of batteries, chlor-alkali industry, water electrolysis to produce hydrogen, capacitors, electrodialysis, sensors, desalination membranes, ultrafiltration membranes, microfiltration membranes, fabrics, and protective equipment.

10. The use according to claim 9, It is characterized in that At least one of the following: proton exchange membranes for fuel cells, flow battery membranes, polyelectrolyte membranes for the chlor-alkali industry, proton exchange membranes for hydrogen production by water electrolysis, acidic primary battery membranes, lithium battery membranes, polyelectrolytes in supercapacitors, and electrodialysis membranes for metal recovery.

11. A fuel cell, It is characterized in that It comprises the composite according to claim 1 or 2 or the ion exchange membrane according to claim 5 or 6.