Zinc-rich coating as well as preparation method and application thereof
The zinc-rich coating composed of modified zinc powder and nano-ZnO particles solves the problem of toxic chromate and high cost in Dacromet coating, and achieves a non-toxic, corrosion-resistant and antibacterial coating suitable for use in marine environments. Anti-corrosion of metal substrates simplifies the preparation process and reduces costs.
Patent Information
- Application Number
- CN202410768415.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-14
AI Technical Summary
Existing Dacromet paints contain toxic hexavalent chromic anhydride that volatilizes under marine conditions, which endangers human health and marine ecology. The preparation process is complex and costly, and it is ineffective against marine microbial corrosion.
The zinc-rich coating is composed of modified zinc powder, acrylic resin varnish, aluminum powder and nano-ZnO particles. The zinc powder is modified by sodium molybdate, trisodium phosphate and sodium acetate to increase the adhesion and corrosion resistance of the coating. And the antibacterial function is enhanced through nano-ZnO particles, which simplifies the preparation process and reduces costs.
It achieves a non-toxic, corrosion-resistant and antibacterial coating, reduces construction costs, improves the comprehensive protective performance under seawater immersion test, and is suitable for anti-corrosion of metal substrates in marine environments.
Smart Images

Figure BDA0004893321430000081 
Figure HDA0004893321450000011 
Figure HDA0004893321450000012
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of anti-corrosion coatings, relates to zinc-rich coatings, and particularly relates to a zinc-rich coating and a preparation method and application thereof. Background Art
[0002] The economic losses caused by the corrosion of steel materials account for about 2-3% of the gross national product of various countries, of which one-third comes from marine corrosion. Corrosive media such as marine atmosphere, seawater and microorganisms can cause serious corrosion damage to the surface of marine steel components, and 20% of this corrosion is caused by microorganisms. Microbial corrosion has been recognized as an important form of corrosion damage to metal structures such as marine ships, oil platforms and submarine pipelines. Preparing a protective coating on the surface of a metal substrate is one of the simplest and most effective means to deal with marine corrosion.
[0003] At present, the surface of metal components in marine working conditions is often anti-corrosion by coating anti-fouling and anti-corrosion coatings. Since the raw materials of Dacromet coatings are cheap, they can not only be coated on various complex parts, but also have the advantages of no hydrogen embrittlement, good heat resistance and corrosion resistance, they have been widely used in marine working conditions. Traditional Dacromet coatings are anti-corrosion coatings with zinc powder, aluminum powder, chromate and deionized water as the main components, which makes the Dacromet coating itself have some serious defects. On the one hand, although most Dacromet coatings on the market can meet the use standards, the toxic hexavalent chromium anhydride left in the coatings is difficult to avoid volatilization during service, which will still cause major safety hazards to human health and the marine ecological environment; on the other hand, in the process of coating Dacromet coatings, the surface of the component substrate needs to be pre-treated, and then the Dacromet coating can be prepared on the surface through spraying-baking-secondary spraying-baking-drying process. Its preparation process is complicated and costly, and ordinary Dacromet coatings have no obvious inhibitory effect on marine microbial corrosion. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a zinc-rich coating and a preparation method and application thereof. The zinc-rich coating of the present invention has good adhesion, flexibility and corrosion resistance, and the coating does not contain toxic chromate substances, which can effectively reduce the pollution to the marine ecological environment; at the same time, after adding a specific proportion of nano ZnO particles to the coating, the comprehensive protective performance of the coating under the seawater immersion test is better, and the preparation process of the coating of the present invention is simple and can effectively reduce the construction cost.
[0005] The technical solution of the present invention is achieved in this way:
[0006] A zinc-rich paint comprises 20-40 parts of modified zinc powder, 55-60 parts of acrylic resin varnish, 4-6 parts of aluminum powder, 2-6 parts of nano particles, 0.3-0.5 parts of dispersant, and 0.2-0.5 parts of defoamer.
[0007] The modified zinc powder is obtained by modifying zinc powder with a modifying liquid, wherein the modifying liquid comprises sodium molybdate, trisodium phosphate, sodium acetate and deionized water.
[0008] The acrylic resin varnish consists of acrylic resin powder, ethyl acetate and xylene.
[0009] Furthermore, the mass volume ratio of sodium molybdate, trisodium phosphate, sodium acetate and deionized water in the modified liquid is 5-7g:3-5g:2-4g:100mL.
[0010] Furthermore, the mass ratio of zinc powder to sodium molybdate is 2 to 3:1.
[0011] Furthermore, the mass ratio of acrylic resin powder, ethyl acetate and xylene is 2-3:3-5:4-6.
[0012] Furthermore, the nanoparticles are nano ZnO particles, and the particle size thereof is 30±10 nm; the zinc powder and aluminum powder are flaky, and the particle size thereof is 30±10 μm.
[0013] Furthermore, the dispersant is Tween 20 (polysorbate 20); and the defoaming agent is one of silicone oil or organosilicon defoaming agents.
[0014] The above-mentioned method for preparing a zinc-rich coating comprises the following steps:
[0015] (1) dissolving sodium molybdate, trisodium phosphate and sodium acetate in deionized water, adding nitric acid to adjust the pH to 7.2±0.1 after they are completely dissolved, then adding zinc powder, stirring magnetically until the solution turns light blue, and then filtering and drying to obtain modified zinc powder;
[0016] (2) uniformly mixing acrylic resin powder, ethyl acetate and xylene to obtain acrylic resin varnish;
[0017] (3) adding the modified zinc powder, aluminum powder and nanoparticles into acrylic resin varnish and stirring and mixing, and then adding a dispersant and a defoamer and mixing evenly to obtain the zinc-rich coating.
[0018] Furthermore, in step (1), the powder is ground and sieved after drying to obtain uniformly dispersed modified zinc powder.
[0019] The above-mentioned application of a zinc-rich coating in the anti-corrosion of steel component substrates is as follows: after the substrate surface is pre-treated by metallographic sandpaper grinding to 400 mesh and cleaning and degreasing, the zinc-rich coating is directly applied to the substrate surface, and after natural ventilation and curing, an anti-corrosion coating is obtained on the substrate surface.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1. The present invention uses sodium molybdate, trisodium phosphate and sodium acetate to modify zinc powder. Sodium molybdate can activate the surface of filler zinc powder, which is beneficial to improve the adhesion between zinc-rich coating and metal substrate. At the same time, the molybdenum compound generated by the reaction of molybdate and zinc powder in the coating can enhance the corrosion resistance of the coating; trisodium phosphate has a certain corrosion inhibition effect, can form a protective film, slow down the corrosion rate of the coating, and trisodium phosphate reacts with zinc powder to generate some insoluble phosphorus compounds, which further improves the corrosion resistance of the coating. In addition, trisodium phosphate has an auxiliary effect, which can adjust the film-forming speed of the coating and the structure of the coating; sodium acetate can enhance the wettability and fluidity of the coating liquid, so that the coating is more evenly distributed on the surface of the substrate, which is beneficial to improve the stability and durability of the coating. Therefore, sodium molybdate, trisodium phosphate and sodium acetate cooperate with each other to greatly improve the corrosion resistance of the coating, and the present invention further improves the comprehensive anti-corrosion performance of the zinc-rich coating under actual working conditions by adjusting the specific gravity of acrylic resin varnish in the coating to compare the corrosion protection effect of the coating sample.
[0022] 2. The present invention adds nano ZnO particles to the zinc-rich coating. On the one hand, the nano particles will fill the pores of the zinc powder and aluminum powder modified by the zinc-rich coating, thereby improving the compactness of the zinc-rich coating, and then effectively preventing the corrosive medium from penetrating into the substrate; on the other hand, the nano ZnO itself has an antibacterial function, which can effectively hinder the attachment of microorganisms to the zinc-rich coating, and fundamentally reduce the possibility of corrosion damage caused by marine microorganisms. At the same time, the zinc particles in the coating will release Zn with a strong bactericidal effect after activation. 2+ This can kill attached bacteria and further enhance the microbial corrosion protection effect of the zinc-rich coating. Therefore, the zinc-rich coating of the present invention is particularly suitable for anti-corrosion engineering of metal substrates in marine environments.
[0023] 3. The zinc-rich coating of the present invention does not contain toxic chromate substances, is eco-friendly, and can be prepared at room temperature (25±3°C). After being cured by ventilation at room temperature, an anti-corrosion coating can be obtained. The preparation cost is low and the construction is relatively simple. According to the test, the coating can be directly applied to the surface of the polished and cleaned test-grade tinplate sheet and AH36 hull steel substrate. The basic performance of the obtained zinc-rich coating sample is good, and it also has good corrosion resistance in seawater. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1-SEM images of Example 1 before and after zinc powder modification.
[0025] Figure 2 -EDS graph of Example 1 before and after zinc powder modification.
[0026] Figure 3 -XRD pattern of modified zinc powder of Example 1.
[0027] Figure 4 -Surface and cross-sectional micromorphology of the anti-corrosion coating obtained in Example 1 and Comparative Example 1.
[0028] Figure 5 -Anti-corrosion coating adhesion test diagram obtained from Example 1, Comparative Example 5 and Comparative Example 6.
[0029] Figure 6 -Results of the anti-corrosion coatings obtained in Example 1 and Comparative Example 6 resisting neutral salt spray for 1000 hours.
[0030] Figure 7 - SEM images of the anti-corrosion coatings obtained in Example 1 and Comparative Example 1 after being immersed in seawater solution for 30 days.
[0031] Figure 8 - EIS spectra of the anti-corrosion coatings obtained in Examples 1 to 5 and Comparative Example 1 after being immersed in seawater solution for 30 days.
[0032] Fig. 9 - Polarization curves of the anti-corrosion coatings obtained in Examples 1 to 5 and Comparative Example 1 after being in a seawater solution for 30 days. DETAILED DESCRIPTION
[0033] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0034] Example 1
[0035] 1) Preparation of modified zinc powder
[0036] 32.35g of sodium molybdate, 20.85g of trisodium phosphate, 13.05g of sodium acetate and 500mL of deionized water were mixed and stirred evenly. After they were completely dissolved, nitric acid was added dropwise to control the pH of the modified solution at 7.2±0.1. Then 80.21g of flaky zinc powder (particle size of about 20-40μm) was weighed and added to the modified solution. Finally, it was stirred at high speed in a magnetic stirrer to make it completely modified. After 10 minutes, the solution gradually turned into light blue, and then it was filtered with a vacuum pump. After filtering, it was placed in an oven at 80℃ for drying. Then the modified zinc powder after grinding and drying was sieved out through a 100-mesh standard sample sieve and sealed for use. The grinding here is mainly to disperse the modified zinc powder that has agglomerated into large particles, and the sieving is to exclude the modified zinc powder that has agglomerated large particles.
[0037] 2) Preparation of acrylic resin varnish
[0038] 50.14 g of acrylic resin powder, 92.55 g of ethyl acetate and 107.55 g of xylene solution were sequentially poured into a beaker and mixed and stirred to obtain acrylic resin varnish after dissolving by stirring.
[0039] 3) Preparation of anti-corrosion coating
[0040] At room temperature, 30.43g of modified zinc powder, 60g of acrylic resin varnish, 5.07g of aluminum powder, 0.3g of Tween 20, 0.2g of BYK-024 defoamer and 4g of nano ZnO were mixed, and the coating liquid was filtered after high-speed stirring and dispersion for 10 minutes. It was applied to the surface of the iron substrate with a 2# soft wool brush, and the zinc-rich anti-corrosion coating was obtained after natural curing in a ventilated place for 48 hours.
[0041] The purpose of filtering the prepared coating liquid is to ensure the purity of the coating liquid and remove some impurities such as sand particles, foreign matter, etc. In addition, insufficient stirring of the zinc-rich coating of the present invention may produce some larger agglomerated particles. If these impurities are not filtered out, uneven defects will be formed on the surface of the coating, affecting the aesthetics and overall quality of the product.
[0042] Example 2
[0043] This embodiment is the same as embodiment 1, except that in step 3), the modified zinc powder is 32.15 g, the aluminum powder is 5.35 g, and the nano ZnO is 2 g.
[0044] Example 3
[0045] This embodiment is the same as embodiment 1, except that in step 3), the modified zinc powder is 31.29 g, the aluminum powder is 5.21 g, and the nano ZnO is 3 g.
[0046] Example 4
[0047] This embodiment is the same as embodiment 1, except that in step 3), the modified zinc powder is 29.57 g, the aluminum powder is 4.93 g, and the nano ZnO is 5 g.
[0048] Example 5
[0049] This embodiment is the same as embodiment 1, except that in step 3), the modified zinc powder is 28.71 g, the aluminum powder is 4.79 g, and the nano ZnO is 6 g.
[0050] Comparative Example 1
[0051] This embodiment is the same as embodiment 1, except that in step 3), the amount of modified zinc powder is 33.86 g, the amount of aluminum powder is 5.64 g, and the amount of nano ZnO is 0 g.
[0052] Comparative Example 2
[0053] This embodiment is the same as embodiment 1, except that sodium tungstate is used instead of sodium molybdate in step 1).
[0054] Comparative Example 3
[0055] This embodiment is the same as embodiment 1, except that sodium dihydrogen phosphate is used instead of trisodium phosphate in step 1).
[0056] Comparative Example 4
[0057] This embodiment is the same as embodiment 1, except that trisodium citrate is used instead of sodium acetate in step 1).
[0058] Comparative Example 5
[0059] This embodiment is the same as embodiment 1, except that in step 3), 4 g of nano-Al2O3 is used to replace 4 g of nano-ZnO particles (the particle sizes of both nano-particles are 30±10 nm).
[0060] Comparative Example 6
[0061] This embodiment is the same as embodiment 3, except that in step 3), the amount of acrylic resin varnish is 50 g.
[0062] Comparative Example 7
[0063] This embodiment is the same as embodiment 3, except that in step 3), the amount of acrylic resin varnish is 65 g.
[0064] Comparative Example 8
[0065] This embodiment is the same as embodiment 3, except that in step 3), the amount of acrylic resin varnish is 70 g.
[0066] 1. The SEM images of zinc powder before and after modification in Example 1 are as follows: Figure 1 (a) Figure 1 As shown in (b), the surface of the unmodified zinc powder is smooth and has no obvious attachments, while the surface of the modified zinc powder (modified zinc powder) is rough and has small particles attached. Figure 2 and Figure 3 As shown, the results show that zinc powder reacts with the modified liquid to generate substances such as Zn3Mo3O3 and Zn4(PO4)2OH2(H2O)3, which are chemically adsorbed on the surface of flaky zinc powder.
[0067] 2. The surface and cross-sectional microscopic morphologies of the anticorrosive coatings obtained in Example 1 and Comparative Example 1 are shown in Figure 4 As shown, Figure 4 (a) and 4(c) are comparative examples 1, Figure 4 (b) and 4 (d) are examples 1, wherein Figure 4It can be seen that the surface of the coating without adding nano ZnO particles is loose, while the nano ZnO particles added in Example 1 fill the pores in the coating, making the surface and cross section of the prepared coating denser and tighter, thereby more effectively preventing the corrosive medium from penetrating into the substrate to corrode the substrate.
[0068] 3. The coatings prepared in the above embodiments and comparative examples were applied on the surface of AH36 hull steel coupons and test-grade tinplate sheets (polished to 400 meshes step by step). After the coatings were cured, the macroscopic appearance was smooth and flat, and no bubble defects occurred. The basic performance of the zinc-rich coatings prepared in the above embodiments 1-5 and comparative examples 1-8 was further tested, and the coating adhesion and neutral salt spray resistance tests were performed on the AH36 hull steel coupons, and the coating flexibility test was performed on the test-grade tinplate sheets. The coating adhesion is evaluated according to the GB / T9286-1998 test standard by detecting the integrity of the coating in the grid by the cross-cutting method. The index of the present invention requires that the adhesion level is ≤1 level; the flexibility is tested according to GB / T 1731-2020, and the coating sample is pressed tightly on the rod shaft of the flexibility tester, and the rod shaft diameter is gradually reduced to observe whether cracks and shedding occur. The index of the present invention requires ≤3mm; the salt spray resistance is tested according to GB / T 1771-2007, and the macroscopic morphology of the surface of each group of coating samples corroded by neutral salt spray is photographed and recorded every 24 hours. The index of the present invention requires that the time for the first red rust point to appear is ≥1000h. The test results are shown in Table 1.
[0069] Table 1. Test results of basic properties of zinc-rich coating
[0070] Example Average thickness / μm Flexibility / mm Adhesion / Grade Neutral salt spray resistance / 1000h Example 1 47 2 0 pass Example 2 51 2 0 pass Example 3 45 2 0 pass Example 4 49 2 0 pass Example 5 42 2 0 pass Comparative Example 1 47 3 1 pass Comparative Example 2 52 2 1 pass Comparative Example 3 49 2 1 pass Comparative Example 4 59 2 1 pass Comparative Example 5 55 3 1 pass Comparative Example 6 47 3 2 Failed Comparative Example 7 52 2 1 pass Comparative Example 8 51 2 1 pass
[0071] It can be seen from Table 1 that: (1) the coating prepared by the present invention is suitable for brushing, and the average thickness of the obtained coating is 50±10 μm; and the acrylic resin varnish prepared in Examples 1 to 5 of the present invention accounts for 60% and is added with nano ZnO. The coating has excellent basic properties, good adhesion, high flexibility, and strong salt spray resistance. By comparing Comparative Examples 2 to 4 with Example 1, it can be seen that replacing any component of the modifying liquid to modify the zinc powder will lead to a decrease in the adhesion of the coating, indicating that there is a synergistic effect between sodium molybdate, trisodium phosphate and sodium acetate to improve the adhesion between the coating and the metal substrate. At the same time, by comparing Comparative Examples 6 to 8 with Example 1, it can be seen that the proportion of acrylic resin varnish in the coating will also affect the adhesion of the coating.
[0072] The thickness of the coating samples prepared in 13 systems such as Examples 1 to 5 and Comparative Examples 1 to 8 is 50±10μm, which is suitable for brushing. The results of the coating sample flexibility test show that the shaft rod diameter of the coating samples of Examples 1 to 5, Comparative Examples 2 to 4 and 7 to 8 systems without cracks is 2mm, and the flexibility is good, while the flexibility of the coating samples of Comparative Examples 1, 5 and 6 is poor, indicating that the specific gravity of the acrylic resin varnish in the coating of the present invention is 60% and the addition of nano ZnO particles will make the flexibility of the zinc-rich coating better, but the use of nano Al2O3 particles instead of nano ZnO will reduce the flexibility of the coating.
[0073] The coating samples of Example 1, Comparative Example 5 and Comparative Example 6 are used as representatives to show the adhesion test results of the three levels of the present invention. Figure 5 As shown, Figure 5 (c) is embodiment 1, Figure 5 (b) is Comparative Example 5, Figure 5 (a) is comparative example 6. It can be seen from the figure that the scratch of the sample of Example 1 is smooth and there is basically no coating shedding around it, which is rated as level 0 according to the standard; a small amount of coating shedding around the scratch of the sample of comparative example 5, the shedding area is less than 5%, and it is rated as level 1 according to the standard; the coating shedding around the scratch of comparative example 6, the shedding area is greater than 5% but less than 15%, and it is rated as level 2 according to the standard, indicating that the addition of nano ZnO will make the coating better combined with the iron substrate surface and the coating adhesion is better.
[0074] The results of the anti-corrosion coatings obtained in Example 1 and Comparative Example 6 resisting neutral salt spray for 1000 hours are shown in the figure below: Figure 6 As shown, Figure 6 (a) is Comparative Example 6, Figure 6 (b) is Example 1. Under the accelerated corrosion test of the coating sample in the salt spray chamber, due to the cathodic protection effect of the coating, the zinc-aluminum powder and nano ZnO in the coating will be corroded preferentially. The corrosion products generated by the zinc-aluminum powder will move to the damaged area of the coating, covering the damaged area on the surface of the coating, so that the coating continues to play a physical shielding role; but as the corrosion time increases, the surface of the coating prepared in Comparative Example 6 with a lower specific gravity of acrylic resin varnish loses its physical shielding effect, cathodic protection effect and self-repairing effect, causing the substrate to suffer corrosion. The coating of Comparative Example 6 has formed red rust spots at a test time lower than 1000h. Subsequently, the corrosive medium causes the corrosion area to expand through the corrosion defects on the surface of the coating. At 1000h, a large area of red rust spots is formed, causing the coating to be damaged and fail, so the neutral salt spray test is shown as failed; while the zinc-rich coating prepared in Example 1 with a specific gravity of 60% of acrylic resin varnish is still flat and smooth with a certain metallic luster after 1000h of corrosion, and the corrosion resistance of the coating is greatly improved, and the neutral salt spray test is shown as passed.
[0075] 4. Using natural seawater rich in bacteria as the corrosion solution, the six groups of modified zinc-rich coating samples (substrate is AH36 hull steel) prepared in Examples 1 to 5 and Comparative Example 1 were subjected to a 30-day immersion corrosion test. The SEM images of the zinc-rich coating coupon samples obtained in Example 1 and Comparative Example 1 after 30 days in the seawater solution are shown in Figure 7, where Figure 7 (a) is Comparative Example 1, Figure 7 (b) is Example 1. It can be seen from the figure that after the anti-corrosion coating sample obtained in Comparative Example 1 was immersed in seawater solution for 30 days, the zinc powder layer on the surface of the coating was activated and dissolved over a large area, and obvious corrosion pits appeared; while the anti-corrosion coating sample obtained in Example 1 was corroded, the surface zinc powder layer had a small activation area, and the surface structure was still relatively intact and flat. Comparing the microscopic corrosion morphology of the two samples, it was found that the coating after adding nano ZnO showed better corrosion resistance in seawater corrosion solution, and had better protection performance against corrosive media, and the improvement of the corrosion resistance of the coating also increased the service life of the coating. This is because the nano ZnO itself has antibacterial properties and its interaction with metal ions will form a protective film on the surface of the filler, thereby reducing the corrosion of the coating surface by microorganisms in seawater and further improving the oxidation resistance and corrosion resistance of the coating. Since nano ZnO has a high surface energy, it is easy to agglomerate when it is added in an organic coating in excessive amounts to reduce energy, thereby losing the characteristics of nano particles. Therefore, it is particularly critical to determine the proportion of nano ZnO added to the coating of the present invention to achieve the best protective performance of the coating. In order to explore the optimal addition ratio of nano ZnO in the coating, the corrosion resistance of each group of coating samples was further evaluated by a three-electrode electrochemical test system. The experimental results are shown in Table 2. The EIS spectra and polarization curves of the anti-corrosion coatings obtained in Examples 1 to 5 and Comparative Example 1 are shown in Table 2. Figure 8 and Fig. 9 shown.
[0076] Table 2. Electrochemical performance test results of the anticorrosion coatings obtained in Examples 1 to 5 and Comparative Example 1
[0077]
[0078] Note: In this work, the threshold value of the open circuit potential (OCP) of the coating cathodic protection is generally selected as the valve potential of the steel substrate cathodic protection effect -0.86V (vs. SCE). When the OCP value is lower than the valve potential, the cathodic protection effect is "passed", and when the OCP value is higher than the valve potential, it is "failed". From the electrochemical performance test results of each group of coatings in Table 2, it can be seen that the open circuit potentials of Examples 1 to 5 and Comparative Example 1 within 30 days are all lower than the valve potential, indicating that the cathodic protection effect of the six groups of coating samples is passed; at the same time, the low-frequency impedance modulus values of the coating samples prepared under the systems of Examples 1 to 5 are greater than those of Comparative Example 1 in the seawater solution environment, and the Nyqusit capacitive reactance arc radius of the sample of Example 1 is the largest, the low-frequency impedance modulus value is the largest, and the corrosion current density obtained by fitting the polarization curve is the smallest. If the amount of nano ZnO added in the coating is further increased, the anti-corrosion performance of the coating will decrease. The electrochemical results show that the corrosion protection effect of the 4% nano ZnO zinc-rich coating in the present invention has reached the best. Considering the high cost of the coating nano ZnO filler, it is more economical and practical to use the zinc-rich coating prepared in Example 1 of the present invention for seawater corrosion protection of metal surfaces.
[0079] Finally, it should be noted that the above embodiments of the present invention are only examples for illustrating the present invention, and are not intended to limit the implementation methods of the present invention. For those skilled in the art, other different forms of changes and modifications can be made based on the above description. It is impossible to list all implementation methods here. Any obvious changes or modifications derived from the technical solution of the present invention are still within the scope of protection of the present invention.
Claims
1. A zinc-rich coating, It is characterized in that It includes 20 to 40 parts of modified zinc powder, 55 to 60 parts of acrylic resin varnish, 4 to 6 parts of aluminum powder, 2 to 6 parts of nanoparticles; 0.3 to 0.5 parts of dispersant; 0.2 to 0.5 parts of defoamer; The modified zinc powder is obtained by modifying zinc powder with a modifying liquid, wherein the modifying liquid comprises sodium molybdate, trisodium phosphate, sodium acetate and deionized water; The acrylic resin varnish consists of acrylic resin powder, ethyl acetate and xylene.
2. A zinc-rich coating according to claim 1, It is characterized in that The mass volume ratio of sodium molybdate, trisodium phosphate, sodium acetate and deionized water in the modified liquid is 5-7g:3-5g:2-4g:100mL.
3. A zinc-rich coating according to claim 1 or 2, It is characterized in that The mass ratio of zinc powder to sodium molybdate is 2-3:
1.
4. A zinc-rich coating according to claim 1 or 2, It is characterized in that The mass ratio of acrylic resin powder, ethyl acetate and xylene is 2-3:3-5:4-6.
5. A zinc-rich coating according to claim 1, It is characterized in that The zinc powder and aluminum powder are in the form of scales, and their particle sizes are both 30±10 μm; the nanoparticles are nano ZnO, and their particle size is 30±10 nm.
6. A zinc-rich coating according to claim 1, It is characterized in that The dispersant is Tween 20; the defoaming agent is one of silicone oil or organosilicon defoaming agents.
7. A method for preparing a zinc-rich coating according to any one of claims 1 to 6, It is characterized in that The following steps are involved: (1) dissolving sodium molybdate, trisodium phosphate and sodium acetate in deionized water, adding nitric acid to adjust the pH to 7.2±0.1 after they are completely dissolved, then adding zinc powder, stirring magnetically until the solution turns light blue, and then filtering and drying to obtain modified zinc powder; (2) uniformly mixing acrylic resin powder, ethyl acetate and xylene to obtain acrylic resin varnish; (3) Adding the modified zinc powder, aluminum powder and nanoparticles into acrylic resin varnish and stirring to mix, and then adding a dispersant and a defoamer and mixing evenly to obtain the zinc-rich coating.
8. A method for preparing a zinc-rich coating according to claim 7, It is characterized in that In step (1), the powder is dried and then ground and sieved to obtain uniformly dispersed modified zinc powder.
9. Use of a zinc-rich coating as claimed in any one of claims 1 to 6 in the corrosion protection of steel component substrates.
10. Application of a zinc-rich coating according to claim 9, It is characterized in that After the substrate surface is pre-treated by grinding with metallographic sandpaper to 400 mesh and cleaning and degreasing, the zinc-rich paint is directly applied to the substrate surface, and after natural ventilation and curing, an anti-corrosion coating is obtained on the substrate surface.
Citation Information
Patent Citations
Efficient zinc-rich coating added with aluminum powder and rare earth element and preparation method thereof
CN103013254A
Chromium-free fingerprint-resistant coating solution and preparation method of hot-dip aluminizing zinc plate
CN105038437A
Preparation methods of coating solution with high corrosion resistance and hot-dipped aluminum-zinc plate with finger resistance
CN105062239A
Method for preparing modified zinc-enriched anti-corrosion coating
CN106634295A
Chromium-free passivation method for zinc powder
CN114592186A