Lubricant composition and production process thereof
Through lubricant compositions composed of erucamide and other materials and specific processes, the problems of lubricating oil being prone to water ingress, emulsification, and rusting under high humidity and low temperature are solved, achieving good anti-rust and lubrication properties, and being safe and environmentally friendly. The production process is simplified.
Patent Information
- Application Number
- CN202410723642.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2024-10-01
AI Technical Summary
Mechanical lubricating oil is prone to water intrusion, emulsification, rust, and condensation during use, which affects the lubrication effect. It also has poor shear resistance, rapid aging, and insufficient thermal conductivity and buffering performance.
A lubricant composition composed of erucamide, emulsified lubricating ester, polyether ester, potassium ricinoleate, self-emulsifying polyester, tall oil amide, amide rust inhibitor, preservative and defoamer, etc., through specific Made with mixing process steps including primary, secondary and tertiary mixing to ensure the stability and performance of the composition.
The lubricant achieves good anti-rust, emulsification and lubrication properties, is safe, non-toxic, odorless, environmentally friendly, and has a simple and fast production process.
Abstract
Description
Technical Field
[0001] The present invention relates to the field of lubricants, and in particular to a lubricant composition and a production process thereof. Background Art
[0002] At present, during the use of mechanical lubricating oil, water can easily enter the lubricating oil through the breathing hole or when the operating environment is humid, causing the lubricating oil to emulsify and the lubricating performance to decrease; the water in the lubricating oil can easily cause metal parts to rust, affecting operation; at low temperatures, the lubricating oil is easy to condense, affecting the lubrication effect; the mechanical shear resistance is poor and it is easy to age and fail; the oil has poor thermal conductivity and poor buffering performance. This has always been a problem in the development of lubricating oil. With the continuous development of lubricating oil technology, the technical breakthrough of lubricating oil has received more and more attention. Summary of the invention
[0003] The main purpose of the present invention is to provide a lubricant composition and a production process thereof, which can effectively solve the problems in the background technology.
[0004] To achieve the above object, the technical solution adopted by the present invention is:
[0005] A lubricant composition is prepared from the following components in parts by weight: 5-10 parts of erucamide, 5-10 parts of emulsified lubricating ester, 5-10 parts of polyether ester, 5-10 parts of potassium ricinoleate, 5-10 parts of self-emulsifying polyester, 5-10 parts of tall oil amide, 5-10 parts of amide rust inhibitor, 0.5-2 parts of preservative, 1-3 parts of defoamer and 60-70 parts of deionized water.
[0006] Preferably, it is made of the following components in parts by weight: 5-8 parts of erucamide, 5-8 parts of emulsified lubricating ester, 6-9 parts of polyether ester, 6-8 parts of potassium ricinoleate, 6-8 parts of self-emulsifying polyester, 6-8 parts of tall oil amide, 6-8 parts of amide rust inhibitor, 1-2 parts of preservative, 1-2 parts of defoaming agent, and 65-70 parts of deionized water.
[0007] Preferably, it is made of the following components in parts by weight: 7 parts of erucamide, 8 parts of emulsified lubricating ester, 7 parts of polyether ester, 7 parts of potassium ricinoleate, 8 parts of self-emulsifying polyester, 7 parts of tall oil amide, 8 parts of amide rust inhibitor, 1 part of preservative, 2 parts of defoamer, and 68 parts of deionized water.
[0008] Preferably, the preservative is kason.
[0009] Preferably, the defoaming agent is polyoxyethylene polyoxypropanolamine ether.
[0010] The production process steps of the lubricant composition are as follows:
[0011] ①, primary mixing: erucamide, emulsified lubricating ester, polyether ester, potassium ricinoleate, self-emulsifying polyester and tall oil amide are mixed and stirred, wherein the stirring time is 10-20 minutes and the mixing speed is 25-30r / min to obtain a primary mixed liquid;
[0012] ②, Secondary mixing: Add the primary mixed solution into deionized water for mixing and stirring, wherein the stirring time is 20-40min and the mixing speed is 50-60r / min to obtain a secondary mixed solution;
[0013] ③. Third mixing: add amide rust inhibitor, preservative and defoamer to the secondary mixed liquid, mix and stir again, the stirring number needs to be 3-4 times, each stirring for 3-5 minutes, stirring once every 1-2 minutes, and the stirring rate is 60-100r / min to finally obtain a lubricant composition.
[0014] Compared with the prior art, the present invention provides a lubricant composition and a production process thereof, which have the following beneficial effects: the lubricant is safe, non-toxic, odorless, and more environmentally friendly, and the lubricant production process is simple, quick and convenient, and the lubricant composition produced has good rust prevention, emulsification and lubrication properties. DETAILED DESCRIPTION
[0015] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.
[0016] Example 1
[0017] A lubricant composition is prepared from the following components in parts by weight: 7 parts of erucamide, 8 parts of emulsified lubricating ester, 7 parts of polyether ester, 7 parts of potassium ricinoleate, 8 parts of self-emulsifying polyester, 7 parts of tall oil amide, 8 parts of amide rust inhibitor, 1 part of preservative, 2 parts of defoaming agent and 68 parts of deionized water.
[0018] Among them, the preservative is Kathon and the defoaming agent is polyoxyethylene polyoxypropanolamine ether.
[0019] The production process steps of the lubricant composition are as follows:
[0020] ①, primary mixing: erucamide, emulsified lubricating ester, polyether ester, potassium ricinoleate, self-emulsifying polyester and tall oil amide are mixed and stirred, wherein the stirring time is 15 minutes and the mixing speed is 25r / min to obtain a primary mixed liquid;
[0021] ②, Secondary mixing: Add the primary mixed solution into deionized water for mixing and stirring, wherein the stirring time is 30 minutes and the mixing speed is 50r / min to obtain a secondary mixed solution;
[0022] ③. Third mixing: add amide rust inhibitor, preservative and defoamer to the secondary mixed liquid, mix and stir again, the stirring number needs to be carried out 3 times, each stirring for 5 minutes, stirring once every 2 minutes, and the stirring rate is 80r / min, finally obtaining a lubricant composition.
[0023] Example 2
[0024] A lubricant composition is prepared from the following components in parts by weight: 7 parts of erucamide, 8 parts of emulsified lubricating ester, 9 parts of polyether ester, 8 parts of potassium ricinoleate, 6 parts of self-emulsifying polyester, 7 parts of tall oil amide, 7 parts of amide rust inhibitor, 2 parts of preservative, 2 parts of defoaming agent, and 70 parts of deionized water.
[0025] Among them, the preservative is Kathon and the defoaming agent is polyoxyethylene polyoxypropanolamine ether.
[0026] The production process steps of the lubricant composition are as follows:
[0027] ①, primary mixing: erucamide, emulsified lubricating ester, polyether ester, potassium ricinoleate, self-emulsifying polyester and tall oil amide are mixed and stirred, wherein the stirring time is 15 minutes and the mixing speed is 26 r / min to obtain a primary mixed solution;
[0028] ②, Secondary mixing: Add the primary mixed solution into deionized water for mixing and stirring, wherein the stirring time is 35 minutes and the mixing speed is 50r / min to obtain a secondary mixed solution;
[0029] ③. Third mixing: add amide rust inhibitor, preservative and defoamer to the secondary mixed liquid, mix and stir again, the stirring number needs to be carried out 3 times, each stirring for 5 minutes, stirring once at an interval of 1 minute, and the stirring rate is 70r / min, finally obtaining a lubricant composition.
[0030] Example 3
[0031] A lubricant composition is prepared from the following components in parts by weight: 7 parts of erucamide, 8 parts of emulsified lubricating ester, 6 parts of polyether ester, 7 parts of potassium ricinoleate, 9 parts of self-emulsifying polyester, 10 parts of tall oil amide, 9 parts of amide rust inhibitor, 1.5 parts of preservative, 3 parts of defoamer and 70 parts of deionized water.
[0032] Among them, the preservative is Kathon and the defoaming agent is polyoxyethylene polyoxypropanolamine ether.
[0033] The production process steps of the lubricant composition are as follows:
[0034] ①, primary mixing: erucamide, emulsified lubricating ester, polyether ester, potassium ricinoleate, self-emulsifying polyester and tall oil amide are mixed and stirred, wherein the stirring time is 18 minutes and the mixing speed is 25r / min to obtain a primary mixed liquid;
[0035] ②, Secondary mixing: Add the primary mixed solution into deionized water for mixing and stirring, wherein the stirring time is 30 minutes and the mixing speed is 55r / min to obtain a secondary mixed solution;
[0036] ③. Third mixing: add amide rust inhibitor, preservative and defoamer to the secondary mixed liquid, mix and stir again, the stirring number needs to be carried out 4 times, each stirring for 3 minutes, stirring once every 2 minutes, and the stirring rate is 90r / min, finally obtaining a lubricant composition.
[0037] Example 4
[0038] A lubricant composition is prepared from the following components in parts by weight: 6 parts of erucamide, 8 parts of emulsified lubricating ester, 7 parts of polyether ester, 7 parts of potassium ricinoleate, 9 parts of self-emulsifying polyester, 7 parts of tall oil amide, 10 parts of amide rust inhibitor, 2 parts of preservative, 3 parts of defoaming agent and 62 parts of deionized water.
[0039] Among them, the preservative is Kathon and the defoaming agent is polyoxyethylene polyoxypropanolamine ether.
[0040] The production process steps of the lubricant composition are as follows:
[0041] ①, primary mixing: erucamide, emulsified lubricating ester, polyether ester, potassium ricinoleate, self-emulsifying polyester and tall oil amide are mixed and stirred, wherein the stirring time is 13 minutes and the mixing speed is 29 r / min to obtain a primary mixed liquid;
[0042] ②, Secondary mixing: Add the primary mixed solution into deionized water for mixing and stirring, wherein the stirring time is 32 minutes and the mixing speed is 60r / min to obtain a secondary mixed solution;
[0043] ③. Third mixing: add amide rust inhibitor, preservative and defoamer to the secondary mixed liquid, mix and stir again, the stirring number needs to be carried out 3 times, each stirring for 3 minutes, stirring once at an interval of 1 minute, and the stirring rate is 60r / min, finally obtaining a lubricant composition.
[0044] Example 5
[0045] A lubricant composition is prepared from the following components in parts by weight: 10 parts of erucamide, 10 parts of emulsified lubricating ester, 9 parts of polyether ester, 8 parts of potassium ricinoleate, 9 parts of self-emulsifying polyester, 10 parts of tall oil amide, 9 parts of amide rust inhibitor, 2 parts of preservative, 3 parts of defoamer and 70 parts of deionized water.
[0046] Among them, the preservative is Kathon and the defoaming agent is polyoxyethylene polyoxypropanolamine ether.
[0047] The production process steps of the lubricant composition are as follows:
[0048] ①, primary mixing: erucamide, emulsified lubricating ester, polyether ester, potassium ricinoleate, self-emulsifying polyester and tall oil amide are mixed and stirred, wherein the stirring time is 20 minutes and the mixing speed is 30r / min to obtain a primary mixed liquid;
[0049] ②, Secondary mixing: Add the primary mixed solution into deionized water for mixing and stirring, wherein the stirring time is 40 minutes and the mixing speed is 50r / min to obtain a secondary mixed solution;
[0050] ③. Third mixing: add amide rust inhibitor, preservative and defoamer to the secondary mixed liquid, mix and stir again, the stirring number needs to be carried out 3 times, each stirring for 4 minutes, stirring once at an interval of 1 minute, and the stirring rate is 80r / min to finally obtain a lubricant composition.
[0051] The invention discloses a lubricant composition and a production process thereof. The lubricant is safe, non-toxic, odorless and more environmentally friendly. The lubricant production process is simple, quick and convenient. The produced lubricant composition has good rust prevention, emulsification and lubrication properties.
[0052] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A lubricant composition, characterized in that , made of the following components in parts by weight: 5-10 parts of erucamide, 5-10 parts of emulsified lubricating ester, 5-10 parts of polyether ester, 5-10 parts of potassium ricinoleate, 5-10 parts of self-emulsifying polyester, 5-10 parts of tall oil amide, 5-10 parts of amide rust inhibitor, 0.5-2 parts of preservative, 1-3 parts of defoaming agent, and 60-70 parts of deionized water.
2. A lubricant composition according to claim 1, characterized in that , made of the following components in parts by weight: 5-8 parts of erucamide, 5-8 parts of emulsified lubricating ester, 6-9 parts of polyether ester, 6-8 parts of potassium ricinoleate, 6-8 parts of self-emulsifying polyester, 6-8 parts of tall oil amide, 6-8 parts of amide rust inhibitor, 1-2 parts of preservative, 1-2 parts of defoaming agent, and 65-70 parts of deionized water.
3. A lubricant composition according to claim 1, characterized in that , made of the following components in parts by weight: 7 parts of erucamide, 8 parts of emulsified lubricating ester, 7 parts of polyether ester, 7 parts of potassium ricinoleate, 8 parts of self-emulsifying polyester, 7 parts of tall oil amide, 8 parts of amide rust inhibitor, 1 part of preservative, 2 parts of defoamer, and 68 parts of deionized water.
4. A lubricant composition according to claim 2, characterized in that: The preservative is Kathon.
5. A lubricant composition according to claim 4, characterized in that: The defoamer is polyoxyethylene polyoxypropanolamine ether.
6. A process for producing a lubricant composition, comprising producing the lubricant composition according to any one of claims 1 to 4, characterized in that: The following steps are involved: ①, primary mixing: erucamide, emulsified lubricating ester, polyether ester, potassium ricinoleate, self-emulsifying polyester and tall oil amide are mixed and stirred, wherein the stirring time is 10-20 minutes and the mixing speed is 25-30r / min to obtain a primary mixed liquid; ②, Secondary mixing: Add the primary mixed solution into deionized water for mixing and stirring, wherein the stirring time is 20-40min and the mixing speed is 50-60r / min to obtain a secondary mixed solution; ③. Third mixing: add amide rust inhibitor, preservative and defoamer to the secondary mixed liquid, mix and stir again, the stirring number needs to be 3-4 times, each stirring for 3-5 minutes, stirring once every 1-2 minutes, and the stirring rate is 60-100r / min to finally obtain a lubricant composition.