Efficient extraction method for battery-grade nickel sulfate solution

Through the joint extraction process of P204 and C272, the problems of long process flow and resource waste in the separation and recovery of nickel and cobalt in the existing technology are solved, and efficient extraction of battery-grade nickel sulfate solution is achieved, reducing operating costs and improving resource utilization. .

CN118726762APending Publication Date: 2024-10-01JINCHUAN GROUP NICKEL COBALT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410894944.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing solvent extraction method in the separation and recovery of nickel and cobalt has problems such as long process flow, low saponification efficiency, multiple equipment, difficult control, high wastewater treatment costs, and high equipment and material requirements, especially when producing battery-grade nickel sulfate solution. Low cost and high resource waste.

Method used

A joint extraction process using P204 and C272 to extract the impurity-removing organic phase and nickel-cobalt separation organic phase is used, sodium soap and nickel soap are simultaneously treated through sodium hydroxide treatment, and sodium washing and nickel washing liquid are used for extraction to achieve resource reuse and The process flow is shortened and the number of equipment and investment are reduced.

Benefits of technology

It improves saponification efficiency, shortens the process flow, reduces operating costs, reduces wastewater treatment costs, improves resource utilization through resource reuse, and meets the chemical composition standards of battery-grade nickel sulfate solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
Patent Text Reader

Abstract

The invention provides an efficient extraction method for a battery-grade nickel sulfate solution, belongs to the technical field of wet-process non-ferrous metallurgy extraction, and solves the problems of low efficiency, resource waste and high cost in the existing extraction process for producing the battery-grade nickel sulfate solution. The efficient extraction method comprises the following steps: synchronously carrying out sodium soap and nickel soap treatment on P204 and a light white oil material; after washing sodium, mixing with a crude nickel sulfate solution, and extracting to obtain P204 raffinate; the P204 loaded organic phase can be repeatedly used after being subjected to washing, reverse extraction and iron washing; synchronously carrying out sodium soap and nickel soap treatment on C272 and the light white oil material, washing sodium, mixing with the P204 raffinate, and extracting to obtain C272 raffinate; deoiling the C272 raffinate to obtain a battery-grade nickel sulfate solution; the C272 loaded organic phase can be repeatedly used after being subjected to washing, reverse extraction and iron washing. According to the method, the nickel washing liquid and the raffinate are recycled, the extraction process flow is shortened, the recycling of resources such as the nickel washing liquid is increased, the equipment investment is reduced, and the production and operation cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of wet nonferrous metallurgy extraction, and in particular relates to a high-efficiency extraction method for battery-grade nickel sulfate solution. Background Art

[0002] At present, the solvent extraction method has the advantages of high selectivity, high recovery rate, simple process, continuous operation and easy automation in the application of nickel and cobalt separation and recovery. It is widely used and mature, and has a higher depth of impurity removal than chemical precipitation, ion exchange and adsorption methods.

[0003] For the production of battery-grade nickel sulfate solution, the solvent extraction method mainly includes the processes of sodium soap, nickel soap, sodium washing, extraction, nickel washing, stripping and iron washing regeneration. Among them, the parameter control of sodium washing, sodium soap and nickel soap is particularly important. The following problems exist in the current extraction production system: 1. Sodium soap and nickel soap are carried out in a distributed manner, which has the problems of long process flow, low saponification efficiency, many extraction equipment, great control difficulty and high operating cost; 2. P204 stripping liquid is discharged in the form of wastewater, resulting in increased wastewater treatment costs; 3. The use of hydrochloric acid for iron washing regeneration increases the requirements for equipment and materials and increases equipment investment. At the same time, the liquid after iron washing contains chloride ions and cannot enter the leaching system, resulting in increased production and operation costs of the entire system. Summary of the invention

[0004] The purpose of the present invention is to provide a method for efficiently extracting a battery-grade nickel sulfate solution, so as to solve the problems of low efficiency, waste of resources and high cost in the existing production of battery-grade nickel sulfate solution extraction.

[0005] The technical solution of the present invention is: a method for efficiently extracting battery-grade nickel sulfate solution, comprising the following steps: Step 1: P204 and light white oil are mixed evenly to obtain an organic phase for extraction and impurity removal, and the organic phase for extraction and impurity removal is treated with sodium soap and nickel soap by sodium hydroxide and P204 raffinate to obtain an organic phase, and the organic phase is washed with sodium by P204 nickel washing solution, and the organic phase is mixed with a crude nickel sulfate solution after sodium washing, and the mixed phase is extracted to obtain a P204 raffinate; Step 2: The mixed solution in step 1 is extracted to obtain a P204-loaded organic phase, which can be repeatedly used as a P204 nickel-washing solution for sodium washing after washing, and the P204-loaded organic phase is continuously stripped and iron-washed after washing, and the stripping solution is back-leached to supplement copper during stripping, and the iron-washing acid can be reused as a raw material after being mixed with light white oil after being back-leached; Step 3: C272 and light white oil are mixed evenly to obtain a nickel-cobalt separation organic phase, and the nickel-cobalt separation organic phase is treated with sodium soap and nickel soap using sodium hydroxide and C272 raffinate to obtain an organic phase, and the organic phase is washed with sodium using C272 nickel washing solution, and the organic phase is mixed with the P204 raffinate in step 1 after sodium washing, and the mixed phase is extracted to obtain C272 raffinate; Step 4: removing oil from the C272 raffinate in step 3 to obtain a battery-grade nickel sulfate solution; Step 5: The mixed solution in step 3 is extracted to obtain a C272 loaded organic phase, which can be washed and reused as a C272 nickel washing solution for sodium washing. The C272 loaded organic phase is washed and further stripped and iron washed. During stripping, the C272 stripping solution is exported as a cobalt sulfate solution, and the iron washing acid can be used as a raw material and mixed with light white oil in a proportion for repeated use.

[0006] As a further improvement of the present invention, in step 1, the raw material of the crude nickel sulfate solution is high nickel matte, and the high nickel matte is subjected to two stages of normal pressure and two stages of pressurization to produce a leaching solution as a crude nickel sulfate solution, the pH of the crude nickel sulfate solution is 3.5-4.0, and the chemical composition content of the crude nickel sulfate solution is: Ni: 102-106 g / L, Cu: 0.4-0.6 / L, Fe: 0.1-0.4 g / L, Co: 1.0- 1.5g / L, Zn: 0.8-1.2g / L, Ca: 0.3-0.6g / L, Mg: 0.4-0.7g / L, Si: 0.06-0.1g / L, Mn: 0.04 -0.08g / L, Pb: 0.01-0.04g / L, Na: 0.08-0.15g / L, Cl: 0.03-0.06g / L, F: 0.01-0.04g / L.

[0007] As a further improvement of the present invention, in step one, sodium soap and nickel soap are simultaneously treated using 30-32% sodium hydroxide and P204 raffinate containing 90-110 g / L of nickel, the pH of the sodium soap and nickel soap in the P204 raffinate is 3.5-4.5, and the P204 nickel washing solution contains 30-60 g / L of nickel and has a pH of 3.0-4.0.

[0008] As a further improvement of the present invention, in step 1, the mixed solution is extracted at a reaction temperature of 40°C-45°C and a ratio of O / A=1.2-1.5:1.

[0009] As a further improvement of the present invention, in step 2, the P204 stripping solution is a solution containing 15-30 g / L copper, ≤0.1 g / L nickel, ≤0.1 g / L cobalt, and a pH of 1.5-2.5.

[0010] As a further improvement of the present invention, in step three, the mixed solution is extracted at a reaction temperature of 45°C-50°C and a ratio of O / A=2-2.5:1; the C272 nickel washing solution contains 30-60 g / L nickel and has a pH of 3.0-4.0, and the pH of the sodium soap and nickel soap in the C272 raffinate is 5.5-6.5.

[0011] As a further improvement of the present invention, in step 4, the chemical composition content of battery-grade nickel sulfate is: Ni: ≥100g / L, Fe: ≤0.002g / L, Cu: ≤0.001g / L, Zn: ≤0.001g / L, Pb: ≤0.001g / L, Ca: ≤0.003g / L, Mg: ≤0.006g / L, Mn: ≤0.004g / L, Na: ≤0.1g / L, Si: ≤0.006g / L, Cl: ≤0.05g / L, F: ≤0.02g / L, oil content ≤3ppm, and pH ≥4.0 at 25°C.

[0012] As a further improvement of the present invention, in step five, the C272 stripping solution is a cobalt sulfate solution containing cobalt ≥ 50 g / L, nickel ≤ 0.5 g / L, and a pH of 1.5-2.5.

[0013] As a further improvement of the present invention, in step 2 and step 5, the iron washing liquid when washing iron with P204 loaded organic phase and C272 loaded organic phase is a ferric sulfate solution containing 3-5 g / L iron and 200-300 g / L acid.

[0014] P204 extraction can be used to separate metal ions such as Ca, Mg, Mn and Zn in the solution, and other impurity metal ions such as Cu, Fe and Co can be preliminarily purified.

[0015] Specifically, the extraction mechanism of phosphonic acid / carboxylic acid extractants is: R-OH+NaOH=R-ONa+H2O 2R-ONa+Ni 2+ =(RO)2Ni+2Na + (RO)2Ni+Me 2+ =(RO)2Me+Ni 2+ Where Me represents a metal ion, including Cu 2+ , Fe 2+ 、Co 2+ 、Zn 2+ , Ca 2+ Mg 2+ , Mn 2+ And other metal ions.

[0016] By using C272 to separate nickel and cobalt from the mixed solution, metal ions such as Cu, Fe, Mg and Zn can be further removed, while achieving the effect of nickel-cobalt separation, thereby obtaining a battery-grade nickel sulfate solution that meets the requirements.

[0017] The present invention adopts the combined extraction process technology of P204 extraction and impurity removal + C272 nickel-cobalt separation, and obtains the following beneficial effects: pH instability during the extraction process will affect the extraction capacity of the extractant, and different extractants will also affect the optimal extraction pH; sodium soap can effectively maintain the pH stability of the method during the extraction process and improve the activity of the extractant, and use sodium hydroxide to react with the organic phase to replace hydrogen ions with sodium ions. If the saponification rate is high, then Na + As the concentration increases, the viscosity of the solution increases, and the two phases separate completely; if the saponification rate is low, it is beneficial to the positive direction of the reaction, releasing H + If the pH value of the equilibrium aqueous phase increases, the pH value of the equilibrium aqueous phase decreases. The role of nickel soap is mainly related to the production of battery-grade nickel sulfate. The nickel ions in the nickel sulfate solution can be replaced by the organic phase after the sodium soap reaction, thereby effectively maintaining the balance of sodium ions in the system. According to the reaction rate, the process technology of synchronous sodium soap and nickel soap is adopted, and the saponification reaction (acid-base reaction) is carried out first. After the sodium soap is completed, the nickel soap reaction is carried out simultaneously, which improves the saponification efficiency, reduces the number of equipment and investment, and shortens the process flow.

[0018] Since the P204 stripping solution contains a high amount of copper, the method effectively replenishes the copper ions in the leaching system by returning the P204 stripping solution to the leaching system for liquid preparation; the method uses nickel sulfate to regenerate iron washing, and the iron washing solution is returned to the leaching system, reducing the consumption of sulfuric acid in the leaching system; the method uses nickel washing solution to wash sodium, reducing the consumption of sulfuric acid in the extraction system. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 Schematic diagram of the process of this method. DETAILED DESCRIPTION

[0020] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0021] Embodiment 1, Step 1: 15% P204 and 85% light white oil are mixed evenly according to a proportion to obtain an organic phase for extraction and impurity removal, and 30% sodium hydroxide and P204 raffinate containing 90 g / L nickel are used to simultaneously treat the organic phase for extraction and impurity removal with sodium soap and nickel soap to obtain an organic phase, and the organic phase is washed with sodium using P204 nickel washing solution, and the organic phase is mixed with a crude nickel sulfate solution after sodium washing, and after mixing, extraction is carried out under the conditions of a reaction temperature of 40°C and a relative O / A ratio of 1.2:1 to obtain a P204 raffinate; the pH of the sodium soap and nickel soap of the P204 raffinate is 3.5, and the P204 nickel washing solution contains 30 g / L nickel and has a pH of 3.0.

[0022] The raw material of crude nickel sulfate solution is high nickel matte. The leaching liquid produced by subjecting the high nickel matte to two stages of normal pressure and two stages of pressurization is crude nickel sulfate solution. The pH value of the crude nickel sulfate solution is 3.5. The chemical composition content of the crude nickel sulfate solution is: Ni: 102g / L, Cu: 0.4 / L, Fe: 0.1g / L, Co: 1.0g / L, Zn: 0.8g / L, Ca: 0.3g / L, Mg: 0.4g / L, Si: 0.06g / L, Mn: 0.04g / L, Pb: 0.01g / L, Na: 0.08g / L, Cl: 0.03g / L, F: 0.01g / L.

[0023] Step 2: The mixed solution in step 1 is extracted to obtain a P204 loaded organic phase, and the P204 loaded organic phase can be repeatedly used as a P204 nickel washing solution for sodium washing after washing. The P204 loaded organic phase is continuously stripped and iron washed after washing, and the stripping solution is leached back to supplement copper during stripping. The iron washing acid can be used as a raw material and mixed with light white oil according to a ratio for repeated use after being leached back; the P204 stripping solution is a solution containing 15 g / L copper, 0.1 g / L nickel, 0.1 g / L cobalt, and a pH of 1.5; the iron washing solution for iron washing with the P204 loaded organic phase is a ferric sulfate solution containing 3 g / L iron and 200 g / L acid.

[0024] Step 3: 10% C272 and 90% light white oil are mixed evenly according to the proportion to obtain a nickel-cobalt separation organic phase, and the organic phase obtained by treating the nickel-cobalt separation organic phase with sodium soap and nickel soap using sodium hydroxide and C272 raffinate is washed with sodium using C272 nickel washing solution, and mixed with the P204 raffinate in step 1 after sodium washing, and extracted at a reaction temperature of 45°C and a relative O / A ratio of 2:1 to obtain a C272 raffinate; the C272 nickel washing solution contains 30g / L nickel and a pH of 3.0, and the pH of the sodium soap and nickel soap of the C272 raffinate is 5.5. The sodium washing solution, sodium soap and nickel soap solution are wastewater, which are sent to a wastewater treatment station for treatment.

[0025] Step 4: Deoil the C272 raffinate in step 3 to obtain a battery-grade nickel sulfate solution; the chemical composition content of battery-grade nickel sulfate is: Ni: 100g / L, Fe: 0.002g / L, Cu: 0.001g / L, Zn: 0.001g / L, Pb: 0.001g / L, Ca: 0.003g / L, Mg: 0.006g / L, Mn: 0.004g / L, Na: 0.1g / L, Si: 0.006g / L, Cl: 0.05g / L, F: 0.02g / L, the oil content is 3ppm, and the pH at 25°C is 4.0.

[0026] Step 5: The mixed solution in step 3 is extracted to obtain a C272 loaded organic phase, and the C272 loaded organic phase can be repeatedly used as a C272 nickel washing solution for sodium washing after washing. The C272 loaded organic phase is further stripped and iron washed after washing. During stripping, the C272 stripping solution is exported as a cobalt sulfate solution, and the iron washing acid can be reused as a raw material by mixing with light white oil according to a ratio after back leaching; the C272 stripping solution is a cobalt sulfate solution containing 50 g / L cobalt, 0.5 g / L nickel, and a pH of 1.5; the iron washing solution for iron washing with the C272 loaded organic phase is a ferric sulfate solution containing 3 g / L iron and 200 g / L acid.

[0027] Embodiment 2, Step 1: 15% P204 and 85% light white oil are mixed evenly according to a proportion to obtain an organic phase for extraction and impurity removal, and 31% sodium hydroxide and P204 raffinate containing 100 g / L nickel are used to simultaneously treat the organic phase for extraction and impurity removal with sodium soap and nickel soap to obtain an organic phase, and the organic phase is washed with sodium using P204 nickel washing solution, and the organic phase is mixed with a crude nickel sulfate solution after sodium washing, and after mixing, extraction is carried out under the conditions of a reaction temperature of 42°C and a relative O / A ratio of 1.4:1 to obtain a P204 raffinate; the pH of the sodium soap and nickel soap of the P204 raffinate is 4.0, and the nickel content of the P204 nickel washing solution is 45 g / L, and the pH is 3.5.

[0028] The raw material of crude nickel sulfate solution is high nickel matte. The leaching liquid produced by subjecting the high nickel matte to two stages of normal pressure and two stages of pressurization is crude nickel sulfate solution. The pH value of crude nickel sulfate solution is 3.7. The chemical composition content of crude nickel sulfate solution is: Ni: 103g / L, Cu: 0.5 / L, Fe: 0.2g / L, Co: 1.3g / L, Zn: 1.0 / L, Ca: 0.4g / L, Mg: 0.5g / L, Si: 0.08g / L, Mn: 0.06g / L, Pb: 0.02g / L, Na: 0.12g / L, Cl: 0.05g / L, F: 0.02g / L.

[0029] Step 2: The mixed solution in step 1 is extracted to obtain a P204 loaded organic phase, and the P204 loaded organic phase can be repeatedly used as a P204 nickel washing solution for sodium washing after washing. The P204 loaded organic phase is continuously stripped and iron washed after washing, and the stripping solution is leached back to supplement copper during stripping. The iron washing acid can be used as a raw material and mixed with light white oil according to a ratio for repeated use after leaching back; the P204 stripping solution is a solution containing 24 g / L copper, 0.09 g / L nickel, 0.09 g / L cobalt, and a pH of 2.0; the iron washing solution for iron washing with the P204 loaded organic phase is a ferric sulfate solution containing 4 g / L iron and 250 g / L acid.

[0030] Step 3: 10% C272 and 90% light white oil are mixed evenly according to the proportion to obtain a nickel-cobalt separation organic phase, and the organic phase obtained by treating the nickel-cobalt separation organic phase with sodium soap and nickel soap using sodium hydroxide and C272 raffinate is washed with sodium using C272 nickel washing solution, and mixed with the P204 raffinate in step 1 after sodium washing, and extracted at a reaction temperature of 47°C and a relative O / A ratio of 2.2:1 to obtain a C272 raffinate; the C272 nickel washing solution contains 45g / L nickel and a pH of 3.5, and the pH of the sodium soap and nickel soap of the C272 raffinate is 6.0. The sodium washing solution, sodium soap and nickel soap solution are wastewater, which are sent to a wastewater treatment station for treatment.

[0031] Step 4: Deoil the C272 raffinate in step 3 to obtain a battery-grade nickel sulfate solution; the chemical composition of the battery-grade nickel sulfate is: Ni: 105g / L, Fe: 0.002g / L, Cu: 0.001g / L, Zn: 0.001g / L, Pb: 0.001g / L, Ca: 0.003g / L, Mg: 0.006g / L, Mn: 0.004g / L, Na: 0.09g / L, Si: 0.005g / L, Cl: 0.04g / L, F: 0.02g / L, the oil content is 2.5ppm, and the pH at 25°C is 5.0.

[0032] Step 5: The mixed solution in step 3 is extracted to obtain a C272 loaded organic phase, and the C272 loaded organic phase can be repeatedly used as a C272 nickel washing solution for sodium washing after washing. The C272 loaded organic phase is further stripped and iron washed after washing. During stripping, the C272 stripping solution is exported as a cobalt sulfate solution, and the iron washing acid can be used as a raw material and mixed with light white oil according to a ratio for repeated use after back leaching; the C272 stripping solution is a cobalt sulfate solution containing 55 g / L cobalt, 0.4 g / L nickel, and a pH of 2.0; the iron washing solution for iron washing with the C272 loaded organic phase is a ferric sulfate solution containing 4 g / L iron and 250 g / L acid.

[0033] Embodiment 3, Step 1: 15% P204 and 85% light white oil are mixed evenly according to a proportion to obtain an organic phase for extraction and impurity removal, and 32% sodium hydroxide and P204 raffinate containing 110 g / L nickel are used to simultaneously treat the organic phase for extraction and impurity removal with sodium soap and nickel soap to obtain an organic phase, and the organic phase is washed with sodium using P204 nickel washing solution, and the organic phase is mixed with a crude nickel sulfate solution after sodium washing, and after mixing, the reaction temperature is 45°C and the ratio O / A is 1.5:1 to obtain a P204 raffinate; the pH of the sodium soap and nickel soap of the P204 raffinate is 4.5, and the nickel content of the P204 nickel washing solution is 60 g / L, and the pH is 4.0.

[0034] The raw material of crude nickel sulfate solution is high nickel matte. The leaching liquid produced by subjecting the high nickel matte to two stages of normal pressure and two stages of pressurization is crude nickel sulfate solution. The pH value of the crude nickel sulfate solution is 4.0. The chemical composition content of the crude nickel sulfate solution is: Ni: 106g / L, Cu: 0.6 / L, Fe: 0.4g / L, Co: 1.5g / L, Zn: 1.2g / L, Ca: 0.6g / L, Mg: 0.7g / L, Si: 0.1g / L, Mn: 0.08g / L, Pb: 0.04g / L, Na: 0.15g / L, Cl: 0.06g / L, F: 0.04g / L.

[0035] Step 2: The mixed solution in step 1 is extracted to obtain a P204 loaded organic phase, and the P204 loaded organic phase can be repeatedly used as a P204 nickel washing solution for sodium washing after washing. The P204 loaded organic phase is continuously stripped and iron washed after washing, and the stripping solution is leached back to supplement copper during stripping. The iron washing acid can be used as a raw material and mixed with light white oil according to a ratio for repeated use after leaching back; the P204 stripping solution is a solution containing 30 g / L copper, 0.08 g / L nickel, 0.08 g / L cobalt, and a pH of 2.5; the iron washing solution for iron washing with the P204 loaded organic phase is a ferric sulfate solution containing 5 g / L iron and 300 g / L acid.

[0036] Step 3: 10% C272 and 90% light white oil are mixed evenly according to the proportion to obtain a nickel-cobalt separation organic phase, and the organic phase obtained by treating the nickel-cobalt separation organic phase with sodium soap and nickel soap using sodium hydroxide and C272 raffinate is washed with sodium using C272 nickel washing solution, and mixed with the P204 raffinate in step 1 after sodium washing, and extracted at a reaction temperature of 50°C and a relative O / A ratio of 2.5:1 to obtain a C272 raffinate; the C272 nickel washing solution contains 60g / L nickel and a pH of 4.0, and the pH of the sodium soap and nickel soap of the C272 raffinate is 6.5. The sodium washing solution, sodium soap and nickel soap solution are wastewater, which are sent to a wastewater treatment station for treatment.

[0037] Step 4: Deoil the C272 raffinate in step 3 to obtain a battery-grade nickel sulfate solution; the chemical composition of the battery-grade nickel sulfate is: Ni: 110g / L, Fe: 0.001g / L, Cu: 0.0009g / L, Zn: 0.001g / L, Pb: 0.001g / L, Ca: 0.002g / L, Mg: 0.004g / L, Mn: 0.002g / L, Na: 0.08g / L, Si: 0.004g / L, Cl: 0.04g / L, F: 0.01 / L, the oil content is 1.5ppm, and the pH at 25°C is 5.5.

[0038] Step 5: The mixed solution in step 3 is extracted to obtain a C272 loaded organic phase, and the C272 loaded organic phase can be repeatedly used as a C272 nickel washing solution for sodium washing after washing. The C272 loaded organic phase is further stripped and iron washed after washing. During stripping, the C272 stripping solution is exported as a cobalt sulfate solution, and the iron washing acid can be reused as a raw material by mixing with light white oil according to a ratio after back leaching; the C272 stripping solution is a cobalt sulfate solution containing 60 g / L cobalt, 0.3 g / L nickel, and a pH of 2.5; the iron washing solution for iron washing with the C272 loaded organic phase is a ferric sulfate solution containing 5 g / L iron and 300 g / L acid.

[0039] The chemical composition of the battery-grade nickel sulfate solution extracted and separated by this production process meets the requirements of industry standards. This production process as a whole prepares crude nickel sulfate solution from high nickel matte to finally extract battery-grade nickel sulfate solution. The process mainly includes two steps: leaching and purification. Purification is extraction. The extraction process is a joint extraction of P204+C272, which mainly includes the simultaneous extraction of sodium soap and nickel soap, sodium washing, extraction, nickel washing (nickel washing solution is returned to the sodium washing section to reduce acid consumption), stripping (stripping solution is mainly impurities such as Ca, Cu, Zn, etc., which are returned to the leaching system for copper supplement), regeneration and iron washing (mainly iron and sulfuric acid, which are returned to the leaching system for acid supplement to reduce acid consumption). The internal circulation method is used to achieve the reuse of nickel washing solution and part of the raffinate, shortening the extraction process, increasing the repeated reuse of resources such as nickel washing solution, reducing equipment investment, and reducing production and operation costs.

Claims

1. A method for efficiently extracting battery-grade nickel sulfate solution, characterized in that: The following steps are involved: Step 1: P204 and light white oil are mixed evenly to obtain an organic phase for extraction and impurity removal, and the organic phase for extraction and impurity removal is treated with sodium soap and nickel soap by sodium hydroxide and P204 raffinate to obtain an organic phase, and the organic phase is washed with sodium by P204 nickel washing solution, and the organic phase is mixed with a crude nickel sulfate solution after sodium washing, and the mixed phase is extracted to obtain a P204 raffinate; Step 2: The mixed solution in step 1 is extracted to obtain a P204-loaded organic phase, which can be repeatedly used as a P204 nickel-washing solution for sodium washing after washing, and the P204-loaded organic phase is continuously stripped and iron-washed after washing, and the stripping solution is back-leached to supplement copper during stripping, and the iron-washing acid can be reused as a raw material after being mixed with light white oil after being back-leached; Step 3: C272 and light white oil are mixed evenly to obtain a nickel-cobalt separation organic phase, and the nickel-cobalt separation organic phase is treated with sodium soap and nickel soap using sodium hydroxide and C272 raffinate to obtain an organic phase, and the organic phase is washed with sodium using C272 nickel washing solution, and the organic phase is mixed with the P204 raffinate in step 1 after sodium washing, and the mixed phase is extracted to obtain C272 raffinate; Step 4: removing oil from the C272 raffinate in step 3 to obtain a battery-grade nickel sulfate solution; Step 5: The mixed solution in step 3 is extracted to obtain a C272 loaded organic phase, which can be washed and reused as a C272 nickel washing solution for sodium washing. The C272 loaded organic phase is washed and further stripped and iron washed. During stripping, the C272 stripping solution is exported as a cobalt sulfate solution, and the iron washing acid can be used as a raw material and mixed with light white oil in a proportion for repeated use.

2. The method for efficiently extracting a battery-grade nickel sulfate solution according to claim 1, characterized in that: In step 1, the raw material of the crude nickel sulfate solution is high nickel matte, and the high nickel matte is subjected to two stages of normal pressure and two stages of pressurization to produce a leaching solution as a crude nickel sulfate solution. The pH value of the crude nickel sulfate solution is 3.5-4.0, and the chemical composition content of the crude nickel sulfate solution is: Ni: 102-106 g / L, Cu: 0.4-0.6 / L, Fe: 0.1-0.4 g / L, Co: 1.0-1.5 g / L , Zn: 0.8-1.2g / L, Ca: 0.3-0.6g / L, Mg: 0.4-0.7g / L, Si: 0.06-0.1g / L, Mn: 0.04-0. 08g / L, Pb: 0.01-0.04g / L, Na: 0.08-0.15g / L, Cl: 0.03-0.06g / L, F: 0.01-0.04g / L.

3. The method for efficiently extracting a battery-grade nickel sulfate solution according to claim 1, characterized in that: In step 1, sodium soap and nickel soap are treated simultaneously using 30-32% sodium hydroxide and P204 raffinate containing 90-110 g / L nickel. The pH of sodium soap and nickel soap in P204 raffinate is 3.5-4.5, and the P204 nickel washing solution contains 30-60 g / L nickel and has a pH of 3.0-4.

0.

4. The method for efficiently extracting a battery-grade nickel sulfate solution according to claim 1, characterized in that: In step 1, the mixed solution is extracted at a reaction temperature of 40°C-45°C and a ratio of O / A=1.2-1.5:

1.

5. The method for efficiently extracting a battery-grade nickel sulfate solution according to claim 1, characterized in that: In step 2, the P204 stripping solution is a solution containing 15-30 g / L copper, ≤0.1 g / L nickel, ≤0.1 g / L cobalt, and a pH of 1.5-2.

5.

6. The method for efficiently extracting a battery-grade nickel sulfate solution according to claim 1, characterized in that: In step three, the mixed solution is extracted at a reaction temperature of 45°C-50°C and a relative O / A ratio of 2-2.5:1; the C272 nickel washing solution contains 30-60 g / L nickel and a pH of 3.0-4.0, and the pH of the sodium soap and nickel soap in the C272 raffinate is 5.5-6.

5.

7. The method for efficiently extracting a battery-grade nickel sulfate solution according to claim 1, characterized in that: In step 4, the chemical composition content of battery-grade nickel sulfate is: Ni: ≥100g / L, Fe: ≤0.002g / L, Cu: ≤0.001g / L, Zn: ≤0.001g / L, Pb: ≤0.001g / L, Ca: ≤0.003g / L, Mg: ≤0.006g / L, Mn: ≤0.004g / L, Na: ≤0.1g / L, Si: ≤0.006g / L, Cl: ≤0.05g / L, F: ≤0.02g / L, oil content ≤3ppm, pH ≥4.0 at 25°C.

8. The method for efficiently extracting a battery-grade nickel sulfate solution according to claim 1, characterized in that: In step 5, the C272 stripping solution is a cobalt sulfate solution containing ≥50 g / L of cobalt, ≤0.5 g / L of nickel, and a pH of 1.5-2.

5.

9. The method for efficiently extracting a battery-grade nickel sulfate solution according to claim 1, characterized in that: In step 2 and step 5, the iron washing solution when P204 loads the organic phase and C272 loads the organic phase for iron washing is a ferric sulfate solution containing 3-5 g / L iron and 200-300 g / L acid.