Preparation method of carbon fiber composite material and application of carbon fiber composite material in scooter
By surface-modifying carbon fiber and nano-alumina-loaded halloysite nanotube composite materials, the problem of interface compatibility between carbon fiber and nylon 6 is solved, which significantly improves the mechanical properties and wear resistance of the scooter pedal and extends its service life.
Patent Information
- Application Number
- CN202410851569.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-01
AI Technical Summary
The compatibility problem at the interface between existing carbon fiber and nylon 6 composite materials leads to a lack of performance, making it difficult to improve the mechanical properties and wear resistance of scooter pedals.
Surface-modified carbon fiber and halloysite nanotube composite material loaded with nano-alumina are used to improve the compatibility of carbon fiber and nylon 6 through functional agent 1 and 2, and the carbon fiber composite material is prepared through a feeder melt extrusion process. .
Significantly improves the mechanical properties and wear resistance of carbon fiber composite materials, extending the service life of the scooter.
Smart Images

Figure CN118725554A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite materials, and in particular to a method for preparing a carbon fiber composite material and application of the carbon fiber composite material in a scooter. Background Art
[0002] With the continuous development of science and technology, people's demand for transportation is also increasing, and modern transportation tools are becoming more and more diverse. Among the many means of transportation, scooters are favored by more and more people due to their convenience and flexibility. In order to meet consumers' dual demands for scooter performance and design, new technologies and new materials in the field of materials science are constantly being introduced into the manufacture of scooters.
[0003] Usually, the pedal of a scooter is made of polymer materials as the main body. Among many polymer materials, PA6 (nylon 6) is often used to make the pedal of a scooter due to its good mechanical properties, heat resistance and other comprehensive properties. In order to make the scooter have higher quality, it is often necessary to prepare a pedal material with better performance. Therefore, it is of great significance to enhance nylon 6.
[0004] In recent years, the composite material prepared by compounding carbon fiber with nylon 6 has the common advantages of both, so its application in the field of scooters has gradually increased. However, carbon fiber itself is an inorganic material, and the interface problem between it and nylon 6 is difficult to be effectively solved, which in turn causes the performance loss of the composite material, which is not conducive to improving product quality. Moreover, although nylon 6 itself has a certain wear resistance, it is difficult to maintain high performance under the high-frequency friction of the scooter pedal.
[0005] Based on this, the present invention provides a carbon fiber composite material, which has excellent mechanical properties and wear resistance and can be directly used as a pedal material for a scooter, so that the scooter has a long service life. Summary of the invention
[0006] 1. Technical issues to be resolved
[0007] In view of the deficiencies in the prior art, the present invention provides a method for preparing a carbon fiber composite material and application of the same in a scooter.
[0008] (II) Technical solution
[0009] A method for preparing a carbon fiber composite material, the carbon fiber composite material comprising the following components in parts by weight: 80-95 parts of PA6, 4-8 parts of functional agent 1, 3-4.5 parts of functional agent 2, 10-20 parts of a compatibilizer, 0.5-1.5 parts of an antioxidant, and 0.5-1 parts of a lubricant;
[0010] The preparation method comprises the following steps:
[0011] S1. Weigh each component according to weight and set aside;
[0012] S2. Place all raw materials in a mixer, control the temperature to 80-90°C, start stirring, mechanically stir at a speed of 1000-1500r / min for 20-30min, cool and discharge, and obtain a pre-mixed material;
[0013] S3, feeding the prepared material into a twin-screw extruder through a feeding port, controlling the temperature in the extruder to be 180-200° C., the screw speed to be 40-60 rpm, performing melt extrusion, pelletizing, and drying to obtain a carbon fiber composite material;
[0014] The compatibilizer is maleic anhydride grafted polypropylene.
[0015] Further preferably, the preparation method of the functional agent 1 comprises the following steps:
[0016] S10, immersing the carbon fiber in concentrated nitric acid and treating it at 80-100° C. for 1-3 hours, separating the material, and washing it thoroughly with deionized water until the washing liquid is neutral, thereby obtaining a carbon fiber oxidation material;
[0017] S20. Add the carbon fiber oxidation material into tetrahydrofuran, sonicate to form a uniform dispersion, then add trimesoyl chloride to the dispersion, stir at room temperature for 1-2 hours under nitrogen protection, then add the bridging monomer to the dispersion, and add a catalyst for catalysis, continue stirring for 6-9 hours, separate and collect the materials, wash and vacuum dry to obtain the functional agent 1.
[0018] Further preferably, in step S10, the length of the carbon fiber is 1-2 mm.
[0019] More preferably, in step S20, the bridging monomer is any one of diethanolamine, triethanolamine or pentaerythritol.
[0020] More preferably, in step S20, the catalyst is pyridine or triethylamine.
[0021] In the above technical scheme, after the carbon fiber is oxidized by concentrated nitric acid, a large number of active oxygen-containing groups such as hydroxyl groups will appear on the surface to form a carbon fiber oxide material, and then the carbon fiber oxide material is modified by trimesoyl chloride, and the acyl chloride groups are modified on the surface of the carbon fiber, and then the bridging monomer is used to condense with the acyl chloride groups. At the same time, the unreacted trimesoyl chloride in the system can undergo an uninterrupted condensation reaction with the bridging monomer, thereby forming a large number of polymer molecular chain coating layers on the surface of the carbon fiber to obtain a functional agent one.
[0022] Further preferably, the preparation method of the functional agent 2 comprises the following steps:
[0023] S100, adding N,N'-bis(2-hydroxyethyl)-N,N'-bis(trimethoxysilylpropyl)ethylenediamine to anhydrous toluene, mechanically mixing to form a uniform solution, then adding 1,2-epoxydodecane to the solution, and adding a phase transfer catalyst, then raising the temperature to 60-70°C, keeping the temperature for 4-6 hours under continuous stirring, cooling and discharging the material to obtain a bridging agent;
[0024] S200, ultrasonically disperse the halloysite nanotubes and nano-alumina in a 70% by volume ethanol solution to form a dispersion, then mix the bridging agent with deionized water, add acetic acid to adjust the pH to 3-4, stir and hydrolyze to form a hydrolyzate, then mix the hydrolyzate and the dispersion, ultrasonically treat for 4-8 hours at a temperature of 70-80°C, discharge the material, and collect the solid material.
[0025] More preferably, in step S100, the molar ratio of N,N'-bis(2-hydroxyethyl)-N,N'-bis(trimethoxysilylpropyl)ethylenediamine to 1,2-epoxydodecane is 1:1-2.
[0026] Further preferably, in step S100, the phase transfer catalyst is boron trifluoride etherate complex.
[0027] Further preferably, in step S200, the mass ratio of halloysite nanotubes to nano-alumina is 1:0.1-0.25.
[0028] In the above technical scheme, N,N'-bis(2-hydroxyethyl)-N,N'-bis(trimethoxysilylpropyl)ethylenediamine and 1,2-epoxydodecane are first used as raw materials. Under the action of a phase transfer catalyst, the active epoxy groups and active hydroxyl substituents between each other can undergo ring-opening addition to prepare a bridging agent. Since both ends of the bridging agent structure contain siloxane groups, after hydrolysis, they can condense with the hydroxyl groups on the surface of halloysite nanotubes and nano-alumina, thereby fixing the nano-alumina on the surface of the halloysite nanotubes to form halloysite nanotubes loaded with nano-alumina, that is, functional agent two.
[0029] An application of a carbon fiber composite material. The carbon fiber composite material prepared by the above preparation method is applied to a scooter.
[0030] (III) Beneficial technical effects
[0031] The functional agent prepared by the present invention is a carbon fiber with a large number of polymer molecular chains modified on the surface. These polymer molecular chains can form a "transition" layer between the carbon fiber and the nylon 6 matrix. The existence of this "transition" layer can effectively improve the compatibility between the nylon 6 matrix and the carbon fiber. Moreover, during the high-temperature melting process, these polymer molecular chains can extend to various regions of the nylon 6 matrix to form a micro-cross-linked network structure, thereby firmly riveting the carbon fiber in the nylon 6 matrix, greatly enhancing the interface bonding force between each other, so that the advantages of carbon fiber can be effectively exerted and the mechanical properties of nylon 6 can be enhanced.
[0032] The second functional agent prepared by the present invention is halloysite nanotubes loaded with nano-alumina. Since the bridging agent structure contains long fatty chains, it has good lubrication effect, which can make the nano-alumina slide relatively on the surface of the halloysite nanotubes, produce a "ball" effect, and effectively improve the wear resistance of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0034] Figure 1 This is the scanning electron microscope image of functional agent 2. DETAILED DESCRIPTION
[0035] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. Preferred embodiments of the present invention are given below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0036] Example 1
[0037] A carbon fiber composite material comprises the following components in parts by weight: 80 parts of PA6, 4 parts of functional agent 1, 3 parts of functional agent 2, 10 parts of compatibilizer maleic anhydride grafted polypropylene, 0.5 parts of antioxidant 1010, and 0.5 parts of lubricant stearic acid;
[0038] The method for preparing the carbon fiber composite material comprises the following steps:
[0039] S1. Weigh each component according to weight and set aside;
[0040] S2. Place all raw materials in a mixer, control the temperature to 80°C, start stirring, mechanically stir at a speed of 1000r / min for 30min, cool and discharge, and obtain a pre-mixed material;
[0041] S3. Feed the prepared material into a twin-screw extruder through a feeding port, control the temperature in the extruder to 180° C., and the screw speed to 50 rpm, perform melt extrusion, pelletize, and dry to obtain a carbon fiber composite material.
[0042] The preparation method of the functional agent 1 comprises the following steps:
[0043] S10, immersing a carbon fiber having a length of 1 mm in concentrated nitric acid having a mass fraction of 69%, and treating the carbon fiber at 100° C. for 2 h, separating the material, and washing the material with deionized water until the washing liquid is neutral, thereby obtaining a carbon fiber oxidation material;
[0044] S20. Add 3.5 g of carbon fiber oxide to tetrahydrofuran, and perform ultrasound to form a uniform dispersion. Then add 1.2 g of trimesoyl chloride to the dispersion. After stirring at room temperature for 1 h under nitrogen protection, add 2 g of triethanolamine to the dispersion, and add 0.3 g of triethylamine for catalysis. After continuing to stir for 8 h, separate and collect the materials, wash and vacuum dry to obtain functional agent 1.
[0045] The functional agent 1 was titrated and tested by soap back titration method to analyze the ester group content. The test results showed that the ester group content of the functional agent 1 was 6.182 mmol / g. Therefore, the polymer molecular chain on the surface of the carbon fiber was a polyester polymer molecular chain.
[0046] The preparation method of the functional agent 2 comprises the following steps:
[0047] S100, adding 0.3 g of N,N'-bis(2-hydroxyethyl)-N,N'-bis(trimethoxysilylpropyl)ethylenediamine to anhydrous toluene, mechanically mixing to form a uniform solution, then adding 0.2 g of 1,2-epoxydodecane to the solution, and adding 0.01 g of boron trifluoride ether complex, and then raising the temperature to 65°C, keeping the temperature for 5 hours under continuous stirring, cooling and discharging the material to obtain a bridging agent;
[0048] S200, ultrasonically disperse 1.2g of halloysite nanotubes and 0.2g of nano-alumina in 80mL of 70% by volume ethanol and solution to form a dispersion, then mix 1.5g of a bridging agent with 20mL of deionized water, add acetic acid to adjust the pH to 3, stir and hydrolyze to form a hydrolyzate, then mix the hydrolyzate and the dispersion, ultrasonicate at 75°C for 6h, discharge the material, and collect the solid material.
[0049] Figure 1This is the scanning electron microscope image of functional agent 2. It can be seen that a large number of nanoparticles are densely dispersed on the surface of the carbon fiber. Analysis shows that the spherical nanoparticles are nano-alumina.
[0050] Example 2
[0051] A carbon fiber composite material comprises the following components in parts by weight: 90 parts of PA6, 6 parts of functional agent 1, 4 parts of functional agent 2, 15 parts of compatibilizer maleic anhydride grafted polypropylene, 1 part of antioxidant 1010, and 0.6 parts of lubricant stearic acid;
[0052] The method for preparing the carbon fiber composite material comprises the following steps:
[0053] S1. Weigh each component according to weight and set aside;
[0054] S2. Place all raw materials in a mixer, control the temperature to 90°C, start stirring, mechanically stir at a speed of 1500r / min for 25min, cool and discharge, and obtain a pre-mixed material;
[0055] S3. Feed the prepared material into a twin-screw extruder through a feeding port, control the temperature in the extruder to 190° C., and the screw speed to 50 rpm, perform melt extrusion, pelletize, and dry to obtain a carbon fiber composite material.
[0056] The preparation methods of the functional agent 1 and the functional agent 2 are the same as those in Example 1.
[0057] Example 3
[0058] A carbon fiber composite material comprises the following components in parts by weight: 95 parts of PA6, 8 parts of functional agent 1, 4.5 parts of functional agent 2, 20 parts of compatibilizer maleic anhydride grafted polypropylene, 1.5 parts of antioxidant 1010, and 1 part of lubricant stearic acid;
[0059] The method for preparing the carbon fiber composite material comprises the following steps:
[0060] S1. Weigh each component according to weight and set aside;
[0061] S2. Place all raw materials in a mixer, control the temperature to 90°C, start stirring, mechanically stir at a speed of 1500r / min for 20min, cool and discharge, and obtain a pre-mixed material;
[0062] S3. Feed the prepared material into a twin-screw extruder through a feeding port, control the temperature in the extruder to 200° C., and the screw speed to 50 rpm, perform melt extrusion, pelletize, and dry to obtain a carbon fiber composite material.
[0063] The preparation methods of the functional agent 1 and the functional agent 2 are the same as those in Example 1.
[0064] Comparative Example 1
[0065] A carbon fiber composite material comprises the following components in parts by weight: 90 parts of PA6, 6 parts of functional agent 1, 15 parts of compatibilizer maleic anhydride grafted polypropylene, 1 part of antioxidant 1010, and 0.6 parts of lubricant stearic acid;
[0066] The method for preparing the carbon fiber composite material comprises the following steps:
[0067] S1. Weigh each component according to weight and set aside;
[0068] S2. Place all raw materials in a mixer, control the temperature to 90°C, start stirring, mechanically stir at a speed of 1500r / min for 25min, cool and discharge, and obtain a pre-mixed material;
[0069] S3. Feed the prepared material into a twin-screw extruder through a feeding port, control the temperature in the extruder to 190° C., and the screw speed to 50 rpm, perform melt extrusion, pelletize, and dry to obtain a carbon fiber composite material.
[0070] The preparation method of the functional agent 1 is the same as that of Example 1.
[0071] Comparative Example 2
[0072] A carbon fiber composite material comprises the following components in parts by weight: 90 parts of PA6, 6 parts of carbon fiber, 4 parts of functional agent II, 15 parts of compatibilizer maleic anhydride grafted polypropylene, 1 part of antioxidant 1010, and 0.6 parts of lubricant stearic acid;
[0073] The method for preparing the carbon fiber composite material comprises the following steps:
[0074] S1. Weigh each component according to weight and set aside;
[0075] S2. Place all raw materials in a mixer, control the temperature to 90°C, start stirring, mechanically stir at a speed of 1500r / min for 25min, cool and discharge, and obtain a pre-mixed material;
[0076] S3. Feed the prepared material into a twin-screw extruder through a feeding port, control the temperature in the extruder to 190° C., and the screw speed to 50 rpm, perform melt extrusion, pelletize, and dry to obtain a carbon fiber composite material.
[0077] The preparation method of the functional agent 2 is the same as that of Example 1.
[0078] Comparative Example 3
[0079] A carbon fiber composite material comprises the following components in parts by weight: 90 parts of PA6, 4 parts of functional agent II, 15 parts of compatibilizer maleic anhydride grafted polypropylene, 1 part of antioxidant 1010, and 0.6 parts of lubricant stearic acid;
[0080] The method for preparing the carbon fiber composite material comprises the following steps:
[0081] S1. Weigh each component according to weight and set aside;
[0082] S2. Place all raw materials in a mixer, control the temperature to 90°C, start stirring, mechanically stir at a speed of 1500r / min for 25min, cool and discharge, and obtain a pre-mixed material;
[0083] S3. Feed the prepared material into a twin-screw extruder through a feeding port, control the temperature in the extruder to 190° C., and the screw speed to 50 rpm, perform melt extrusion, pelletize, and dry to obtain a carbon fiber composite material.
[0084] The preparation method of the functional agent 2 is the same as that of Example 1.
[0085] Test Case
[0086] Examples 1 to 3 and Comparative Example 3 were made into samples of corresponding sizes, and tensile properties were tested according to standard GB / T1040.2-2022;
[0087] According to the standard GB / T 9341-2008, tensile properties test was carried out;
[0088] According to the standard GB / T 3960-2016, the test load force was set to 1000N and the rotation speed was set to 0.43m / s to test the friction coefficient of the plastic and evaluate the wear resistance of the sample;
[0089] The test results are shown in the table below:
[0090] project Tensile strength / MPa Bending strength / MPa Friction coefficient Example 1 109.4 160.3 0.142 Example 2 111.0 162.1 0.138 Example 3 109.8 161.6 0.161 Comparative Example 1 108.9 158.8 0.412 Comparative Example 2 96.1 137.0 0.152 Comparative Example 3 79.5 97.1 0.149
[0091] It is obvious from the analysis and test that the carbon fiber composite material made with functional agent 1 and functional agent 2 as additives has significantly better mechanical properties, a lower friction coefficient and better wear resistance. After removing functional agent 2, the wear resistance of the composite material is significantly reduced. After replacing functional agent 1 with untreated carbon fiber, the mechanical properties are significantly reduced. This is due to the interface problem that makes it impossible to efficiently exert the performance of carbon fiber.
[0092] Based on the ideal embodiment of the present invention, through the above description, relevant personnel can make various changes and modifications without departing from the technical concept of the present invention. The technical scope of the present invention is not limited to the content in the specification, and the technical scope must be determined according to the scope of the claims.
Claims
1. A method for preparing a carbon fiber composite material, characterized in that: The carbon fiber composite material comprises the following components in parts by weight: 80-95 parts of PA6, 4-8 parts of functional agent 1, 3-4.5 parts of functional agent 2, 10-20 parts of compatibilizer, 0.5-1.5 parts of antioxidant, and 0.5-1 part of lubricant; The preparation method comprises the following steps: S1. Weigh each component according to weight and set aside; S2. Place all raw materials in a mixer, control the temperature to 80-90°C, start stirring, mechanically stir at a speed of 1000-1500r / min for 20-30min, cool and discharge, and obtain a pre-mixed material; S3, feeding the prepared material into a twin-screw extruder through a feeding port, controlling the temperature in the extruder to be 180-200° C., the screw speed to be 40-60 rpm, performing melt extrusion, pelletizing, and drying to obtain a carbon fiber composite material; The compatibilizer is maleic anhydride grafted polypropylene.
2. The method for preparing a carbon fiber composite material according to claim 1, characterized in that: The preparation method of the functional agent 1 comprises the following steps: S10, immersing the carbon fiber in concentrated nitric acid and treating it at 80-100° C. for 1-3 hours, separating the material, and washing it thoroughly with deionized water until the washing liquid is neutral, thereby obtaining a carbon fiber oxidation material; S20. Add the carbon fiber oxidation material into tetrahydrofuran, sonicate to form a uniform dispersion, then add trimesoyl chloride to the dispersion, stir at room temperature for 1-2 hours under nitrogen protection, then add the bridging monomer to the dispersion, and add a catalyst for catalysis, continue stirring for 6-9 hours, separate and collect the materials, wash and vacuum dry to obtain the functional agent 1.
3. The method for preparing a carbon fiber composite material according to claim 2, characterized in that: In the step S10, the length of the carbon fiber is 1-2 mm.
4. The method for preparing a carbon fiber composite material according to claim 2, characterized in that: In the step S20, the bridging monomer is any one of diethanolamine, triethanolamine or pentaerythritol.
5. The method for preparing a carbon fiber composite material according to claim 2, characterized in that: In the step S20, the catalyst is pyridine or triethylamine.
6. The method for preparing a carbon fiber composite material according to claim 1, characterized in that: The preparation method of the functional agent 2 comprises the following steps: S100, adding N,N'-bis(2-hydroxyethyl)-N,N'-bis(trimethoxysilylpropyl)ethylenediamine to anhydrous toluene, mechanically mixing to form a uniform solution, then adding 1,2-epoxydodecane to the solution, and adding a phase transfer catalyst, then raising the temperature to 60-70°C, keeping the temperature for 4-6 hours under continuous stirring, cooling and discharging the material to obtain a bridging agent; S200, ultrasonically disperse the halloysite nanotubes and nano-alumina in a 70% by volume ethanol solution to form a dispersion, then mix the bridging agent with deionized water, add acetic acid to adjust the pH to 3-4, stir and hydrolyze to form a hydrolyzate, then mix the hydrolyzate and the dispersion, ultrasonically treat for 4-8 hours at a temperature of 70-80°C, discharge the material, and collect the solid material.
7. The method for preparing a carbon fiber composite material according to claim 1, characterized in that: In the step S100, the molar ratio of N,N'-bis(2-hydroxyethyl)-N,N'-bis(trimethoxysilylpropyl)ethylenediamine to 1,2-epoxydodecane is 1:1-2.
8. The method for preparing a carbon fiber composite material according to claim 1, characterized in that: In the step S100, the phase transfer catalyst is boron trifluoride etherate complex.
9. The method for preparing a carbon fiber composite material according to claim 1, characterized in that: In the step S200, the mass ratio of the halloysite nanotubes to the nano-alumina is 1:0.1-0.
25.
10. An application of a carbon fiber composite material, characterized in that: The carbon fiber composite material prepared by the preparation method as claimed in claim 1 is applied to a scooter.
Citation Information
Patent Citations
Carbon fiber reinforced nylon material as well as preparation raw material, preparation method and application thereof
CN110041700A
Automotive carbon fiber reinforced nylon composite material and preparation method thereof
CN114921094A
Low-temperature toughened and modified nylon 6 composite material and preparation method thereof
CN117343535A
Low-linear-expansion polyamide resin composition and polyamide resin molding composed of the same
JP2017210544A
Joined body
US20190276720A1
Cited By
High-voltage vacuum insulating part material and preparation method thereof
CN119432060A