Glass wool adhesive and preparation method thereof

By using different types of coupling agents in glass wool adhesives to form chemical bonds, the problems of sticky adhesives at high temperatures and large usage are solved, the strength and service life of glass wool are improved, and better Bonding effect and mechanical properties.

CN118725751APending Publication Date: 2024-10-01QINGYUAN HANJIANG GLASSWOOL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411022062.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing glass wool adhesives tend to become sticky at high temperatures, causing the glass wool to deform, and the amount of adhesive used is large, which affects the strength and service life of the glass wool.

Method used

Different types of coupling agents are added to the glass wool adhesive, such as silane coupling agents, titanate coupling agents and aluminate coupling agents, to form chemical bonds with inorganic and organic materials through reactive functional groups to improve interfacial adhesion. Knot strength, reduce the amount of adhesive added and improve the overall strength of glass wool.

Benefits of technology

By forming chemical bonds, the interfacial adhesion of glass wool is improved, the amount of adhesive used is reduced, the strength and service life of glass wool are improved, and the problem of thermal deformation is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004967574470000031
    Figure BDA0004967574470000031
  • Figure BDA0004967574470000051
    Figure BDA0004967574470000051
  • Figure BDA0004967574470000061
    Figure BDA0004967574470000061
Patent Text Reader

Abstract

The invention belongs to the technical field of glass wool preparation, and discloses a glass wool adhesive. Comprising 6 to 10 parts of acrylic acid, 0.5 to 2 parts of a foaming agent, 20 to 25 parts of hydroxyethyl acrylate, 1 to 3 parts of sodium hypophosphite, 1 to 2 parts of sodium persulfate, 30 to 60 parts of an acrylic copolymer aqueous solution, 3 to 5 parts of chlorinated trimethyl aminopropyl methacrylamide, 1 to 2 parts of diallyl phthalate, 0.5 to 3 parts of a coupling agent and 10 to 15 parts of deionized water. Wherein the coupling agent is selected from at least one of a silane coupling agent, a titanate coupling agent, an aluminate coupling agent, a phosphate coupling agent and a zirconate coupling agent, and through the design, the overall strength of the glass wool cannot be lost or even is improved to a certain extent while the addition amount of the adhesive is reduced in the actual application process. The invention further discloses a preparation method for preparing the glass wool adhesive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of glass wool preparation, and in particular to a glass wool adhesive and a preparation method thereof. Background Art

[0002] Glass wool is an inorganic thermal insulation material and an important member in the field of thermal insulation materials. It not only has excellent properties such as non-flammability, low thermal conductivity, and good chemical stability, but can also be compounded or deeply processed with other materials to expand the application field of the product. Glass wool products have been increasingly widely used in construction, metallurgy, petroleum, chemical industry, national defense and military industries and high-tech industries, and have played an important role in the development of the national economy. However, glass wool is relatively brittle and generally has low mechanical strength. It is easy for cellulose to break after long-term use. At the same time, glass wool is an insulation material with a low thermal conductivity relative to other raw materials. There is an adhesive on the surface of the glass wool, and the adhesive is easy to become sticky when heated and even cause the glass wool to deform. Therefore, when using glass wool as an insulation layer, in order not to affect the use effect and service life of the glass wool, it is of great significance to reduce the amount of adhesive used and improve the adhesive's bonding ability to the glass wool.

[0003] Chinese patent application 201810900384.0 discloses a method for preparing high-strength and high-temperature resistant glass wool, firstly, waste glass, calcite, nano-alumina, borax, carbon nanotubes, calcium oxide, magnesium silicate, and titanium dioxide are used to prepare glass liquid, and then the glass liquid is placed in a glass wool centrifuge for centrifugal blowing to obtain glass fiber, and the glass wool adhesive is evenly sprayed on the surface of the glass fiber, and then the glass fiber is collected by a cotton collector and transported to a curing furnace for curing to obtain glass wool. The glass wool prepared by this scheme has good mechanical strength. According to the value of the elongation at break, it can be seen that the glass wool has good elasticity, thereby preventing the problem of thermal deformation caused by sudden temperature changes. The thermal conductivity of the glass wool is as low as 0.007w / mk, which shows that the glass wool has good thermal conductivity and prevents the glass wool from overheating and affecting the use effect and service life;

[0004] Further observation of the scheme shows that although the scheme uses a glass wool adhesive and discloses a preparation method of the glass wool adhesive, and the preparation method is specifically:

[0005] (1) dispersing 10 to 30 parts of white carbon black, 6 to 15 parts of aluminum borate whiskers, 6 to 12 parts of magnesium borate whiskers, and 8 to 16 parts of mica powder in 80 to 100 parts of 0.01 M PBS buffer at pH 7.4, then adding a silane coupling agent with a final concentration of 10 to 20 wt%, stirring and reacting at a temperature of 35 to 50° C. and a speed of 200 to 500 r / min for 1 to 2 hours; removing the upper layer solvent by centrifugation, washing the lower layer precipitated particles with deionized water for 2 to 3 times, and drying them in an oven for standby use;

[0006] (2) Add 4 to 7 parts of dispersant to 60 to 80 parts of solvent, and add 30 to 50 parts of nano-SiO 2 Modified boron phenolic resin, 12-18 parts of phenolic epoxy vinyl ester, 10-15 parts of bisphenol A epoxy vinyl ester, 8-14 parts of polyarylether ether nitrile, 5-10 parts of bismaleimide, raise the temperature to 50-60°C under vacuum, continue stirring to react for 1.5-3h, then add 5-8 parts of hexamethylenetetramine and 6-12 parts of 4,4'-diaminodiphenylmethane and continue stirring for 40-60min to obtain an adhesive for glass wool;

[0007] It can be seen that although the scheme discloses the use of a silane coupling agent, it does not disclose which specific silane coupling agent is used, nor does it attempt to use other types of coupling agents.

[0008] Chinese patent application 201810789515.2 A method for preparing an anti-corrosion high-adhesion glass wool adhesive comprises the following steps: S1. preparing samarium nitrate;

[0009] S2. Preparation of samarium nitrate modified nano-silica;

[0010] S3. Preparing a formaldehyde solution of nano-silica;

[0011] S4. Preparation of silica-modified phenolic resin;

[0012] S5. Weigh the following ingredients by weight: 40 to 50 parts of silica-modified phenolic resin, 1 to 3 parts of amino-modified silicone oil, 6 to 12 parts of titanate coupling agent, 5 to 10 parts of diesel, 3 to 8 parts of olive oil, 5 to 15 parts of carboxyl-terminated nitrile rubber toughened modified epoxy resin, and 5 to 10 parts of polyvinyl alcohol;

[0013] S6. The components in each weight portion in step S5 are heated, stirred and mixed uniformly;

[0014] It can be seen from step 5 of the scheme that, while adding the phenolic resin, the scheme also adds a certain amount of titanate coupling agent. However, further observation of the embodiments of the scheme shows that the scheme does not disclose the specific amount of titanate coupling agent used.

[0015] The technical problem to be solved by this solution is: how to provide a glass fiber adhesive that can improve the strength of glass fibers. Summary of the invention

[0016] The purpose of the present invention is to provide a glass fiber adhesive capable of improving the strength of glass fibers. By adding a coupling agent to the glass wool adhesive, since the coupling agent contains two or more reactive functional groups, one functional group reacts with an inorganic material, and the other functional group reacts with an organic material, thereby forming a chemical bond between the two materials (adhesive and glass fiber) to improve the interfacial bonding force, thereby achieving the goal of reducing the amount of adhesive added while achieving the overall strength of the glass wool without loss or even improving it to a certain extent;

[0017] Another object of the present application is to provide a preparation method for preparing the above-mentioned glass fiber adhesive.

[0018] To achieve the above object, the present application discloses a glass wool adhesive, which comprises the following components by weight:

[0019]

[0020] The coupling agent is selected from at least one of a silane coupling agent, a titanate coupling agent, an aluminate coupling agent, a phosphate coupling agent, and a zirconate coupling agent.

[0021] Preferably, the coupling agent at least comprises a silane coupling agent.

[0022] Preferably, the silane coupling agent is selected from at least one of methacryloxypropyltrimethoxysilane, methacryloxypropyltriisopropoxysilane, methacryloxypropylphenyldimethoxysilane, mercaptopropyltrimethoxysilane, mercaptopropylmethyldimethoxysilane and mercaptopropyltriisopropoxysilane.

[0023] Preferably, the silane coupling agent is a mixture of methacryloxypropyltrimethoxysilane and mercaptopropyltrimethoxysilane, and the mass ratio of methacryloxypropyltrimethoxysilane to mercaptopropyltrimethoxysilane is 2 to 4:1.

[0024] Preferably, the coupling agent is a mixture of a silane coupling agent, a titanate coupling agent and an aluminate coupling agent, and the mass ratio of the silane coupling agent, the titanate coupling agent and the aluminate coupling agent is 1 to 3:1:1.

[0025] Preferably, the titanate coupling agent is selected from at least one of tetraisopropoxytitanium, tetraethoxytitanium, tetra-n-butoxytitanium and tetra-n-propoxytitanium.

[0026] Preferably, the aluminate coupling agent is selected from at least one of triisopropoxyaluminum, triethoxyaluminum, tri-n-butoxyaluminum, and tri-n-propoxyaluminum.

[0027] Preferably, the mass fraction of acrylic acid in the aqueous solution of the acrylic copolymer is 36-38 wt %, and the number average molecular weight of the acrylic copolymer is 800-1000.

[0028] Preferably, the foaming agent is oxalic acid or oxalate.

[0029] In addition, the present application also discloses a preparation method for the above-mentioned glass wool adhesive, which comprises mixing acrylic acid, a foaming agent, hydroxyethyl acrylate, sodium hypophosphite, sodium persulfate, an aqueous solution of an acrylic copolymer, trimethylaminopropyl methacrylamide chloride, diallyl phthalate, a coupling agent, and deionized water, and reacting the mixture at 50 to 60° C. and normal pressure for 1 to 2 hours to obtain a glass wool adhesive.

[0030] The beneficial effects of this application are:

[0031] The present application adds a coupling agent to the glass wool adhesive. Since the coupling agent contains two or more reactive functional groups, one functional group reacts with inorganic materials and the other functional group reacts with organic materials, thereby forming a chemical bond between the two materials (adhesive and glass fiber) to improve the interfacial bonding strength. In this way, the overall strength of the glass wool will not be lost and may even be improved while reducing the amount of adhesive added. DETAILED DESCRIPTION

[0032] The present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. In the description of the present invention, it should be noted that, if no specific conditions are specified in the embodiments, the conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0033] Before the examples are presented, the following necessary description is first given of the preparation method of the glass wool adhesive:

[0034] A method for preparing a glass wool adhesive comprises mixing acrylic acid, a foaming agent, hydroxyethyl acrylate, sodium hypophosphite, sodium persulfate, an aqueous solution of an acrylic copolymer, trimethylaminopropyl methacrylamide chloride, diallyl phthalate, a coupling agent and deionized water, and reacting the mixture at 55° C. and normal pressure for 2 hours to obtain the glass wool adhesive.

[0035] The supplier information of the raw materials involved in the examples and comparative examples is shown in Table 1:

[0036] Table 1

[0037]

[0038] Embodiments 1 to 4

[0039] A glass wool adhesive, the formula of which is shown in Table 2:

[0040] Table 2

[0041]

[0042] It should be noted that in Examples 1 to 4, the mass fraction of acrylic acid in the aqueous solution of the acrylic copolymer is 36wt%, 37wt%, 38wt% and 36wt%, respectively, and the number average molecular weight of the acrylic copolymer is 800, 900, 1000 and 800, respectively.

[0043] Example 5

[0044] The method is substantially the same as Example 1, except that the methacryloxypropyltrimethoxysilane is replaced with the same mass fraction of mercaptopropyltrimethoxysilane.

[0045] Example 6

[0046] It is basically the same as Example 1, except that a mixture of methacryloxypropyltrimethoxysilane and mercaptopropyltrimethoxysilane in equal parts by mass is used to replace methacryloxypropyltrimethoxysilane, and in the mixture, the mass ratio of methacryloxypropyltrimethoxysilane to mercaptopropyltrimethoxysilane is 3:1.

[0047] Example 7

[0048] It is basically the same as Example 1, except that a mixture of methacryloxypropyltrimethoxysilane and mercaptopropyltrimethoxysilane in equal parts by mass is used to replace methacryloxypropyltrimethoxysilane, and in the mixture, the mass ratio of methacryloxypropyltrimethoxysilane to mercaptopropyltrimethoxysilane is 5:1.

[0049] Example 8

[0050] The method is substantially the same as Example 1, except that the methacryloxypropyltrimethoxysilane is replaced by tetraisopropoxytitanium in the same mass fraction.

[0051] Example 9

[0052] The method is basically the same as Example 1, except that the methacryloxypropyltrimethoxysilane is replaced by triisopropoxyaluminum in the same mass fraction.

[0053] Example 10

[0054] It is basically the same as Example 1, except that a mixture of methacryloxypropyltrimethoxysilane, mercaptopropyltrimethoxysilane, tetraisopropoxytitanium and triisopropoxyaluminum is used to replace methacryloxypropyltrimethoxysilane, and the mass ratio of methacryloxypropyltrimethoxysilane, mercaptopropyltrimethoxysilane, tetraisopropoxytitanium and triisopropoxyaluminum in the mixture is 2.25:0.75:1:1.

[0055] Embodiment 11

[0056] It is basically the same as Example 1, except that a mixture of methacryloxypropyl trimethoxysilane, mercaptopropyl trimethoxysilane, diisopropoxydiethoxytitanium, and diisopropoxyethoxyaluminum is used to replace methacryloxypropyl trimethoxysilane, and the mass ratio of methacryloxypropyl trimethoxysilane, mercaptopropyl trimethoxysilane, diisopropoxydiethoxytitanium, and diisopropoxyethoxyaluminum in the mixture is 2.25:0.75:1:1.

[0057] Example 12

[0058] The method is substantially the same as Example 6, except that the mass fraction of acrylic acid in the aqueous solution of the acrylic acid copolymer is 37 wt %, and the number average molecular weight of the acrylic acid copolymer is 900.

[0059] Embodiment 13

[0060] The method is substantially the same as Example 6, except that the mass fraction of acrylic acid in the acrylic acid copolymer aqueous solution is 37 wt %, and the number average molecular weight of the acrylic acid copolymer is 1000.

[0061] Embodiment 14

[0062] The method is substantially the same as Example 6, except that the mass fraction of acrylic acid in the acrylic copolymer aqueous solution is 37 wt %, and the number average molecular weight of the acrylic copolymer is 800.

[0063] Comparative Examples 1 to 5

[0064] An adhesive, the formula of which is shown in Table 3:

[0065] Table 3

[0066]

[0067] Performance Testing:

[0068] 1. Viscosity is measured using a Tu-4 cup.

[0069] 2. Yellowing resistance: Take 4g of the sample of the above embodiment in a culture dish, place it in a vacuum drying oven at 60℃ for 24 hours to remove moisture, and then react it in a muffle furnace at 200℃ for 5 minutes. Observe whether the cured adhesive turns yellow;

[0070] 3. Water resistance: Prepare the sample as in Test 2. After curing and cooling to room temperature, add water to the culture dish to submerge the adhesive, soak for 24 hours, and observe the changes in the adhesive after soaking.

[0071] 4. Bubble forming ability: Prepare samples as in Test 2. Observe the condition of bubbles formed after curing (bubble size and quantity).

[0072] 5. Tensile strength: Take the sample of the above embodiment and fill the sample preparation mold, place it in a vacuum drying oven at 60°C for 24 hours to remove water; repeat the above steps until the reactants fill the mold after removing water; react in a muffle furnace at 200°C for 5 minutes, demold after cooling and measure. The test results are shown in Table 3:

[0073] Table 3

[0074] Group Viscosity / s Yellowing Water resistance Bubble formation conditions Tensile strength / psi Example 1 23 No yellowing No change Large and few bubbles 43 Example 2 22 No yellowing No change Large and few bubbles 42 Example 3 22 No yellowing No change Large and few bubbles 43 Example 4 24 No yellowing No change Large and few bubbles 44 Example 5 21 No yellowing No change Large and few bubbles 42 Example 6 24 No yellowing No change Large and few bubbles 48 Example 7 22 No yellowing No change Large and few bubbles 45 Example 8 23 No yellowing No change Large and few bubbles 42 Example 9 22 No yellowing No change Large and few bubbles 41 Example 10 24 No yellowing No change Large and few bubbles 52 Embodiment 11 23 No yellowing No change Large and few bubbles 43 Example 12 24 No yellowing No change Large and few bubbles 45 Embodiment 13 26 No yellowing No change Large and few bubbles 42 Embodiment 14 23 No yellowing No change Large and few bubbles 43 Comparative Example 1 19 No yellowing No change Large and few bubbles 38 Comparative Example 2 18 No yellowing No change Large and few bubbles 39 Comparative Example 3 20 No yellowing No change Large and few bubbles 37 Comparative Example 4 19 No yellowing No change Large and few bubbles 38 Comparative Example 5 19 No yellowing No change Large and few bubbles 36

[0075] Result analysis:

[0076] 1. It can be seen from Examples 1 to 4 that when the addition amount of each component in Examples 1 to 4 is slightly adjusted, the viscosity and tensile strength of Examples 1 to 4 fluctuate to a certain extent, but the overall fluctuation range is small;

[0077] 2. It can be seen from Examples 5 to 7 that when mercaptopropyltrimethoxysilane is used alone to replace methacryloxypropyltrimethoxysilane, the tensile strength of Example 5 shows a certain downward trend;

[0078] Further observation of Example 6 shows that when methacryloxypropyl trimethoxysilane and mercaptopropyl trimethoxysilane are used simultaneously, Example 6 is significantly improved relative to Example 1 and Example 5. It can be seen that when methacryloxypropyl trimethoxysilane and mercaptopropyl trimethoxysilane are used in combination, the coupling effect of the coupling agent is significantly improved. We believe that the reason for this phenomenon is the difference in the key functional groups of the two silanes, which can react with glass wool and other additives in different types of chemical reactions, thereby forming a composite material with a richer structure, thereby improving the overall structural strength of the adhesive;

[0079] In Example 7, the addition of too much methacryloxypropyltrimethoxysilane may reduce the richness of the material structure, so that the tensile strength of the adhesive is closer to that of Example 1;

[0080] 3. It can be seen from Examples 1 and 8 to 11 that when titanate coupling agent and aluminate coupling agent are used to replace silane coupling agent, the tensile strength of Examples 8 and 9 both show a significant downward trend. When Example 10 uses a mixture of methacryloxypropyl trimethoxysilane, mercaptopropyl trimethoxysilane, tetraisopropoxy titanium and triisopropoxy aluminum to replace methacryloxypropyl trimethoxysilane, the tensile strength of Example 10 is not only significantly improved relative to Examples 8 and 9, but also has a certain degree of improvement relative to Example 6. It can be seen that in the case of methacryloxypropyl trimethoxysilane, the tensile strength of Example 10 is significantly improved relative to Examples 8 and 9. When the mass ratio of acryloyloxypropyl trimethoxysilane to mercaptopropyl trimethoxysilane is 3:1 (2.25:0.75), further adding titanate coupling agent and aluminate coupling agent can further improve the mechanical properties of the glass adhesive. It is speculated that the reason for this phenomenon may be that Example 10 introduces titanate coupling agent and aluminate coupling agent on the basis of Example 6 to further enhance the stability of the material and reduce the generation of microcracks at the interface of the material, thereby improving the fracture toughness and impact resistance of the adhesive system, and then improving the tensile strength of the glass adhesive;

[0081] In addition, during the subsequent use process, the titanate coupling agent and the aluminate coupling agent can also form Ti-O-Si bonds and Al-OS with the glass fiber, so that the bonding force between the binder and the glass fiber matrix is ​​further enhanced;

[0082] 4. It can be seen from Comparative Examples 1 to 6 that when the raw materials lack any of the coupling agent, hydroxyethyl acrylate, trimethylaminopropyl methacrylamide chloride, diallyl phthalate, and acrylic acid, the mechanical properties of the glass adhesive all show a significant downward trend. It can be seen that any of the coupling agent, hydroxyethyl acrylate, trimethylaminopropyl methacrylamide chloride, diallyl phthalate, and acrylic acid is indispensable.

Claims

1. A glass wool adhesive, characterized in that: By mass, it includes the following components: The coupling agent is selected from at least one of a silane coupling agent, a titanate coupling agent, an aluminate coupling agent, a phosphate coupling agent, and a zirconate coupling agent.

2. The glass wool adhesive according to claim 1, characterized in that: The coupling agent at least includes a silane coupling agent.

3. The glass wool adhesive according to claim 1, characterized in that: The silane coupling agent is selected from at least one of methacryloxypropyl trimethoxysilane, methacryloxypropyl triisopropoxysilane, methacryloxypropyl phenyl dimethoxy silane, mercaptopropyl trimethoxy silane, mercaptopropyl methyl dimethoxy silane and mercaptopropyl triisopropoxy silane.

4. The glass wool adhesive according to claim 1, characterized in that: The silane coupling agent is a mixture of methacryloxypropyl trimethoxysilane and mercaptopropyl trimethoxysilane, and the mass ratio of methacryloxypropyl trimethoxysilane to mercaptopropyl trimethoxysilane is 2-4:

1.

5. The glass wool adhesive according to claim 1, characterized in that: The coupling agent is a mixture of a silane coupling agent, a titanate coupling agent and an aluminate coupling agent, and the mass ratio of the silane coupling agent, the titanate coupling agent and the aluminate coupling agent is 1 to 3:1:

1.

6. The glass wool adhesive according to claim 1, characterized in that: The titanate coupling agent is selected from at least one of tetraisopropoxytitanium, tetraethoxytitanium, tetra-n-butoxytitanium and tetra-n-propoxytitanium.

7. The glass wool adhesive according to claim 1, characterized in that: The aluminate coupling agent is selected from at least one of triisopropoxy aluminum, triethoxy aluminum, tri-n-butoxy aluminum, and tri-n-propoxy aluminum.

8. The glass wool adhesive according to claim 1, characterized in that: The mass fraction of acrylic acid in the acrylic copolymer aqueous solution is 36-38wt%, and the number average molecular weight of the acrylic copolymer is 800-1000.

9. The glass wool adhesive according to claim 1, characterized in that: The foaming agent is oxalic acid or oxalate.

10. A method for preparing the glass wool adhesive according to any one of claims 1 to 9, characterized in that: Acrylic acid, foaming agent, hydroxyethyl acrylate, sodium hypophosphite, sodium persulfate, acrylic acid copolymer aqueous solution, trimethylaminopropyl methacrylamide chloride, diallyl phthalate, coupling agent and deionized water are mixed and reacted at 50-60° C. and normal pressure for 1-2 hours to obtain a glass wool adhesive.

Citation Information

Patent Citations

  • Preparation method of high-strength high-temperature-resistant glass cotton

    CN108751726A

  • Preparation method of antiseptic high-adhesion glass cotton adhesive

    CN109135637A