Carbon dot starch composite material as well as preparation method and application thereof

By combining carbon quantum dots with starch, the monodisperse state of carbon dots is achieved, which solves the problem of difficulty in carrying and storing carbon dot aqueous solutions, provides a solid-state fluorescent material suitable for fingerprint imprinting, and maintains efficient fluorescent properties.

CN118725850APending Publication Date: 2024-10-01SHENYANG NORMAL UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410761257.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing carbon dot aqueous solution is difficult to carry and store, and the aggregation of solid carbon dots causes fluorescence quenching, making it difficult to use for fingerprint imprinting.

Method used

Starch is used as a dispersion material, and carbon quantum dots are generated through hydrothermal reaction or microwave treatment, and mixed with starch to achieve a monodispersed state of carbon dots through surface hydrogen bonding to avoid fluorescence quenching caused by aggregation.

Benefits of technology

It achieves the monodisperse state of carbon dots in the solid state, maintains the fluorescence luminescence performance, and provides a solid-state luminescent material that is easy to carry and store, and is suitable for fingerprint imprinting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725850A_ABST
    Figure CN118725850A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of carbon dot materials, and discloses a carbon dot starch composite material as well as a preparation method and application thereof. The preparation method comprises the following steps: uniformly mixing citric acid serving as a carbon source and urea serving as a nitrogen source in water to obtain a mixed solution; enabling the citric acid in the mixed solution to react with urea by adopting a hydrothermal reaction or microwave treatment mode, and forming carbon quantum dots, so as to obtain a carbon dot solution; and uniformly mixing the carbon dot solution with starch, and drying to obtain the carbon dot starch composite material. The starch is used as a dispersion material of a carbon dot solution, and the carbon dots can exist in a solid luminescent material in a monodisperse state, so that the fluorescence quenching phenomenon of the carbon dots caused by aggregation is effectively avoided, and the prepared carbon dot starch composite material can effectively ensure the fluorescence luminescence performance of the solid carbon dots; therefore, the carbon dot starch composite material prepared by the invention can be used in fingerprint imprinting in the form of a solid luminescent material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of carbon dot materials, and in particular to a carbon dot starch composite material and a preparation method and application thereof. Background Art

[0002] Carbon quantum dots (CDs), also known as carbon dots, are a new type of fluorescent carbon nanomaterials with a size of less than 10nm. They have low cost, simple and diverse synthesis routes, good water solubility, low toxicity, environmental friendliness, high biocompatibility, easy surface functionalization, high fluorescence intensity, and good photostability. They are an ideal fluorescent material.

[0003] However, since the aggregation of solid carbon dots will cause fluorescence quenching, the carbon dot materials used for fingerprint imprinting in the prior art are mainly carbon dot aqueous solutions. However, carbon dot aqueous solutions are not easy to carry and store. Therefore, it is necessary to provide a fluorescent material that is easy to carry and store and has good fluorescent luminescence properties.

[0004] To this end, the present invention provides a carbon dot starch composite material and a preparation method and application thereof. Summary of the invention

[0005] In order to solve the deficiencies in the above-mentioned prior art, the present invention provides a carbon dot starch composite material and a preparation method and application thereof. The present invention uses starch as a dispersing material, can achieve a monodispersed state of carbon dots in a solid form, effectively avoids the fluorescence quenching phenomenon of carbon dots caused by aggregation, so that the carbon dot starch composite material prepared by the present invention can effectively ensure the fluorescence luminescence performance of solid carbon dots, and further enables the carbon dot starch composite material prepared by the present invention to be used in fingerprint imprinting in the form of a solid luminescent material.

[0006] The carbon dot starch composite material and its preparation method and application are achieved by the following technical solutions:

[0007] The first object of the present invention is to provide a method for preparing a carbon dot starch composite material, comprising the following steps:

[0008] Step 1: using citric acid as a carbon source and urea as a nitrogen source, mixing the two in water to obtain a mixed solution; using a hydrothermal reaction or microwave treatment method to make the citric acid and urea in the mixed solution react to form carbon quantum dots, thereby obtaining a carbon dot solution.

[0009] It should be noted that the present invention uses citric acid and urea as raw materials and water as solvent, and uniformly disperses citric acid and urea in water to form a mixed solution with uniform components. Citric acid can be dissociated into citrate ions (C6H5O7 - ), C6H5O7 -A carbon source and a reducing agent can be provided so that in the subsequent heating process or microwave process, citric acid can fully contact and react with urea, that is, the citric acid ions and the amino groups in the urea undergo a deamination reaction to form ammonia and a new intermediate product. The intermediate product further reacts to form a graphene structure, in which the carbon atoms are provided by the citric acid ions and the nitrogen atoms are provided by the amino groups in the urea. The graphene structure has full aromaticity, resulting in the formation of carbon dots (carbon quantum dots) to obtain a carbon dot solution.

[0010] The present invention takes into account the ratio of each element of the carbon dots, and the surface functional groups and atomic structure are all related to the ratio of citric acid and urea. In order to ensure that the carbon dot solution can be obtained regardless of whether the hydrothermal reaction method or the microwave treatment method is adopted, in some feasible embodiments of the present invention, the mass ratio of the citric acid to the urea is 1:1.5-2.5, so that the obtained carbon dots have a higher fluorescence quantum efficiency.

[0011] In order to ensure that the water used in the present invention can fully disperse or dissolve the citric acid and urea, in some feasible embodiments of the present invention, the usage ratio of the water to the citric acid is 15-25 mL:1 g.

[0012] When the carbon dot solution is prepared by hydrothermal reaction, in order to ensure that during the hydrothermal reaction, citric acid can dissociate into citric acid ions, and at the same time, the amino groups in urea react with citric acid to form intermediate products, and the intermediate products further react to form carbon dots, that is, blue carbon dots, to obtain a blue carbon dot solution, in some feasible embodiments of the present invention, the temperature of the hydrothermal reaction is 150-170° C. And in order to ensure that citric acid and urea can form blue carbon dots at this temperature, in some feasible embodiments of the present invention, the time of the hydrothermal reaction is 3-5 hours.

[0013] It can be understood that since the hydrothermal product obtained by the hydrothermal reaction has the defect of uneven sample size, in some feasible embodiments of the present invention, the hydrothermal product is also post-treated to achieve the purpose of obtaining carbon dots of suitable size through post-treatment. And the post-treatment is carried out by the following steps: filtering the hydrothermal product with a filter membrane to obtain a filtrate; dialysis treatment of the filtrate to achieve filtering treatment of the filtrate through dialysis treatment to obtain a blue carbon dot solution. Among them, in some feasible embodiments of the present invention, the pore size of the filter membrane used is 0.22μm. And in order to ensure that the above effect can be achieved through dialysis treatment, in a feasible embodiment of the present invention, the filtrate is added to a clean dialysis bag, clamped with a sealing clamp, placed in a container filled with deionized water, and then dialyzed at 70°C for at least three times, each time for 10 minutes, to finally obtain a blue carbon dot solution.

[0014] When the carbon dot solution is prepared by microwave treatment, in order to ensure that during the microwave treatment, citric acid and urea undergo a pyrolysis reaction under microwave radiation to produce carbon ions, free radicals or thermal decomposition products; carbon ions, free radicals or thermal decomposition products polymerize under high temperature conditions to form carbon clusters; carbon clusters further pyrolyze at high temperature to generate smaller carbon clusters or nano carbon dots, that is, to form green carbon dots, and obtain a green carbon dot solution, in some feasible embodiments of the present invention, the power of the microwave treatment is 600 to 800 W. And in order to ensure that citric acid and urea can form green carbon dots at this temperature, in some feasible embodiments of the present invention, the time of the microwave treatment is 4 to 8 minutes.

[0015] It can be understood that since the microwave product obtained by microwave treatment has the defect of uneven distribution of carbon dots, in some feasible embodiments of the present invention, the microwave product of the microwave treatment is also post-processed to achieve the purpose of obtaining carbon dots of suitable size through post-processing. And the post-processing is carried out by the following steps: after dispersing the microwave product in water, centrifuging at least 2 times, and the obtained supernatant is the green carbon dot solution. Among them, in order to remove large particles of solid in the microwave product, in some feasible embodiments of the present invention, the volume ratio of water used to disperse the microwave product to the microwave product is 30-40:25-35.

[0016] In order to ensure that large solid particles in the microwave product can be removed by centrifugal treatment, in some feasible embodiments of the present invention, the centrifugal speed is 8000 r / min and each time is 8 to 12 minutes.

[0017] Step 2: Mix the carbon dot solution and starch and then dry them to obtain the carbon dot starch composite material.

[0018] It should be noted that in order to obtain solid-state luminescent materials and avoid the fluorescence quenching phenomenon caused by the aggregation of solid carbon dots when the carbon dot solution is prepared into a solid state, the present invention preferably uses starch as a dispersing material for the carbon dot solution, and the starch surface contains a large number of hydroxyl functional groups, and the blue carbon dots and green carbon dots obtained in the present invention have amide groups on their surfaces, so that starch can be combined with blue carbon dots and green carbon dots respectively through surface hydrogen bonding, thereby allowing green carbon dots or blue carbon dots to be adsorbed on the surface of starch, thereby achieving a monodisperse state of green carbon dots or blue carbon dots, so that in the formed solid material, green carbon dots or blue carbon dots exist not in an agglomerated state, but in a monodisperse state, thereby effectively avoiding the fluorescence quenching phenomenon of carbon dots caused by aggregation, so that the carbon dot starch composite material prepared by the present invention can effectively guarantee the fluorescence luminescence performance of solid carbon dots, and thus the carbon dot starch composite material prepared by the present invention can be used in fingerprint imprinting in the form of solid-state luminescent materials. Moreover, the present invention uses starch as a dispersing material, which is not only environmentally friendly and pollution-free, but also inexpensive, easily available, and biodegradable.

[0019] And in order to ensure that the starch used can achieve the above-mentioned technical effects, in some feasible embodiments of the present invention, the starch used is one or more of potato starch, corn starch, tapioca starch, sweet potato starch and rice starch. Among them, when the starch used is corn starch, corn starch with a mean particle size of 13 to 17 μm is preferred. When the starch used is potato starch, potato starch with a mean particle size of 30 to 35 μm is preferred. When the starch used is tapioca starch, tapioca starch with a mean particle size of 18 to 22 μm is preferred. When the starch used is sweet potato starch, sweet potato starch with a mean particle size of 16 to 20 μm is preferred. When the starch used is rice starch, rice starch with a mean particle size of 2 to 8 μm is preferred.

[0020] In order to ensure that the amount of starch added is sufficient to achieve monodispersity of the carbon dots, in some feasible embodiments of the present invention, the mass ratio of the carbon dot solution to the starch is 40 to 50:1.

[0021] In order to ensure that the starch and carbon dot solution are fully mixed, in some feasible embodiments of the present invention, the mixture is mixed by stirring, and the stirring time is 10 to 20 minutes until the mixture becomes a paste.

[0022] It can be understood that since the amount of starch used is relatively small relative to the amount of carbon dot solution used, there may be carbon dots adsorbed in starch to form a carbon dot-starch composite material. Therefore, in some feasible embodiments of the present invention, it is necessary to filter the mixed material to remove the unabsorbed carbon dots by filtration to improve the purity of the obtained carbon dot-starch composite material.

[0023] It is understandable that since there may still be moisture in the product after the above filtration, in some feasible embodiments of the present invention, it is necessary to remove the moisture therein by drying, and the drying temperature is 55-65° C. and the drying time is 1-3 hours.

[0024] The present invention takes into account that the product may agglomerate during the drying process, which is not conducive to its subsequent application as a fluorescent material. Therefore, in some feasible embodiments of the present invention, the dried product needs to be ground to a particle size of 1 nm to 40 μm to ensure that the ground product has good fluorescent properties.

[0025] The second object of the present invention is to provide a carbon dot starch composite material prepared by the above preparation method.

[0026] The third object of the present invention is to provide the application of the above carbon dot starch composite material in fingerprint imprinting.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] The present invention uses starch as a dispersing material for a carbon dot solution, so that the starch and the carbon dots are combined together through surface hydrogen bonding, and then the carbon dots are adsorbed on the surface of the starch, thereby achieving a monodisperse state of the carbon dots, so that in the formed solid material, the carbon dots are not present in an agglomerated state, but in a monodisperse state, thereby effectively avoiding the fluorescence quenching phenomenon of the carbon dots caused by aggregation, so that the carbon dot starch composite material prepared by the present invention can effectively guarantee the fluorescent luminescence performance of the solid carbon dots, and then the carbon dot starch composite material prepared by the present invention can be used in fingerprint imprinting in the form of a solid luminescent material.

[0029] The present invention uses starch as the dispersing material, which is not only environmentally friendly and pollution-free, but also cheap, easily available and biodegradable.

[0030] The preparation method of the present invention is simple and easy to operate, and can be easily promoted for large-scale production and use, which is conducive to the application of carbon dot materials in a solid form as fluorescent markers in fingerprint imprinting, thus expanding the application field of carbon dots. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 UV absorption and fluorescence spectra of b-CDs.

[0032] Figure 2 UV absorption spectrum and fluorescence spectrum of g-CDs.

[0033] Figure 3 UV absorption spectrum and fluorescence spectrum of b-CDs@St.

[0034] Figure 4Ultraviolet absorption spectrum and fluorescence spectrum of g-CDs@St.

[0035] Figure 5 Infrared spectra of b-CDs@St and g-CDs@St.

[0036] Figure 6 The fingerprints were collected on glass and plastic plates using g-CDs@St and b-CDs@St as fluorescent markers. Figure 6 (a) is a fingerprint imprint photograph collected on a glass plate under sunlight using b-CDs@St as a fluorescent marker; Figure 6 (b) is a fingerprint imprint photograph collected on a glass plate under sunlight using g-CDs@St as a fluorescent marker; Figure 6 (c) is a fingerprint imprint photograph collected on a plastic plate under sunlight using b-CDs@St as a fluorescent marker; Figure 6 (d) is a fingerprint imprint photograph collected on a plastic plate under sunlight using g-CDs@St as a fluorescent marker; Figure 6 (e) is a fingerprint imprint photograph collected on a glass plate under ultraviolet light using b-CDs@St as a fluorescent marker; Figure 6 (f) is a fingerprint imprint photograph collected on a glass plate under ultraviolet light using g-CDs@St as a fluorescent marker; Figure 6 (g) is a fingerprint imprint photograph collected on a plastic plate under ultraviolet light using b-CDs@St as a fluorescent marker; Figure 6 (h) is a fingerprint imprint photograph collected on a plastic plate under ultraviolet light using g-CDs@St as a fluorescent marker. DETAILED DESCRIPTION

[0037] The technical solutions in the embodiments of the present invention will be described clearly and completely below. It should be noted that the starch used in the following embodiments of the present invention is potato starch produced by Dongmei Starch Products Factory.

[0038] Example 1

[0039] This embodiment provides a carbon dot starch composite material, which is prepared by the following steps:

[0040] Step 1: Prepare carbon dot solution:

[0041] 1) According to the ratio of 1g:2g:20mL, weigh the corresponding mass of citric acid and urea, and the corresponding volume of deionized water, and disperse the weighed citric acid and urea in the deionized water, stir evenly to form a colorless and transparent mixed solution.

[0042] 2) The mixed solution obtained above was transferred to a stainless steel autoclave lined with polytetrafluoroethylene and subjected to hydrothermal reaction at 160° C. for 4 h to obtain a dark brown liquid, indicating the initial formation of blue light carbon dots.

[0043] 3) The dark brown liquid was taken out with a syringe, filtered through a 0.22 μm membrane filter to obtain a filtrate, and the filtrate was added to a clean dialysis bag, which was clamped with a sealing clip and placed in a 100 mL beaker filled with deionized water. The temperature was controlled at 70°C by a magnetic stirring heater, and dialyzed three times for 10 min each time to finally obtain a blue carbon dot solution.

[0044] Step 2: Compound carbon dot solution and starch:

[0045] 1) The blue light carbon dot solution and starch were stirred and mixed uniformly at a mass ratio of 45:1 to obtain a mixture.

[0046] 2) Filter the mixture obtained above to remove the unabsorbed blue light starch composite material in the mixture, and dry the solid block remaining on the filter paper in an oven. Grind the dried solid block in an agate mortar to obtain a blue light carbon dot starch composite material, which is referred to as b-CDs@St.

[0047] Example 2

[0048] This embodiment provides a carbon dot starch composite material, which is prepared by the following steps:

[0049] Step 1: Prepare carbon dot solution:

[0050] 1) According to the ratio of 1g:2g:20mL, weigh the corresponding mass of citric acid and urea, and the corresponding volume of deionized water, and disperse the weighed citric acid and urea in the deionized water, stir evenly to form a colorless and transparent mixed solution.

[0051] 2) The mixed solution obtained above was placed in a microwave oven and microwaved at a power of 700 W for 6 min. It can be observed that during the microwave process, the solution changed from colorless and transparent to brown and finally to a dark brown solid, indicating the formation of green light carbon dots.

[0052] 3) The dark brown solid was redispersed in 30 mL of deionized water and centrifuged twice, each time for 10 min at a centrifugal speed of 8000 rpm. After centrifugation, the supernatant was retained and the precipitated large solid particles were removed to obtain a green light carbon dot solution.

[0053] Step 2: Compound carbon dot solution and starch:

[0054] 1) The green light carbon dot solution and starch were stirred and mixed uniformly at a mass ratio of 45:1 to obtain a mixture.

[0055] 2) Filter the mixture obtained above to remove the unabsorbed blue light starch composite material in the mixture, and dry the solid block remaining on the filter paper in an oven. Grind the dried solid block in an agate mortar to obtain the green light carbon dot starch composite material, which is referred to as g-CDs@St.

[0056] Example 3

[0057] Step 1: Prepare carbon dot solution:

[0058] 1) According to the ratio of 1g:1.5g:15mL, weigh the corresponding mass of citric acid and urea, and the corresponding volume of deionized water, and disperse the weighed citric acid and urea in the deionized water, stir evenly to form a colorless and transparent mixed solution.

[0059] 2) The mixed solution obtained above was transferred to a stainless steel autoclave lined with polytetrafluoroethylene and subjected to hydrothermal reaction at 150° C. for 5 h to obtain a dark brown liquid, indicating the initial formation of blue light carbon dots.

[0060] 3) The dark brown liquid was taken out with a syringe, filtered through a 0.22 μm membrane filter to obtain a filtrate, and the filtrate was added to a clean dialysis bag, which was clamped with a sealing clip and placed in a 100 mL beaker filled with deionized water. The temperature was controlled at 70°C by a magnetic stirring heater, and dialyzed three times for 10 min each time to finally obtain a blue carbon dot solution.

[0061] Step 2: Compound carbon dot solution and starch:

[0062] 1) The blue light carbon dot solution and starch were stirred and mixed uniformly at a mass ratio of 40:1 to obtain a mixture.

[0063] 2) Filter the mixture obtained above to remove the unabsorbed blue light starch composite material in the mixture, and dry the solid block remaining on the filter paper in an oven. Grind the dried solid block in an agate mortar to obtain the blue light carbon dot starch composite material.

[0064] Example 4

[0065] Step 1: Prepare carbon dot solution:

[0066] 1) According to the ratio of 1g:2.5g:25mL, weigh the corresponding mass of citric acid and urea, and the corresponding volume of deionized water, and disperse the weighed citric acid and urea in the deionized water, stir evenly to form a colorless and transparent mixed solution.

[0067] 2) The mixed solution obtained above was transferred to a stainless steel autoclave lined with polytetrafluoroethylene and subjected to hydrothermal reaction at 170° C. for 3 h to obtain a dark brown liquid, indicating the initial formation of blue light carbon dots.

[0068] 3) The dark brown liquid was taken out with a syringe, filtered through a 0.22 μm membrane filter to obtain a filtrate, and the filtrate was added to a clean dialysis bag, which was clamped with a sealing clip and placed in a 100 mL beaker filled with deionized water. The temperature was controlled at 70°C by a magnetic stirring heater, and dialyzed three times for 10 min each time to finally obtain a blue carbon dot solution.

[0069] Step 2: Compound carbon dot solution and starch:

[0070] 1) The blue light carbon dot solution and starch were stirred and mixed uniformly at a mass ratio of 50:1 to obtain a mixture.

[0071] 2) Filter the mixture obtained above to remove the unabsorbed blue light starch composite material in the mixture, and dry the solid block remaining on the filter paper in an oven. Grind the dried solid block in an agate mortar to obtain the blue light carbon dot starch composite material.

[0072] Comparative Example 1

[0073] This comparative example provides a carbon dot starch composite material, which is prepared by the following steps:

[0074] Step 1: Prepare carbon dot solution:

[0075] 1) According to the ratio of 1g:2g:20mL, weigh the corresponding mass of citric acid and urea, and the corresponding volume of deionized water, and disperse the weighed citric acid and urea in the deionized water, stir evenly to form a colorless and transparent mixed solution.

[0076] 2) The mixed solution obtained above was transferred to a stainless steel autoclave lined with polytetrafluoroethylene and subjected to hydrothermal reaction at 160° C. for 4 h to obtain a dark brown liquid, indicating the initial formation of blue light carbon dots.

[0077] 3) The dark brown liquid was taken out with a syringe, filtered through a 0.22 μm membrane filter to obtain a filtrate, and the filtrate was added to a clean dialysis bag, clamped with a sealing clip, and placed in a 100 mL beaker filled with deionized water. The temperature was controlled at 70°C by a magnetic stirring heater, and dialyzed three times for 10 min each time to finally obtain a blue carbon dot solution, which was referred to as b-CDs.

[0078] That is, the difference between this comparative example and Example 1 is only that:

[0079] This comparative example is not compounded with starch.

[0080] Comparative Example 2

[0081] This comparative example provides a carbon dot starch composite material, which is prepared by the following steps:

[0082] Step 1: Prepare carbon dot solution:

[0083] 1) According to the ratio of 1g:2g:20mL, weigh the corresponding mass of citric acid and urea, and the corresponding volume of deionized water, and disperse the weighed citric acid and urea in the deionized water, stir evenly to form a colorless and transparent mixed solution.

[0084] 2) The mixed solution obtained above was placed in a microwave oven and microwaved at a power of 700 W for 6 min. It can be observed that during the microwave process, the solution changed from colorless and transparent to brown and finally to a dark brown solid, indicating the formation of green light carbon dots.

[0085] 3) The dark brown solid was redispersed in 30 mL of deionized water and centrifuged twice, each time for 10 min at a centrifugal speed of 8000 rpm. After centrifugation, the supernatant was retained and the precipitated large solid particles were removed to obtain a green light carbon dot solution, which was referred to as g-CDs.

[0086] That is, the difference between this comparative example and Example 2 is only that:

[0087] This comparative example is not compounded with starch.

[0088] Experimental Section

[0089] (I) Testing of UV absorption spectrum and fluorescence spectrum

[0090] The present invention takes the blue light carbon dot solution (b-CDs) obtained in Comparative Example 1 and the green carbon dot solution (g-CDs) obtained in Comparative Example 2 as examples, and performs ultraviolet absorption spectrum test and fluorescence spectrum test on them respectively, and the test results are as follows: Figure 1 and Figure 2 shown.

[0091] in, Figure 1 The ultraviolet absorption spectrum and fluorescence spectrum of b-CDs show that the blue-light carbon dots can emit light with a wavelength of about 440nm, that is, the emitted light is blue light, which indicates that the present invention has successfully synthesized the blue-light carbon dots.

[0092] Figure 2 The ultraviolet absorption spectrum and fluorescence spectrum of g-CDs show that the green carbon dots can emit light with a wavelength of about 510 nm, that is, green light, which indicates that the present invention has successfully synthesized green carbon dots.

[0093] The present invention also performs fluorescence spectrum tests on the blue carbon dot starch composite material (b-CDs@St) of Example 1 and the green carbon dot starch composite material (g-CDs@St) of Example 2, and the test results are as follows: Figure 3 and Figure 4 shown.

[0094] in, Figure 3 The fluorescence spectrum of b-CDs@St shows that the emission spectra of the blue light carbon dot starch composite material and the blue light carbon dot are consistent, which indicates that the blue light carbon dot has good dispersion on the starch surface. The maximum excitation wavelength of b-CDs@St is 320nm, and the maximum emission wavelength is 441nm.

[0095] Figure 4 Figure 2 is the fluorescence spectrum of g-CDs@St. It can be seen that the emission spectra of the blue carbon dot starch composite material and the green carbon dot are consistent, which indicates that the green carbon dots have good dispersion on the starch surface. The maximum excitation wavelength of g-CDs@St is 374nm, and the maximum emission wavelength is 518nm.

[0096] And through Figure 1-4 It can also be seen that the present invention uses starch as a dispersing material, which can achieve a monodisperse state of carbon dots in a solid form, effectively avoiding the fluorescence quenching phenomenon of carbon dots caused by aggregation, so that the carbon dot starch composite material prepared by the present invention can effectively ensure the fluorescent luminescence performance of solid carbon dots.

[0097] (II) Fluorescence quantum yield

[0098] Fluorescence quantum yield is an important performance parameter of CDs, which refers to the ratio of the number of photons emitted as secondary radiation fluorescence to the number of photons absorbed as primary radiation of excitation light. There are two methods for determining carbon quantum yield: relative method and absolute method. The fluorescence quantum yield of CDs is usually measured by relative method. When the solution is dilute, the relationship between fluorescence intensity, excitation light intensity and fluorescence quantum yield is as follows: At the same excitation wavelength, the ratio of the fluorescence quantum yields of the two substances satisfies the following relationship:

[0099] F=KI0clεφ (1)

[0100] Among them, F is the fluorescence intensity; K is the instrument constant; I0 ​​is the excitation light intensity; c is the sample concentration; l is the light path of the absorption cell; ε is the absorption coefficient of the sample; φ is the quantum yield. Among them, clε can be expressed by the optical density A and substituted into formula (1) to write

[0101] F=KI0Aφ (2)

[0102] When comparing the fluorescence intensities of the two solutions, the following relationship holds:

[0103] F1 / F2=K1I 01 A1φ1 / K2I 02 A2φ2 (3)

[0104] If the two use the same device and the same measurement conditions, that is, K1 = K2, I 01 =I 02 but:

[0105] F1 / F2=A1φ1 / A2φ2 (4)

[0106] Right now:

[0107] φ1 / φ2=F1A2 / F2A1 (5).

[0108] The present invention uses quinine sulfate (with known quantum yield) as a standard test solution, obtains the fluorescence spectra of the standard test solution and CDs through a fluorescence spectrometer, and uses an integration method to obtain the emission spectrum area F (that is, the total amount of emitted fluorescence). The fluorescence quantum yield of the CDs composite material can be calculated by a formula.

[0109] It is calculated that the quantum yield of b-CDs in comparative example 1 is 13.8%; the quantum yield of b-CDs@St in example 1 is 51.2%; the quantum yield of g-CDs in comparative example 2 is 14.1%; and the quantum yield of g-CDs@St in example 2 is 26.3%.

[0110] According to the above calculation results, it can be seen that the quantum yield of the material after compounding with starch is significantly improved, which shows that the present invention can make the carbon dots in a monodisperse state in the solid state by compounding the carbon dots with starch, effectively preventing the carbon dots from aggregating and improving the fluorescence quantum yield.

[0111] (III) Infrared spectrum test

[0112] The present invention takes the blue carbon dot starch composite material (b-CDs@St) of Example 1 and the green carbon dot starch composite material (g-CDs@St) of Example 2 as examples, and performs infrared absorption spectrum tests on them respectively, and the test results are as follows: Figure 5 shown.

[0113] And according to Figure 5 The test results show that the two carbon dots are at 2931 and 2884 cm -1 There is a C-H stretching vibration peak at 1634cm -1 There is a stretching vibration peak of C=O at 1452cm -1 There is a stretching vibration peak of C-N; combined with 3287cm -1The stretching vibration peak of N-H at , and the corresponding stretching vibration absorption peaks of C=O and C-N in the amide, indicate that amide groups are also produced during the carbonization process.

[0114] (IV) Application in fingerprint imprinting

[0115] The present invention takes the blue carbon dot starch composite material (b-CDs@St) of Example 1 and the green carbon dot starch composite material (g-CDs@St) of Example 2 as examples, and tests them according to the following methods to test their application effects in fingerprint imprinting:

[0116] Press your finger on glass and plastic to prepare a fingerprint sample, then dry it in the air for 1-2 minutes; finally sprinkle g-CDs@St and b-CDs@St on the fingerprint sample, and remove the excess powder with a brush. Irradiate it under fluorescent light and ultraviolet light respectively. The test results are as follows Figure 6 shown.

[0117] Figure 6 The fingerprints collected on glass and plastic plates are imprinted using green light carbon dot starch composite materials and blue light carbon dot starch composite materials as fluorescent markers. Figure 6 (a) is a fingerprint imprint photograph collected on a glass plate under sunlight using b-CDs@St as a fluorescent marker; Figure 6 (b) is a fingerprint imprint photograph collected on a glass plate under sunlight using g-CDs@St as a fluorescent marker; Figure 6 (c) is a fingerprint imprint photograph collected on a plastic plate under sunlight using b-CDs@St as a fluorescent marker; Figure 6 (d) is a fingerprint imprint photograph collected on a plastic plate under sunlight using g-CDs@St as a fluorescent marker; Figure 6 (e) is a fingerprint imprint photograph collected on a glass plate under ultraviolet light using b-CDs@St as a fluorescent marker; Figure 6 (f) is a fingerprint imprint photograph collected on a glass plate under ultraviolet light using g-CDs@St as a fluorescent marker; Figure 6 (g) is a fingerprint imprint photograph collected on a plastic plate under ultraviolet light using b-CDs@St as a fluorescent marker; Figure 6 (h) is a fingerprint imprint photograph collected on a plastic plate under ultraviolet light using g-CDs@St as a fluorescent marker.

[0118] from Figure 6It can be seen that compared to daylight, the details of the fingerprint can be clearly seen under ultraviolet light, while the existing liquid fluorescent markers will diffuse on the surface, which shows that the carbon dot starch composite material of the present invention effectively avoids this behavior, so that the carbon dot starch composite material of the present invention can be used as a fluorescent marker in fingerprint imprinting, opening up the application field of carbon dots.

[0119] Obviously, the above embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

Claims

1. A method for preparing a carbon dot starch composite material, characterized in that: The following steps are involved: Using citric acid as a carbon source and urea as a nitrogen source, the two are mixed in water to obtain a mixed solution; Using a hydrothermal reaction or microwave treatment method, the citric acid and urea in the mixed solution react to form carbon quantum dots, thereby obtaining a carbon dot solution; The carbon dot solution and starch are mixed evenly and then dried to obtain the carbon dot starch composite material.

2. The preparation method according to claim 1, characterized in that The mass ratio of the citric acid to the urea is 1:1.5-2.

5.

3. The preparation method according to claim 1, characterized in that: The mass ratio of the carbon dot solution to starch is 40-50:

1.

4. The preparation method according to claim 1, characterized in that: When the carbon dot solution is prepared by a hydrothermal reaction, the temperature of the hydrothermal reaction is 150-170°C.

5. The preparation method according to claim 4, characterized in that: The hydrothermal product of the hydrothermal reaction is also post-treated, and the post-treatment is carried out by the following steps: The hydrothermal product is filtered through a filter membrane to obtain a filtrate; the filtrate is dialyzed to obtain the carbon dot solution.

6. The preparation method according to claim 1, characterized in that: When the carbon dot solution is prepared by microwave treatment, the power of the microwave treatment is 600-800W.

7. The preparation method according to claim 6, characterized in that: The microwave product of the microwave treatment is also post-treated, and the post-treatment is carried out by the following steps: After the microwave product is dispersed in water, the mixture is centrifuged at least twice, and the obtained supernatant is the carbon dot solution.

8. The preparation method according to claim 1, characterized in that: The usage ratio of the water to the citric acid is 15-25 mL:1 g.

9. A carbon dot starch composite material prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the carbon dot starch composite material according to claim 9 in fingerprint imprinting.

Citation Information

Cited By

  • Hydrophobic carbon dots as well as preparation method and application thereof

    CN120059741A