Composite phase change energy storage material as well as preparation method and application thereof

By adsorbing n-alkyl alcohol on expanded graphite, composite phase change energy storage materials are prepared, which solves the problem of insufficient phase change latent heat and leakage in the existing technology, achieves efficient thermal energy storage and release, meets actual energy storage needs, and The preparation process is simplified.

CN118725830APending Publication Date: 2024-10-01INSTITUTE OF APPLIED CHEMISTRY JIANGXI ACADEMY OF SCIENCES +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410742791.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The latent heat of phase change of existing composite phase change energy storage materials is generally less than 150J/g, which is difficult to meet actual energy storage needs. At the same time, leakage problems exist, which limits their application in actual scenarios.

Method used

Expanded graphite is used as a porous carrier material to adsorb n-alkyl alcohol (such as n-tetradecanol and n-cetadecanol), and a composite phase change energy storage material is prepared through an impregnation process to increase the latent heat of phase change and solve the leakage problem. The porous scaffold of expanded graphite The structure and good thermal conductivity further improve the material's cycle stability and thermal energy storage and release efficiency.

Benefits of technology

The latent heat of phase change is achieved ≥208J/g, which improves the thermal conductivity and cycle stability of the material, meets the actual energy storage needs, simplifies the preparation process, reduces the cost, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725830A_ABST
    Figure CN118725830A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of phase change energy storage materials, and particularly relates to a composite phase change energy storage material and a preparation method and application thereof. The expanded graphite with light weight and high porosity is used as a porous carrier material, the content of a phase change material (n-alkyl alcohol) in the composite phase change energy storage material is greatly increased, the loss of latent heat is reduced, n-tetradecanol or n-hexadecanol with proper phase change temperature and high latent heat of phase change is used as the phase change material, and the phase change energy storage material is suitable for large-scale production. The obtained composite phase change energy storage material is high in phase change latent heat and can well meet the actual energy storage requirement; in addition, the thermal conductivity of the composite phase change energy storage material is greatly improved due to the good thermal conductivity of the expanded graphite, and the time required for heat energy storage and release is shortened; in addition, the porous scaffold structure of the expanded graphite effectively solves the leakage problem in the solid-liquid phase change process of the composite phase change energy storage material, and improves the cycle stability of the composite phase change energy storage material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of phase change energy storage materials, and specifically relates to a composite phase change energy storage material and a preparation method and application thereof. Background Art

[0002] In nature, solar energy is the most abundant and easily accessible energy source. However, the intermittent nature of solar energy acquisition limits its scope of use. Therefore, the research on solar thermal energy storage technology (TES) has attracted widespread attention and attention. Based on different energy storage principles, TES can be divided into latent heat, sensible heat and thermochemical energy storage technologies.

[0003] Latent heat energy storage technology uses phase change materials (PCM) as a medium to store and release energy during a phase change process with a basically constant temperature. PCM has a high energy storage density and a basically constant phase change temperature. It has low technical difficulty, relatively low cost, environmental protection and high safety. It has obvious advantages over sensible heat and thermochemical energy storage technologies.

[0004] PCM can be divided into organic, inorganic and eutectic mixtures according to the material composition. Its low phase change latent heat, low thermal conductivity and leakage problems limit the application of TES in practical scenarios. In order to solve the leakage problem, the existing technology mainly adopts microcapsule method and porous material adsorption method. Among them, the microcapsule method is complicated, while the porous material adsorption method is simpler. Commonly used porous materials include expanded perlite, expanded graphite, expanded vermiculite, halloysite nanotubes, diatomaceous earth, bentonite and kaolin. For example, the prior art (Jingyu Huang, Shilei Lu, Xiangfei Kong. et all. Form-Stable Phase Change Materials Based on Eutectic Mixture of Tetradecanol and Fatty Acids for Building Energy Storage: Preparation and Performance Analysis [J] Materials 2013, 6, 4758-4775) discloses a tetradecanol-fatty acid eutectic mixture composite phase change energy storage material, with latent heat of melting and latent heat of solidification of 107.38 J / g and 108.46 J / g, respectively. However, the phase change latent heat of the composite phase change material in the prior art is generally less than 150 J / g, which is difficult to meet the actual energy storage needs. Summary of the invention

[0005] The purpose of the present invention is to provide a composite phase change energy storage material and a preparation method and application thereof. The composite phase change energy storage material provided by the present invention has high phase change latent heat and can well meet actual energy storage needs.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] The invention provides a composite phase-change energy storage material, comprising expanded graphite and n-alkyl alcohol adsorbed on the surface and pores of the expanded graphite; the n-alkyl alcohol comprises n-tetradecanol and / or n-hexadecanol; and the phase change latent heat of the composite phase-change energy storage material is ≥208 J / g.

[0008] Preferably, the phase change temperature of the composite phase change energy storage material is 34-37°C.

[0009] Preferably, the mass ratio of the expanded graphite to the n-alkyl alcohol is 1:5-14.

[0010] Preferably, the mass ratio of the expanded graphite to the n-alkyl alcohol is 1:10-12.

[0011] The present invention provides a method for preparing the composite phase change energy storage material described in the above technical solution, comprising the following steps:

[0012] The expanded graphite and n-alkyl alcohol are mixed and impregnated to obtain a composite phase change energy storage material.

[0013] Preferably, the immersion temperature is 40-60° C. and the time is 2-4 hours.

[0014] Preferably, the impregnation includes vacuum impregnation; the vacuum degree of the vacuum impregnation is -0.01 MPa to -0.1 MPa.

[0015] Preferably, the expanded graphite is dried before mixing;

[0016] The drying temperature is 90-120° C., the pressure is 0.101 MPa, and the drying time is 0.5-1.5 h.

[0017] Preferably, the impregnation process further comprises stirring several times, the time interval between two stirrings is 0.5 to 1.5 hours, and the time of a single stirring is 1 to 5 minutes.

[0018] The present invention provides the application of the composite phase change energy storage material described in the above technical solution or the composite phase change energy storage material prepared by the preparation method described in the above technical solution in thermal energy storage technology.

[0019] The invention provides a composite phase-change energy storage material, comprising expanded graphite and n-alkyl alcohol adsorbed on the surface and in the pores of the expanded graphite. The present invention adopts light-weight and high-porosity expanded graphite (EG) as a porous carrier material, greatly improves the content of phase change material (n-alkyl alcohol) in the composite phase change energy storage material, reduces the loss of latent heat, adopts n-tetradecanol (TD) with an appropriate phase change temperature (about 36°C) and a high phase change latent heat (about 224 J / g) or n-hexadecanol with an appropriate phase change temperature (about 48°C) and a high phase change latent heat (about 232 J / g) as the phase change material, and the phase change latent heat of the obtained composite phase change energy storage material is ≥208 J / g, thereby improving the phase change latent heat of the composite phase change energy storage material; moreover, the good thermal conductivity of the expanded graphite greatly improves the thermal conductivity of the composite phase change energy storage material, shortens the time required for heat energy storage and release; in addition, the porous support structure of the expanded graphite effectively solves the leakage problem in the solid-liquid phase change process of the composite phase change energy storage material, improves the cycle stability of the composite phase change energy storage material, and can well meet the actual energy storage demand.

[0020] The present invention also provides a method for preparing the composite phase-change energy storage material described in the above technical solution. The preparation method provided by the present invention is simple to operate, low in cost, has little environmental pollution, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 N2 adsorption-desorption isotherm and pore size distribution curve of expanded graphite (inset);

[0022] Figure 2 is the SEM image of expanded graphite;

[0023] Figure 3 This is the SEM image of TD / EG composite phase change energy storage material;

[0024] Figure 4 Typical XRD patterns of expanded graphite, tetradecanol and TD / EG composite phase change energy storage materials;

[0025] Figure 5 FT-IR spectra of expanded graphite, tetradecanol and TD / EG composite phase change energy storage materials;

[0026] Figure 6 The melting and solidification curves of tetradecanol and TD / EG composite phase change energy storage materials;

[0027] Figure 7 This is the TGA diagram of n-tetradecanol and TD / EG composite phase change energy storage material;

[0028] Figure 8 The thermal conductivity diagram of expanded graphite, tetradecanol and TD / EG composite phase change energy storage material;

[0029] Fig. 9 It is a heat storage and release characteristic curve of expanded graphite, n-tetradecanol and TD / EG composite phase change energy storage material;

[0030] Fig.10 DSC curve of TD / EG composite phase change energy storage material before and after thermal cycling. DETAILED DESCRIPTION

[0031] The invention provides a composite phase-change energy storage material, comprising expanded graphite and n-alkyl alcohol adsorbed on the expanded graphite; the n-alkyl alcohol comprises n-tetradecanol and / or n-hexadecanol.

[0032] In the present invention, unless otherwise specified, the reagents used are commercially available products well known to those skilled in the art.

[0033] In the present invention, the n-alkyl alcohol includes n-tetradecanol and / or n-hexadecanol, preferably n-tetradecanol. In the present invention, the phase change latent heat of the composite phase change energy storage material is ≥208 J / g, preferably 208-210 J / g, more preferably 208.39-209.09 J / g; the phase change temperature of the composite phase change energy storage material is preferably 34-37°C, more preferably 35-36.5°C, and most preferably 35.54-35.78°C.

[0034] In the present invention, the mass ratio of the expanded graphite to the n-alkyl alcohol is preferably 1:5-14, more preferably 1:8-13, and most preferably 1:10-12.

[0035] The present invention provides a method for preparing the composite phase-change energy storage material described in the above technical solution, comprising the following steps: mixing expanded graphite and n-alkyl alcohol, and impregnating the mixture to obtain the composite phase-change energy storage material.

[0036] In the present invention, the expanded graphite is preferably dried before mixing; the drying temperature is preferably 90-120°C, more preferably 95-115°C, and most preferably 100-105°C; the drying is preferably carried out in a normal pressure drying oven; the drying pressure is preferably 0.101MPa; the drying time is 0.5-1.5h, more preferably 0.6-1.2h, and most preferably 0.8-1h. The present invention removes the moisture adsorbed by the expanded graphite during the storage process by drying the expanded graphite before mixing.

[0037] The present invention has no particular limitation on the mixing method, and any mixing method known in the art may be used, such as physical mixing.

[0038] In the present invention, the impregnation temperature is preferably 40-60°C, more preferably 42-55°C, and most preferably 45-50°C; the impregnation time is preferably 2-4h, more preferably 2.5-3.5h, and most preferably 3-3.2h; the impregnation preferably includes vacuum impregnation; the vacuum degree of the vacuum impregnation is preferably -0.01MPa to -0.1MPa, more preferably -0.05 to -0.1MPa, and most preferably -0.08 to -0.1MPa. In the present invention, the impregnation process preferably also includes several stirrings, and the time interval between two stirrings is preferably 0.5-1.5h, more preferably 0.6-1.2h, and most preferably 0.8-1h; the single stirring time is preferably 1-5min, more preferably 1-4min, and most preferably 1-2min.

[0039] After the impregnation is completed, the present invention preferably further comprises cooling the impregnated product obtained by the impregnation to room temperature to obtain a composite phase change energy storage material. The present invention has no particular limitation on the cooling method and rate, and it is sufficient that the impregnated product can be cooled to room temperature.

[0040] The present invention provides the application of the composite phase change energy storage material described in the above technical solution or the composite phase change energy storage material prepared by the preparation method described in the above technical solution in thermal energy storage technology (TES). In the present invention, the thermal energy storage technology preferably includes building energy-saving or thermal insulation materials. The composite phase change energy storage material provided by the present invention has high phase change latent heat, good thermal conductivity, and high cycle stability, and has broad application prospects in thermal energy storage technologies such as building energy-saving or thermal insulation materials.

[0041] In order to further illustrate the present invention, a composite phase change energy storage material provided by the present invention and its preparation method and application are described in detail below in conjunction with the accompanying drawings and embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0042] Example 1

[0043] The expanded graphite was placed in a 105°C atmospheric pressure drying oven and dried for 1 hour to obtain dry expanded graphite. 1.2 g of n-tetradecanol and 0.1 g of dry expanded graphite were physically mixed, placed in a vacuum drying oven at 45°C, and vacuum impregnated for 3 hours at a vacuum degree of -0.1 MPa, stirred for 1 minute every 1 hour, and after the impregnation was completed, the impregnated sample was taken out and cooled to room temperature to obtain a TD / EG composite phase change energy storage material, in which the mass ratio of n-tetradecanol to expanded graphite was 12:1.

[0044] Example 2

[0045] The expanded graphite was placed in a 105°C atmospheric pressure drying oven and dried for 1 hour to obtain dry expanded graphite. 1 g of n-tetradecanol and 0.1 g of dry expanded graphite were physically mixed, placed in a vacuum drying oven at 45°C, and vacuum impregnated for 3 hours at a vacuum degree of -0.1 MPa, stirred for 1 minute every 1 hour, and after the impregnation was completed, the impregnated sample was taken out and cooled to room temperature to obtain a TD / EG composite phase change energy storage material, in which the mass ratio of n-tetradecanol to expanded graphite was 10:1.

[0046] Test Example 1

[0047] (1) Microstructure and morphology of expanded graphite and TD / EG composite phase change energy storage materials

[0048] The specific surface area, pore volume and pore size distribution of expanded graphite were determined using a fully automatic specific surface and pore analyzer. Figure 1 The N2 adsorption-desorption isotherm and pore size distribution curve of expanded graphite (inset). The specific surface area of ​​expanded graphite is 33.1634 m 2 / g, pore volume is 0.1129cm 3 / g, the average pore size is 12.3554nm, and most of the expanded graphite has a mesoporous pore structure with a high surface area and high pore volume, thus having a huge adsorption capacity.

[0049] Figure 2 This is a SEM (scanning electron microscope) image of expanded graphite. Figure 2 It can be seen that the appearance of expanded graphite is a spiral worm-like graphite rod (indicated by the red line). Under magnification, it is observed that it has a unique multi-level structure and abundant pores, such as the intermediate crack-like pore structure (indicated by the yellow line) and the honeycomb pore structure (indicated by the green line).

[0050] Figure 3 This is the SEM image of TD / EG composite phase change energy storage material. Figure 3 It can be seen that compared with the long worm-like graphite rods of expanded graphite, the TD / EG composite phase change energy storage material presents many short worm-like graphite rods. Due to the existence of capillary force and surface tension, magnified observation shows that n-tetradecanol is absorbed into the multi-level pore structure of expanded graphite to form many small heat storage units.

[0051] (2) Crystal and chemical structure of expanded graphite, tetradecanol and TD / EG composite phase change energy storage materials

[0052] Figure 4The typical XRD patterns of expanded graphite, tetradecanol and TD / EG composite phase change energy storage materials show that all diffraction peaks of TD / EG composite phase change energy storage materials are well fitted with the diffraction peaks of expanded graphite and tetradecanol, indicating that TD / EG composite phase change energy storage materials are just physical combinations of expanded graphite and tetradecanol, and no new substances are produced during the combination process. The crystallinity of tetradecanol in pure phase change energy storage materials and TD / EG composite phase change energy storage materials was calculated using Jade data analysis software, and the results were 34.06% and 31.78%, respectively. The crystallinity of tetradecanol in TD / EG composite phase change energy storage materials decreased slightly, because the interconnected porous channels of expanded graphite restrict the free movement of tetradecanol molecules to a certain extent, thereby hindering the crystallization of tetradecanol.

[0053] Figure 5 The FT-IR spectra of expanded graphite, tetradecanol and TD / EG composite phase change energy storage material. The infrared absorption peak of expanded graphite is at 3430 cm -1 、1630cm -1 and 1345cm -1 The OH stretching vibration peak and OH bending vibration peak of water adsorbed in the air and the CH bending vibration peak of alkane adsorbed in the air are respectively; in the infrared absorption curve of n-tetradecanol, 3330cm -1 The OH stretching vibration peak of adsorbed water and primary alcohol is 2920 cm -1 and 2850cm -1 The two strong absorption bands at 1630 cm-1 are the antisymmetric and symmetric stretching vibration peaks of -CH3 and -CH2 groups. -1 The OH bending vibration peak of physically adsorbed water is 1465 cm -1 The OH bending vibration peak of primary alcohol is 1345 cm -1 The peak of CH bending vibration of -CH3 is 1060cm -1 The strong absorption band at 720 cm is the CO stretching vibration peak of the primary alcohol, and -1 For the TD / EG composite phase change energy storage material, the absorption curve contains all the representative bands of expanded graphite and tetradecanol, with only a slight change in relative intensity, and no new absorption bands are generated. It can be seen that there is no chemical interaction between expanded graphite and tetradecanol, and the chemical stability is good. Figure 4 The XRD results are consistent with those in .

[0054] (3) Phase change temperature and latent heat of TD / EG composite phase change energy storage materials

[0055] Table 1 shows the thermal properties of tetradecanol and TD / EG composite phase change energy storage materials. Figure 6These are the melting and solidification curves of n-tetradecanol and TD / EG composite phase change energy storage materials.

[0056] Table 1 Thermal properties of tetradecanol and TD / EG composite phase change energy storage materials

[0057]

[0058] From Table 1 and Figure 6 It can be seen that the melting and solidification phase transition temperatures of n-tetradecanol are 36.06℃ and 35.27℃, respectively, and the melting and solidification phase change latent heats are 223.78J / g and 223.81J / g, respectively. The melting and solidification phase transition temperatures of TD / EG composite phase change energy storage materials are 35.54℃ and 35.7℃, respectively, and the melting and solidification phase change latent heats are 209.09J / g and 208.39J / g, respectively. The phase change temperatures of n-tetradecanol and TD / EG composite phase change energy storage materials are very close, and the phase change latent heat of the latter is 91% of the former, which is close to the mass fraction of the enthalpy TD therein.

[0059] (4) Thermal stability of TD / EG composite phase change energy storage materials

[0060] Figure 7 This is the TGA (thermogravimetric analysis) diagram of the tetradecanol and TD / EG composite phase change energy storage material. Figure 7 It can be seen that n-tetradecanol and TD / EG composite phase change energy storage materials undergo one-step thermal decomposition in the range of 165-282°C. Therefore, when the temperature is lower than 165°C, n-tetradecanol and TD / EG composite phase change energy storage materials have good thermal stability.

[0061] (5) Thermal conductivity and heat storage and release characteristics of TD / EG composite phase change energy storage materials

[0062] Figure 8 is the thermal conductivity diagram of expanded graphite, tetradecanol and TD / EG composite phase change energy storage material, Figure 8 It can be seen that the thermal conductivity of n-tetradecanol, expanded graphite and TD / EG composite phase change energy storage materials are 0.330 W / mk, 8.129 W / mk and 7.388 W / mk, respectively. The thermal conductivity of TD / EG composite phase change energy storage material is 22 times that of pure phase change material (n-tetradecanol), and it has good thermal conductivity. The reason is that n-tetradecanol is distributed in the multi-layer structure of worm-like expanded graphite. The worm-like expanded graphite serves as a flexible skeleton, and the internal structure is cross-linked to form an efficient heat transfer channel, which improves the thermal conductivity of TD / EG composite phase change energy storage material.

[0063] Fig. 9The heat storage and release characteristics curve of expanded graphite, tetradecanol and TD / EG composite phase change energy storage material are shown in Figure 2. By comparing with expanded graphite and tetradecanol, the heat storage and release performance of TD / EG composite phase change energy storage material is evaluated by temperature change time. Fig. 9 It can be seen that when the temperature rises from 15°C to 60°C, the time required for expanded graphite, n-tetradecanol and TD / EG composite phase change energy storage materials are 70s, 520s and 1210s respectively. The time required for n-tetradecanol is 2.3 times that of the TD / EG composite phase change energy storage material, and the time required for the TD / EG composite phase change energy storage material is 7.4 times that of expanded graphite; when the temperature drops from 60°C to 20°C, the time required for expanded graphite, n-tetradecanol and TD / EG composite phase change energy storage materials are 60s, 900s and 2020s respectively. The time required for n-tetradecanol is 2.2 times that of the TD / EG composite phase change energy storage material, and the time required for the TD / EG composite phase change energy storage material is 15 times that of expanded graphite. This shows that the thermal response rate of the TD / EG composite phase change energy storage material is faster than that of n-tetradecanol, but slower than that of expanded graphite. The reason is that the addition of expanded graphite in the TD / EG composite phase change energy storage material enhances its thermal conductivity, while the addition of n-tetradecanol makes it have the characteristics of phase change endothermic and exothermic, which delays the change of system temperature and plays a role in regulating the change of external ambient temperature.

[0064] (6) Cyclic stability of TD / EG composite phase change energy storage materials

[0065] Thermal stability is one of the factors that determine whether phase change energy storage materials can be used for a long time. Therefore, DSC was used to test the TD / EG composite phase change energy storage materials after 0, 100, 200 and 300 melting / solidification cycles. The results are shown in Table 2 and Fig.10 Table 2 shows the thermal properties of TD / EG composite phase change energy storage materials before and after thermal cycling. Fig.10 DSC curve of TD / EG composite phase change energy storage material before and after thermal cycling.

[0066] Table 2 Thermal properties of TD / EG composite phase change energy storage materials before and after thermal cycling

[0067]

[0068] From Table 2 and Fig.10 It can be seen that the melting temperature and solidification temperature of the TD / EG composite phase change energy storage material have no significant changes before and after thermal cycling, and the relative standard deviation (RSD) is 0.11% and 0.13% respectively; its melting enthalpy and solidification enthalpy have no significant difference, and the RSD is 0.79% and 0.67% respectively. Therefore, after 300 thermal cycles, the TD / EG composite phase change energy storage material has good cycle stability.

[0069] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A composite phase change energy storage material, characterized in that: The composite phase-change energy storage material comprises expanded graphite and n-alkyl alcohol adsorbed on the surface and pores of the expanded graphite; the n-alkyl alcohol comprises n-tetradecanol and / or n-hexadecanol; and the phase change latent heat of the composite phase-change energy storage material is ≥208 J / g.

2. The composite phase change energy storage material according to claim 1, characterized in that: The phase change temperature of the composite phase change energy storage material is 34-37°C.

3. The composite phase change energy storage material according to claim 1 or 2, characterized in that: The mass ratio of the expanded graphite to the n-alkyl alcohol is 1:5-14.

4. The composite phase change energy storage material according to claim 3, characterized in that: The mass ratio of the expanded graphite to the n-alkyl alcohol is 1:10-12.

5. The method for preparing the composite phase change energy storage material according to any one of claims 1 to 4, characterized in that: The following steps are involved: The expanded graphite and n-alkyl alcohol are mixed and impregnated to obtain a composite phase change energy storage material.

6. The preparation method according to claim 5, characterized in that: The immersion temperature is 40-60° C. and the immersion time is 2-4 hours.

7. The preparation method according to claim 5 or 6, characterized in that: The impregnation includes vacuum impregnation; the vacuum degree of the vacuum impregnation is -0.01MPa to -0.1MPa.

8. The preparation method according to claim 5, characterized in that: The expanded graphite is also dried before mixing; The drying temperature is 90-120° C., the pressure is 0.101 MPa, and the drying time is 0.5-1.5 h.

9. The preparation method according to claim 5, characterized in that: The immersion process also includes several stirrings, the time interval between two stirrings is 0.5 to 1.5 hours, and the time of a single stirring is 1 to 5 minutes.

10. Application of the composite phase change energy storage material according to any one of claims 1 to 4 or the composite phase change energy storage material prepared by the preparation method according to any one of claims 5 to 9 in thermal energy storage technology.