Semiconductor bonding method

By providing permeability and wettability on the surface of the substrate in semiconductor manufacturing, coating resin and ethanol to form a resin and viscosity layer, and curing under pressure, the problem of insufficient bonding strength of epoxy resin glue is solved and the bonding is significantly improved. performance and product life.

CN118725752APending Publication Date: 2024-10-01SAE TECH DELEVOPMENT DONGGUAN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310329151.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In semiconductor manufacturing, the bonding force of epoxy resin glue is insufficient, resulting in weak bonding, and the uniformity affects the bonding force.

Method used

By providing permeability and wettability on the surface of the substrate, the resin solution is first coated and solidified into a resin layer to form an epoxy resin layer, and ethanol is coated on it to form a viscosity layer. After the adhesive parts are bonded, they are pressed and solidified. , to increase the contact area and bonding depth between the epoxy resin and the substrate.

Benefits of technology

Significantly improves the bonding force between the epoxy resin glue and the base material, enhances the bonding performance, and extends the service life of the product.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a bonding method of a semiconductor. The bonding method comprises the following steps: fully dissolving resin in ethanol and acetone to form a resin solution; coating the bonding surface of the base material with the resin solution, and curing to form a resin layer; coating epoxy resin glue on the resin layer to form an epoxy resin layer; coating ethanol on the epoxy resin layer to form a viscosity layer; and bonding a to-be-bonded piece on the viscosity layer and curing the to-be-bonded piece. Good permeability and wettability are provided on the surface of a bonded base material, and the epoxy resin adhesive can be helped to permeate into micro cracks and micropores in the surface layer of the base material, so that the bonding force is improved, and the bonding effect is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of microelectronic processing, and in particular to a semiconductor bonding method. Background Art

[0002] In the field of semiconductor manufacturing, epoxy resin glue is often used for bonding. Whether the bonding strength is sufficient is the key. If the bonding strength is not strong, it is easy to fall off, and the uniformity of the adhesive will also affect the bonding strength.

[0003] There is an urgent need to provide an improved semiconductor bonding method to overcome the above defects. Summary of the invention

[0004] The object of the present invention is to provide an improved semiconductor bonding method, which provides good permeability and wettability on the surface of the bonding substrate, and can help the epoxy resin glue penetrate into the micro cracks and micro pores on the surface of the substrate, thereby improving the bonding strength.

[0005] To achieve the above object, the semiconductor bonding method of the present invention comprises the following steps:

[0006] The resin is fully dissolved in ethanol and acetone to form a resin solution;

[0007] Applying the resin solution on the bonding surface of the substrate and curing it to form a resin layer;

[0008] coating epoxy resin glue on the resin layer to form an epoxy resin layer;

[0009] coating ethanol on the epoxy resin layer to form a viscosity layer; and

[0010] The parts to be bonded are bonded to the adhesive layer and cured.

[0011] Compared with the prior art, the bonding method of the present invention coats a dissolved resin solution on the bonding surface and solidifies it into a resin layer. The purpose of this step is to allow the resin solution to penetrate into the fine pores and microcracks on the surface of the substrate, thereby improving the adhesion, and then forming an epoxy resin layer on the resin layer. Ethanol is coated on the epoxy resin layer, and the ethanol will dilute the surface of the epoxy resin to a certain depth below the surface to form a viscosity layer. In this way, the bonding effect of the adhesive part after being bonded thereon and solidified is very good, which increases the contact area and bonding depth between the epoxy resin and the substrate surface, and effectively improves the bonding strength.

[0012] Preferably, the resin in the resin solution accounts for 10%-20% of the total mass.

[0013] Preferably, the thickness of the resin layer is 0.15-0.25 mm.

[0014] Preferably, forming the epoxy resin layer specifically comprises: coating the epoxy resin glue on the resin layer, and then heating at a temperature of 110-120° C. for 1-1.5 hours.

[0015] Preferably, the step of bonding the workpiece to be bonded to the viscosity layer and curing the workpiece includes: pasting the workpiece to be bonded to the viscosity layer and pressurizing and curing the workpiece.

[0016] Preferably, the pressurization pressure of the pressurized curing is controlled to be 3.0-5.0 MPa.

[0017] Preferably, the pressurization time of the pressurization curing is 2-2.5 hours.

[0018] Preferably, the temperature of the pressurized curing is 100-120°C. DETAILED DESCRIPTION

[0019] The semiconductor bonding method of the present invention is further described below in conjunction with the examples, but the present invention is not limited thereby. The method of the present invention is intended to provide an improved semiconductor bonding method, which provides good permeability and wettability on the surface of the bonded substrate, and can help the epoxy resin glue penetrate into the micro cracks and micro pores on the surface of the substrate, thereby improving the bonding strength.

[0020] In one embodiment of the semiconductor bonding method of the present invention, the following steps are included:

[0021] The resin is fully dissolved in ethanol and acetone to form a resin solution;

[0022] Applying the resin solution on the bonding surface of the substrate and curing it to form a resin layer;

[0023] coating epoxy resin glue on the resin layer to form an epoxy resin layer;

[0024] coating ethanol on the epoxy resin layer to form a viscosity layer; and

[0025] The parts to be bonded are bonded to the adhesive layer and cured.

[0026] The bonding method of the present invention coats a dissolved resin solution on the bonding surface and solidifies it into a resin layer. The purpose of this step is to allow the resin solution to penetrate into the fine pores and microcracks on the surface of the substrate, thereby improving the bonding degree, and then forming an epoxy resin layer on the resin layer. Ethanol is coated on the epoxy resin layer, and the ethanol will dilute the surface of the epoxy resin to a certain depth below the surface to form a viscosity layer. In this way, the bonding effect of the adhesive member after being bonded thereon and solidified is very good, which increases the contact area and bonding depth between the epoxy resin and the substrate surface, and effectively improves the bonding strength.

[0027] Specifically, in one embodiment, the resin in the resin solution accounts for 10%-20% of the total mass. The resin is fully dissolved in ethanol and acetone until no precipitate is left.

[0028] The resin solution is applied to the bonding interface of the substrate, and after the acetone evaporates, the resin is cured on the interface. Preferably, the thickness of the resin layer formed after curing is 0.15-0.25 mm. This step allows the resin to penetrate into the tiny cavities on the surface of the substrate, thereby improving the adhesion.

[0029] Then, epoxy resin glue is applied on the surface of the resin layer, for example, epoxy resin AB glue is used. Preferably, the coating thickness of the epoxy resin glue is 0.30-0.5 mm, and the epoxy resin glue is heated for 1-1.5 hours at a heating temperature of 110-120° C., thereby forming an epoxy resin layer on the surface of the resin layer.

[0030] Next, ethanol is applied on the epoxy resin layer, which dilutes the surface and the depth of 0.05 mm below the surface, thereby generating a viscosity layer. The contact area of ​​the diluted viscosity layer relative to the original epoxy resin layer is increased, which is beneficial to improving the bonding strength.

[0031] Next, the parts to be bonded are bonded to the viscosity layer of the epoxy resin and pressurized for curing. Specifically, the pressurization pressure is controlled at 3.0 MPa-5.0 MPa, the pressurization time is 2-2.5 hours, and the temperature during pressurization curing is maintained at 100°C-120°C.

[0032] Therefore, the bonding method of the present invention provides good permeability and wettability on the surface of the bonded substrate, which can help the epoxy resin glue penetrate into the micro cracks and micro pores on the surface of the substrate, increase the contact area and bonding depth between the epoxy resin glue and the substrate surface, significantly improve the bonding performance, and increase the service life of the product.

[0033] The above disclosure is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of rights of the present invention. Therefore, equivalent changes made according to the scope of the patent application of the present invention are still within the scope covered by the present invention.

Claims

1. A semiconductor bonding method, characterized in that: The following steps are involved: The resin is fully dissolved in ethanol and acetone to form a resin solution; Applying the resin solution on the bonding surface of the substrate and curing it to form a resin layer; coating epoxy resin glue on the resin layer to form an epoxy resin layer; coating ethanol on the epoxy resin layer to form a viscosity layer; as well as The parts to be bonded are bonded to the adhesive layer and cured.

2. The semiconductor bonding method according to claim 1, wherein: The resin in the resin solution accounts for 10%-20% of the total mass.

3. The semiconductor bonding method according to claim 1, wherein: The thickness of the resin layer is 0.15-0.25 mm.

4. The semiconductor bonding method according to claim 1, wherein: The step of forming the epoxy resin layer specifically includes: coating the epoxy resin glue on the resin layer, and then heating the layer at a temperature of 110-120° C. for 1-1.5 hours.

5. The semiconductor bonding method according to claim 1, wherein: The thickness of the epoxy resin layer is 0.30-0.5 mm.

6. The semiconductor bonding method according to claim 1, wherein: The step of bonding the workpiece to be bonded to the viscosity layer and curing the workpiece includes: pasting the workpiece to be bonded to the viscosity layer and pressurizing and curing the workpiece.

7. The semiconductor bonding method according to claim 6, wherein: The pressurization pressure of the pressurized curing is controlled to be 3.0-5.0 MPa.

8. The semiconductor bonding method according to claim 7, wherein: The pressurizing time of the pressurizing curing is 2-2.5 hours.

9. The semiconductor bonding method according to claim 8, characterized in that: The temperature of the pressurized curing is 100-120°C.