High-temperature heating preparation process for automobile suspension spring
By using a stepping heating furnace and high-temperature oxidative heating method in the production of automobile suspension springs, the problem of complete decarbonization caused by the low-temperature heating process is solved, achieving zero complete decarbonization and improving product quality, improving production efficiency.
Patent Information
- Application Number
- CN202410693758.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-31
- Publication Date
- 2024-10-01
AI Technical Summary
When the existing low-temperature heating process is used to produce automobile suspension spring steel, it is easy to cause complete decarburization of the surface, affecting the fatigue life. The process failure rate is high, the production efficiency is low, and it cannot meet the quality requirements of the new process.
A stepping heating furnace is used, which is divided into a preheating section, a heating section, a second heating section and a soaking section. The high temperature is heated to 1220°C to 1260°C and maintained in an oxidizing atmosphere for a certain period of time. The heating time is controlled to optimize the furnace gas atmosphere. and heating temperature, using high-temperature oxidative heating method to reduce the thickness of the decarburization layer.
It achieves zero decarbonization, reduces the thickness of the decarburization layer, improves product quality, meets customer requirements, improves production efficiency, and avoids process failures.
Smart Images

Figure CN118726731A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of suspension spring processing, in particular to a high-temperature heating preparation process for an automobile suspension spring. Background Art
[0002] At present, the requirements for the quality of spring products in automobile parts are becoming increasingly stringent, especially after downstream users gradually replaced the production equipment and process technology with a higher degree of automation. The requirements for raw material surface quality, decarburization performance and organizational qualification rate are more stringent, which restricts the production efficiency and product quality of downstream users. Decarburization on the surface of spring steel will seriously damage the fatigue performance of the spring, especially when the ferrite is fully decarburized on the surface of wire spring steel, the fatigue limit life of the spring can be reduced by 50%. 55SiCr spring steel users have gradually updated from the original hot coil spring to cold coil spring production, and the original wire decarburization quality can no longer meet the quality requirements of the new process.
[0003] In the production process of spring steel, low temperature and rapid heating process is the mainstream process. Due to different equipment capabilities, most manufacturers use the starting rolling temperature between 850 and 1000℃ when producing spring steel. Low temperature heating process can effectively control the thickness of the decarburized layer of spring steel, but this type of heating process still has the following limitations in actual production.
[0004] 55SiCr silicon-containing spring steel is prone to surface full decarburization. When the heating temperature is ≥980℃, silicon-containing steel begins to produce partial full decarburization, and the surface of the continuous casting billet often has partial full decarburization. If a low-temperature heating process is used, silicon-based spring steel generally needs to adopt an ultra-low temperature rolling temperature of 830-870℃, combined with the full peeling treatment of the billet surface to solve the problem of surface full decarburization. This not only puts too high demands on the capacity of the rough rolling equipment, but also increases the processing cost. The low-temperature heating process has a low heating temperature and a short time, so the segregation of the billet cannot be improved in the heating process, which is not conducive to the improvement of the fatigue life of the finished product. The low-temperature heating process has high requirements for the smooth production, and the probability of process failure in production is high, which can easily cause heating overtime furnace unloading accidents. When scheduling production, it is also easy to adopt empty furnace feeding when heating furnace feeding because of the large difference in heating temperature with other steel grades, which reduces production efficiency.
[0005] Wire spring steel product 55SiCr is used to make automobile suspension springs, which has high requirements for the decarburization layer that affects fatigue life (full decarburization is not allowed). Traditionally, low-temperature fast firing is generally used to control full decarburization, but the process window is narrow. Improper control can easily lead to uneven heating and too low center temperature, resulting in poor density in the center of the rolled piece. Fractures occurred during customer use. Summary of the invention
[0006] The object of the present invention is to provide a high temperature heating preparation process for automobile suspension springs to solve the problems raised in the above background technology.
[0007] To achieve the above object, the present invention provides the following technical solution: a high temperature heating preparation process for an automobile suspension spring, the preparation process comprising the following steps:
[0008] The 55SiCr steel billet for automobile suspension spring is placed in a walking beam heating furnace, which is divided into a preheating section, a first heating section, a second heating section and a soaking section;
[0009] In the preheating section, the steel billet is preliminarily heated to remove surface moisture and oil;
[0010] In the heating stage, the temperature is gradually raised to a temperature range of 850-1000°C for preheating;
[0011] In the second heating stage and the soaking stage, the steel billet is heated to a high temperature range of 1220°C to 1260°C and maintained for a certain period of time;
[0012] In the high temperature range of 1220℃ to 1260℃, the atmosphere in the furnace is controlled to be an oxidizing atmosphere to increase the oxidation and burning rate of the steel billet surface, thereby reducing the thickness of the decarburized layer;
[0013] The heating time in the high temperature section is controlled between 27 minutes and 60 minutes to ensure the elimination of the original decarburization layer of the billet and the decarburization layer generated in the low temperature heating section;
[0014] After heating is completed, the steel billet is subsequently rolled and cooled to finally obtain the automobile suspension spring product.
[0015] Preferably, the method further includes analyzing factors affecting decarburization, including analyzing the influence of carbon potential on decarburization and analyzing the influence of heating time on decarburization;
[0016] The influence of carbon potential on decarburization was analyzed, including the influence of furnace gas atmosphere on carbon potential difference. High-coke mixed gas was used as heating furnace fuel. The ratio of blast furnace gas and coke oven gas was 0.47:0.53. The composition of the fuel gas was: H2: 32.85-33.55%, CH4: 13.45-14.85%, CO: 15.21-18.0%, C2H2: 1.0-2.1%, O2: 0.21-0.43%, CO2: 0.75-1.65, N2: 23.2-29.15%. The air-fuel ratio of the reducing atmosphere was controlled at 1.8-2.0, and the air-fuel ratio of the oxidizing atmosphere was controlled at 2.8-3.0.
[0017] Preferably, analyzing the effect of carbon potential on decarburization also includes analyzing the effect of heating temperature on carbon potential difference, and controlling the heating temperature in two temperature ranges of ≤1050°C and 1220-1260°C. When heating in the temperature range of ≤1050°C, the furnace gas atmosphere of the heating furnace is controlled to be a reducing atmosphere, which is beneficial to reducing the thickness of the decarburization layer; when heating in the temperature range of 1220-1260°C, the change in carbon activity of the furnace gas approaches zero, and the effect of the furnace gas atmosphere on the decarburization trend of the steel changes little. The oxidizing furnace gas atmosphere is more conducive to increasing the oxidation and burning rate of the billet surface. At this time, the oxidation and burning rate is greater than the increase rate of the decarburization layer, which is generally more conducive to reducing the thickness of the decarburization layer. The furnace gas atmosphere should be controlled as an oxidizing atmosphere.
[0018] Preferably, the effect of heating time on decarburization is analyzed. The square root of the heating time is proportional to the thickness of the decarburized layer generated during the heating process. The inflection point of the increase in decarburization rate within the same heating time is 1000°C. When heating in a temperature range of ≤1050°C, the heating process of the spring steel should control the heating time in the high temperature range of ≥1000°C, and the heating time in the temperature range of ≤1050°C should be controlled within 30 to 34 minutes.
[0019] When heating at a temperature range of 1220-1260°C, the final decarburization layer thickness of the finished product is the combined result of surface decarburization and oxidation burning. In an oxidizing atmosphere, the burning rate is greater than the rate of decarburization formation. The heating time at 1220-1260°C is controlled at 27-31 minutes.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The high-temperature heating preparation process for automobile suspension springs proposed in the present invention is implemented in a walking beam heating furnace, which is divided into a preheating section, a heating section, a second heating section, and a soaking section. The high-temperature heating process is implemented by heat preservation at a high temperature of 1220-1260°C in the second heating section and the soaking section. During high-temperature heating, the oxidation rate of the steel billet surface is greater than the diffusion rate of carbon, so full decarburization can be achieved to zero.
[0022] By optimizing the heating process parameters, the high-temperature burning method is used to control the steel for automobile suspension springs; the problems existing in the low-temperature heating process are solved, the thickness of the decarburized layer is reduced and the formation of a full decarburized layer is avoided; the inhibitory effect on the thickness of the decarburized layer on the surface of the automobile suspension spring product in the temperature range of 1220-1260°C is achieved. Under the conditions of 1220-1260°C, an oxidizing furnace atmosphere is used to effectively remove the decarburized layer on the surface of the 180mm×240mm cross-section blank by burning, which is more conducive to reducing the thickness of the decarburized layer and avoiding the formation of a full decarburized layer. The high-temperature oxidative heating process is not sensitive to the residence time of the spring steel blank in the high-temperature section. Properly extending the residence time in the high-temperature section is more conducive to reducing the thickness of the decarburized layer. The patent of this invention provides a new high-temperature heating process that is first applied to the new technology of 55SiCr for automobile suspension spring products, and has been successfully applied to mass production, fully meeting the requirements of customers. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Schematic diagram of the effect of CO concentration on 55SiCr decarburization in the present invention;
[0024] Figure 2 Schematic diagram of the effect of temperature on the carbon potential in steel and furnace gas and the carbon potential difference between the two;
[0025] Figure 3 This is a schematic diagram of the decarburized layer thickness of 55SiCr at different heating temperatures of the present invention;
[0026] Figure 4 This is a schematic diagram of the decarburized layer on the surface of the finished product of the heating process in the temperature range of ≤1050°C of the present invention;
[0027] Figure 5 This is a schematic diagram of the decarburization layer on the surface of the finished product of the rapid heating process in the temperature range of 1220-1260°C of the present invention. DETAILED DESCRIPTION
[0028] In order to make the purpose and technical solution of the present invention clearly and completely described, and the advantages more clearly understood, the embodiments of the present invention are further described in detail with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are part of the embodiments of the present invention, rather than all of the embodiments, and are only used to explain the embodiments of the present invention, and are not used to limit the embodiments of the present invention. All other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Embodiment 1
[0030] See also Figures 1 to 3 The present invention provides a technical solution: a high temperature heating preparation process for an automobile suspension spring, the preparation process comprising the following steps:
[0031] The 55SiCr steel billet for automobile suspension spring is placed in a walking beam heating furnace, which is divided into a preheating section, a first heating section, a second heating section and a soaking section;
[0032] In the preheating section, the steel billet is preliminarily heated to remove surface moisture and oil;
[0033] In the heating stage, the temperature is gradually raised to a temperature range of 850-1000°C for preheating;
[0034] In the second heating stage and the soaking stage, the steel billet is heated to a high temperature range of 1220°C to 1260°C and maintained for a certain period of time;
[0035] In the high temperature range of 1220℃ to 1260℃, the atmosphere in the furnace is controlled to be an oxidizing atmosphere to increase the oxidation and burning rate of the steel billet surface, thereby reducing the thickness of the decarburized layer;
[0036] The heating time in the high temperature section is controlled between 27 minutes and 60 minutes to ensure the elimination of the original decarburization layer of the billet and the decarburization layer generated in the low temperature heating section;
[0037] After heating is completed, the steel billet is subsequently rolled and cooled to finally obtain the automobile suspension spring product.
[0038] It also includes: optimizing the heating process and conducting research on high-temperature heating controlled decarburization process.
[0039] 1. Factors affecting decarburization: The factors affecting decarburization are mainly carbon potential, furnace atmosphere, heating temperature and heating time. The carbon potential difference between the carbon content in the steel and the furnace atmosphere is the fundamental driving force for decarburization on the steel surface during the heating process. The greater the carbon potential difference between the two, the greater the decarburization tendency of the steel during the heating process, and the smaller the carbon potential difference, the smaller the decarburization tendency. The heating time is another key factor that determines the thickness of the decarburization layer on the steel surface during the heating process.
[0040] 2. Factors affecting carbon potential: Carbon potential is a thermodynamic property of the atmosphere, indicating a balance ability of the atmosphere. Reducing the carbon potential difference between the billet and the heating furnace atmosphere can effectively control decarburization. In addition to the steel grade characteristics of the steel itself, the factors affecting the carbon potential difference mainly include the furnace atmosphere and the heating temperature.
[0041] (1) Effect of furnace atmosphere on carbon potential difference: Different gases have different effects on the decarburization of steel. The main gases in industrial heating furnaces are CO, CO2, O2, N2, H2, CH4, H2O, etc. Among them, H2O has the strongest decarburization ability, followed by CO2 and O2, and then H2; while CO and CH4 will inhibit the decarburization of steel. Figure 1The figure shows the change of 55SiCr surface decarburization with the CO content in the furnace gas. The experimental heating temperature is 1100℃ and the heating time is 60min.
[0042] from Figure 1 It can be concluded that when the CO concentration in the gas is lower than 30%, the change of CO content has little effect on the thickness of the decarburized layer on the steel surface.
[0043] High coke mixed gas is used as heating furnace fuel, and the ratio of blast furnace gas to coke oven gas is 0.47:0.53. The main components of the gas are: H2 (32.85-33.55%), CH4 (13.45-14.85%), CO (15.21-18.0%), C2H2 (1.0-2.1), O2 (0.21-0.43%), CO2 (0.75-1.65), N2 (23.2-29.15%). Considering the comprehensive effects of CO, CH4 and H2 in the main combustible gases in the gas.
[0044] For the setting of the air-fuel ratio of the heating furnace, fine-tuning is still carried out on the premise of ensuring combustion efficiency and complete combustion of the fuel. The air-fuel ratio of the reducing atmosphere is controlled at 1.8-2.0, and the air-fuel ratio of the oxidizing atmosphere is controlled at 2.8-3.0.
[0045] (2) Effect of heating temperature on carbon potential difference: When steel is heated, there is a carbon chemical potential gradient between its surface and the furnace gas, which triggers the decarburization reaction. The power of decarburization depends on the difference between the carbon potential of the furnace gas and the carbon content in the steel, as well as the diffusion rate of carbon in the metal, both of which are directly related to the heating temperature.
[0046] The carbon potential (chemical potential) of steel and furnace gas can be obtained by thermodynamic calculation. For a certain mixing ratio of fuel gas, the carbon activity of gas at different temperatures (with graphite as the standard state) can be obtained by formula (1),
[0047] (2) Calculation shows that T is the absolute temperature.
[0048] CO2+C=2CO (1)
[0049] ΔG 0 =170707.2-174.47T (2)
[0050] The carbon activity in the metal is mainly affected by the carbon and silicon content in the austenite (with graphite as the standard state). By consulting the "Handbook of Commonly Used Icons for Steelmaking" and considering the effect of silicon on carbon, the carbon activity of 55SiCr at different heating temperatures can be obtained.
[0051] Figure 2The carbon potential in 55SiCr, the carbon potential of furnace gas (CO content is 96.77%) and the carbon potential difference between the two change at different heating temperatures. Figure 3 The decarburized layer thickness of 55SiCr at different heating temperatures was observed after the 55SiCr was heated in a furnace with a CO content of 96.77% for 60 minutes.
[0052] from Figure 2 It can be seen that as the temperature increases, the carbon potential of the furnace gas continues to decrease, but the rate continues to decrease. The carbon potential value in 55SiCr also gradually decreases, but the rate of decrease first decreases and then increases at 1150℃. Therefore, the trend of the carbon potential difference between the two with temperature is that it first increases and then decreases, with a peak at 1150℃.
[0053] Combination Figure 3 It can be seen that under certain furnace atmosphere and heating time, the variation trend of the decarburized layer thickness of 55SiCr with heating temperature is consistent with the variation trend of carbon potential difference with temperature.
[0054] Judging from the trend of the decarburization layer thickness changing with heating temperature, in order to control the decarburization layer thickness, the most sensitive temperature range of 1100-1180℃ should be avoided when selecting the heating temperature.
[0055] The two temperature ranges of ≤1050℃ and 1220~1260℃ can significantly reduce the carbon potential difference, which is more conducive to controlling decarburization. When low-temperature heating is adopted, the furnace gas atmosphere of the heating furnace should be controlled as a reducing atmosphere, which is more conducive to reducing the thickness of the decarburization layer. When heating at high temperature, because the change of furnace gas carbon activity in this temperature range approaches zero, the effect of furnace gas atmosphere on the decarburization trend of steel changes little. However, the oxidizing furnace gas atmosphere is more conducive to increasing the oxidation and burning rate of the billet surface. At this time, the oxidation and burning rate is greater than the increase rate of the decarburization layer, which is generally more conducive to reducing the thickness of the decarburization layer. Therefore, when using the high-temperature heating process, the furnace gas atmosphere should be controlled as an oxidizing atmosphere.
[0056] 3. The influence of heating time on decarburization: The square root of heating time is proportional to the thickness of the decarburized layer produced during the heating process, so the heating time should be strictly controlled when heating spring steel. From the trend of the influence of heating temperature change on the change of decarburized layer thickness, the inflection point of the increase in decarburization rate within the same heating time is around 1000℃. Therefore, when using the low-temperature heating process, the heating process of spring steel should focus on controlling the heating time of the high-temperature section ≥1000℃.
[0057] When using a high-temperature heating process of 1220-1260℃, the thickness of the final decarburized layer of the finished product is the combined result of two factors: surface decarburization and oxidation burning. The burning rate is greater than the rate of decarburization formation in an oxidizing atmosphere. Therefore, the heating time of the high-temperature section is not very sensitive. At the same time, from the perspective of eliminating the original decarburized layer of the billet and the decarburized layer generated by the heating low-temperature section, the heating time of the high-temperature section must meet a lower limit, and the shorter the better.
[0058] Embodiment 2
[0059] Refer to the attached Figure 4 and Figure 5 As shown, based on the first embodiment, the following contents are proposed:
[0060] (1) Production process: blast furnace molten iron - molten iron, ferroalloy - converter smelting - refining - continuous casting - inspection - storage of ingots - walking beam heating furnace - roughing mill (1-7 trains) - intermediate rolling mill (8-13 trains) - pre-finishing mill (14-21 trains) - pre-water cooling - finishing mill (22-25 trains) - water cooling - sizing mill (26-29 trains) - water cooling - laying head - air cooling - coiling - PF line - inspection - packaging - storage.
[0061] (2) High temperature heating process practice
[0062] According to the heating process of the test plan, φ20mm specification 55SiCr spring steel was produced using 180mm×240mm cross-section billets. Table 1 shows the heating conditions of the trial rolling batch.
[0063] Table 1 Heating and decarburization of spring steel produced by high temperature oxidation process
[0064]
[0065] Figure 4 and Figure 5 φ20mm under low temperature oxidation heating process and high temperature rapid heating process respectively.
[0066] Metallographic photograph of the surface decarburized layer of 55SiCr wire.
[0067] from Figure 4 and Figure 5 It can be seen that the 55SiCr spring steel produced by the conventional low-temperature rapid heating process has full decarburization on the surface of the finished product in the form of dots and blocks (5-7), with a depth of 0-0.019mm and 0-0.015mm, but there is obvious full decarburization. However, the surface of the finished product produced by the high-temperature oxidizing atmosphere heating process has no full decarburization at all, and the thickness of the decarburization layer is almost zero.
[0068] Embodiment 3
[0069] On the basis of Example 2, a high temperature heating preparation process for automobile suspension springs based on an oxidizing atmosphere is proposed;
[0070] Raw material preparation: 55SiCr steel billet for automobile suspension spring is selected as raw material.
[0071] Heating process:
[0072] Preheating section: The steel billet is placed in the preheating section of the walking beam heating furnace for preliminary heating to remove surface moisture and oil.
[0073] Heating stage: gradually raise the temperature to a temperature range of 850-1000°C for preheating treatment.
[0074] Second heating stage and soaking stage: heat the steel billet in a high temperature range of 1220℃ to 1260℃ and keep it for a certain period of time. During this period, the atmosphere in the furnace is controlled to be an oxidizing atmosphere to accelerate the oxidation and burning rate of the steel billet surface and reduce the thickness of the decarburized layer.
[0075] Subsequent processing: After heating, the steel billet is subjected to subsequent rolling and cooling treatment to obtain automobile suspension spring products.
[0076] Features analysis:
[0077] Application of oxidizing atmosphere: In the second heating stage and the soaking stage, by controlling the atmosphere in the furnace to an oxidizing atmosphere, the thickness of the decarburized layer is effectively reduced and the product quality is improved.
[0078] Control of heating time: The heating time in the high temperature section is controlled between 27 minutes and 60 minutes to ensure the elimination of the original decarburization layer of the billet and the decarburization layer generated in the low temperature heating section.
[0079] Embodiment 4
[0080] Based on Example 3, an optimized preparation process considering the effects of carbon potential and heating time on decarburization is proposed;
[0081] Process steps:
[0082] Raw material preparation: 55SiCr steel billet for automobile suspension spring is selected as raw material.
[0083] Heating process: atmosphere and temperature control: when heating in the temperature range of ≤1050℃, the furnace gas atmosphere is controlled to be a reducing atmosphere to reduce the thickness of the decarburized layer; when heating in the temperature range of 1220~1260℃, the furnace gas atmosphere is controlled to be an oxidizing atmosphere to increase the oxidation burning rate of the billet surface and reduce the thickness of the decarburized layer.
[0084] Heating time control: When heating in the temperature range of ≤1050℃, the heating time is controlled within 30-34min; when heating in the temperature range of 1220-1260℃, the heating time is controlled within 27-31min.
[0085] Subsequent processing: After heating, subsequent rolling and cooling processes are carried out to obtain automobile suspension spring products.
[0086] Features analysis:
[0087] Relationship between carbon potential and decarburization: By analyzing the influence of carbon potential on decarburization, the furnace atmosphere and heating temperature are reasonably controlled to achieve effective control of the decarburization layer thickness.
[0088] Optimization of heating time: Based on the analysis of the impact of heating time on decarburization, the heating time was optimized to further improve product quality and production efficiency.
[0089] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A high temperature heating preparation process for automobile suspension springs, characterized in that: The preparation process comprises the following steps: The 55SiCr steel billet for automobile suspension spring is placed in a walking beam heating furnace, which is divided into a preheating section, a first heating section, a second heating section and a soaking section; In the preheating section, the steel billet is preliminarily heated to remove surface moisture and oil; In the heating stage, the temperature is gradually raised to a temperature range of 850-1000°C for preheating; In the second heating stage and the soaking stage, the steel billet is heated to a high temperature range of 1220°C to 1260°C and maintained for a certain period of time; In the high temperature range of 1220℃ to 1260℃, the atmosphere in the furnace is controlled to be an oxidizing atmosphere to increase the oxidation and burning rate of the steel billet surface, thereby reducing the thickness of the decarburized layer; The heating time in the high temperature section is controlled between 27 minutes and 60 minutes to ensure the elimination of the original decarburization layer of the billet and the decarburization layer generated in the low temperature heating section; After heating is completed, the steel billet is subsequently rolled and cooled to finally obtain the automobile suspension spring product.
2. The high temperature heating preparation process for automobile suspension spring according to claim 1, characterized in that: It also includes the analysis of factors affecting decarburization, including the analysis of the effect of carbon potential on decarburization and the analysis of the effect of heating time on decarburization; The influence of carbon potential on decarburization was analyzed, including the influence of furnace gas atmosphere on carbon potential difference. High-coke mixed gas was used as heating furnace fuel. The ratio of blast furnace gas and coke oven gas was 0.47:0.
53. The composition of the fuel gas was: H2: 32.85-33.55%, CH4: 13.45-14.85%, CO: 15.21-18.0%, C2H2: 1.0-2.1%, O2: 0.21-0.43%, CO2: 0.75-1.65, N2: 23.2-29.15%. The air-fuel ratio of the reducing atmosphere was controlled at 1.8-2.0, and the air-fuel ratio of the oxidizing atmosphere was controlled at 2.8-3.
0.
3. The high temperature heating preparation process for automobile suspension spring according to claim 2, characterized in that: Analysis of the effect of carbon potential on decarburization also includes analysis of the effect of heating temperature on carbon potential difference. The heating temperature is controlled in two temperature ranges of ≤1050℃ and 1220-1260℃. When heating in the temperature range of ≤1050℃, the furnace gas atmosphere of the heating furnace is controlled to be a reducing atmosphere, which is beneficial to reducing the thickness of the decarburization layer. When heating in the temperature range of 1220-1260℃, the change in carbon activity of the furnace gas approaches zero, and the effect of the furnace gas atmosphere on the decarburization trend of steel is very small. The oxidizing furnace gas atmosphere is more conducive to increasing the oxidation and burning rate of the billet surface. At this time, the oxidation and burning rate is greater than the increase rate of the decarburization layer, which is generally more conducive to reducing the thickness of the decarburization layer. The furnace gas atmosphere should be controlled as an oxidizing atmosphere.
4. The high temperature heating preparation process for automobile suspension spring according to claim 1, characterized in that: Analyze the effect of heating time on decarburization. The square root of heating time is proportional to the thickness of the decarburized layer produced during the heating process. The inflection point of the increase in decarburization rate within the same heating time is 1000℃. When heating in the temperature range of ≤1050℃, the heating process of spring steel should control the heating time in the high temperature range of ≥1000℃, and the heating time in the temperature range of ≤1050℃ should be controlled within 30-34min. When heating at a temperature range of 1220-1260°C, the final decarburization layer thickness of the finished product is the combined result of surface decarburization and oxidation burning. In an oxidizing atmosphere, the burning rate is greater than the rate of decarburization formation. The heating time at 1220-1260°C is controlled at 27-31 minutes.