Corrosion-resistant copper-based nickel-aluminum alloy and preparation method thereof

CN118726792AInactive Publication Date: 2024-10-01NINGBO SHENGRONGFA NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410966727.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing copper-nickel alloys are easily affected by rain corrosion in outdoor environments, resulting in a decrease in corrosion resistance. In particular, the composite oxide layers of Al2O3, Ni0 and Cu2O are fragile and difficult to isolate corrosive media for a long time.

Method used

The spider web-like micro-nano La2O3 rough structure and nano-porous composite film layer combination technology are used to form a hydrophobic layer. Through the addition of Cr and Zr elements, the stability and strength of the oxide layer are enhanced, and the corrosion resistance of the copper-based nickel-aluminum alloy is improved.

Benefits of technology

Significantly improves the corrosion resistance and wear resistance of copper-based nickel-aluminum alloys, prolongs the stability of the oxide layer, reduces the possibility of corrosion media adhering and breaking, and enhances its corrosion resistance in long-term use.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of functional alloy materials, in particular to a corrosion-resistant copper-based nickel-aluminum alloy and a preparation method thereof. The corrosion-resistant copper-based nickel-aluminum alloy comprises the following raw materials in percentage by mass: 20-26% of Ni, 6-8% of Al, 3-5% of La, 2-4% of trace elements and the balance of Cu, the corrosion-resistant copper-based nickel aluminum alloy is a nano-porous film layer copper-based nickel aluminum alloy with a cobweb-shaped micro-nano La2O3 coarse structure attached to the surface. The corrosion-resistant copper-based nickel-aluminum alloy disclosed by the invention has more excellent corrosion resistance and wear resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of functional alloy materials, and more specifically, to a corrosion-resistant copper-based nickel-aluminum alloy and a preparation method thereof. Background Art

[0002] Metal materials are indispensable in modern engineering construction. However, since most metal materials are exposed to the outdoors, they can easily cause a lot of economic losses and waste of resources due to insufficient mechanical properties and corrosion resistance. Therefore, it is particularly important to prepare more corrosion-resistant metal materials.

[0003] Copper and copper alloys have excellent corrosion resistance and mechanical properties, especially copper-nickel alloys, which also have excellent electrical and thermal conductivity and ductility, and are therefore used in more engineering fields. However, with the progress of the times and the development of industry, the acid content in rainwater has increased significantly. Therefore, there is an urgent need for a copper-based alloy material with better corrosion resistance. Summary of the invention

[0004] In order to improve the defects of conventional copper-nickel alloys which still have insufficient corrosion resistance, the present application provides a corrosion-resistant copper-based nickel-aluminum alloy and a preparation method thereof.

[0005] In the first aspect, the present application provides a corrosion-resistant copper-based nickel-aluminum alloy and a preparation method thereof, using the following technical solution: A corrosion-resistant copper-based nickel-aluminum alloy comprises the following raw materials in percentage by mass: 20-26% Ni, 6-8% Al, 3-5% La and 0-4% trace elements, with the balance being Cu.

[0006] Preferably, the La is attached to the surface of the copper-based nickel-aluminum alloy in the form of a spider-web-like micro-nano La2O3 rough structure.

[0007] When Al is added to the copper-nickel alloy, a composite oxide layer of Al2O3, Ni0 and Cu2O will gradually form on the surface of the copper-based nickel-aluminum alloy in the early stage of corrosion. The composite oxide layer containing Al2O3 is more stable, thus obtaining better corrosion resistance. However, at the same time, the composite oxide layer of Al2O3, Ni0 and Cu2O is relatively fragile and cannot completely isolate the internal metal from the corrosive medium. The corrosion in the outdoor environment is long-term and uninterrupted. Therefore, after the composite oxide layer of Al2O3, Ni0 and Cu2O is broken, the corrosion resistance of the copper-based nickel-aluminum alloy will also decrease significantly.

[0008] At present, the corrosion in the outdoor environment is generally rainwater corrosion. When rainwater adheres to the surface of copper-based nickel-aluminum alloy for a long time, the composite oxide layer of Al2O3, Ni0 and Cu2O is easily broken. However, when La is attached to the surface of copper-based nickel-aluminum alloy in the form of a spider web-like micro-nano La2O3 rough structure, the spider web-like micro-nano La2O3 rough structure will form a bionic hydrophobic layer, and the super-hydrophobic properties of La2O3 itself will work together to make the corrosion-resistant copper-based nickel-aluminum alloy have an extremely good hydrophobic effect on rainwater, making it difficult for corrosive media to adhere to the surface of the corrosion-resistant copper-based nickel-aluminum alloy, thereby reducing the possibility of Al2O3, Ni0 and Cu2O composite oxide layer breaking, thereby improving the corrosion resistance of the corrosion-resistant copper-based nickel-aluminum alloy.

[0009] Preferably, a nanoporous composite membrane layer is formed on the surface of the copper-based nickel-aluminum alloy, and the spider-web-like micro-nano La2O3 rough structure is inserted into the pores of the nanoporous composite membrane layer.

[0010] Although the spiderweb-like micro-nano La2O3 rough structure can improve the corrosion resistance of copper-based nickel-aluminum alloy by increasing its surface hydrophobicity, the connection effect between the spiderweb-like micro-nano La2O3 rough structure and the Al2O3, Ni0 and Cu2O composite oxide layer needs to be strengthened. After the corrosion-resistant copper-based nickel-aluminum alloy is used for a long time, the spiderweb-like micro-nano La2O3 rough structure is easily fallen off, resulting in the deterioration of its hydrophobicity.

[0011] After the nanoporous composite film layer is formed on the surface of the copper-based nickel-aluminum alloy, the spider-web-like micro-nano La2O3 rough structure can be inserted into the pores of the nanoporous composite film layer, thereby playing a multi-point supporting and connecting role, effectively reducing the possibility of the spider-web-like micro-nano La2O3 rough structure falling off, and indirectly improving the corrosion resistance of the copper-based nickel-aluminum alloy.

[0012] Preferably, the trace elements include Cr.

[0013] After the nanoporous composite film layer is formed, the stability of the Al2O3, Ni0 and Cu2O composite oxide layers will be reduced to a certain extent. When the Cr element is added, Cr will form a Cr2O3 inner oxide film during the sintering process, and then with the synergistic cooperation of the Al2O3, Ni0 and Cu2O composite oxide layers, better corrosion resistance will be obtained.

[0014] Preferably, the trace elements also include Zr.

[0015] After the formation of the nanoporous composite film layer, the stability of the Al2O3, Ni0 and Cu2O composite oxide layers will be reduced to a certain extent. When the Zr element is added, the Zr element can slightly improve the strength of the Al2O3, Ni0 and Cu2O composite oxide layers as a whole, while improving the connection effect between the spider-web-like micro-nano La2O3 rough structure and the Al2O3, Ni0 and Cu2O composite oxide layers, and can also improve the corrosion resistance of the copper-based nickel-aluminum alloy.

[0016] Preferably, the corrosion-resistant copper-based nickel-aluminum alloy comprises the following raw materials in percentage by mass: Ni 20-26%, Al 6-8%, La 3-5%, Cr 1-3% and Zr 1-2%, with the remainder being Cu.

[0017] When the elements of the corrosion-resistant copper-based nickel-aluminum alloy adopt the above-mentioned mass percentages, the prepared copper-based nickel-aluminum alloy will have better corrosion resistance and wear resistance.

[0018] In a second aspect, the present application provides a method for preparing a corrosion-resistant copper-based nickel-aluminum alloy, using the following technical solution: A method for preparing a corrosion-resistant copper-based nickel-aluminum alloy comprises the following steps: Step 1: First, Cu, Ni, Al and trace elements are mixed in proportion, then melted, homogenized and annealed, and finally immersed in a 3.5% sodium chloride aqueous solution for 3-5 hours for pre-corrosion to prepare a copper-based nickel-aluminum alloy, with a melting temperature of 1300-1400°C, insulation for 10-15 minutes, and a casting temperature of 1250-1300°C; the homogenization annealing temperature is 900-1000°C, insulation for 1-3 hours, and cooling with the furnace; Step 2: Clean the copper-based nickel-aluminum alloy with acetone, anhydrous ethanol and deionized water, and then dry it for use; then prepare lanthanum nitrate electrodeposition solution according to the proportion of La, adjust the voltage to 3V, short-circuit the positive and negative poles of the power supply, adjust the current to 2mA, connect the graphite electrode to the positive pole of the power supply, connect the copper-based nickel-aluminum alloy to the negative pole of the power supply, and electrodeposit for 10 minutes at a water bath temperature of 25°C. Finally, dry the product under a pressure of -0.1Mpa and a temperature of 185°C for 3 hours to obtain a corrosion-resistant copper-based nickel-aluminum alloy; The corrosion-resistant copper-based nickel-aluminum alloy is a copper-based nickel-aluminum alloy with a spider-web-like micro-nano La2O3 rough structure attached to the surface.

[0019] A method for preparing a corrosion-resistant copper-based nickel-aluminum alloy comprises the following steps: Step 1: First, Cu, Ni, Al and trace elements are mixed in proportion, and then melt-cast and homogenize anneal to prepare a copper-based nickel-aluminum alloy, with a melting temperature of 1300-1400°C, insulation for 10-15 minutes, and a casting temperature of 1250-1300°C; the homogenization annealing temperature is 900-1000°C, insulation for 1-3 hours, and cooling with the furnace; Step 2: Clean the copper-based nickel-aluminum alloy with acetone, anhydrous ethanol and deionized water, and then dry it for standby use; then prepare an oxalic acid solution with a concentration of 5wt%, adjust the voltage to 50V, short-circuit the positive and negative electrodes of the power supply, connect the copper-based nickel-aluminum alloy to the positive electrode of the power supply, connect the graphite electrode to the negative electrode of the power supply, treat it at a water bath temperature of 0°C for 40 minutes, and finally dry it to obtain a nanoporous film layer copper-based nickel-aluminum alloy; Step 3, the nanoporous film layer copper-based nickel-aluminum alloy is cleaned with acetone, anhydrous ethanol and deionized water, and then dried for use; then, a lanthanum nitrate electrodeposition solution is prepared according to the proportion of La, the voltage is adjusted to 3V, the positive and negative electrodes of the power supply are short-circuited, the current is adjusted to 2mA, the graphite electrode is connected to the positive electrode of the power supply, and the nanoporous film layer copper-based nickel-aluminum alloy is connected to the negative electrode of the power supply, and the electrodeposition is carried out at a water bath temperature of 25°C for 10min, and finally the product is placed in an environment of pressure -0.1Mpa and temperature 185°C and dried for 3h to obtain a corrosion-resistant copper-based nickel-aluminum alloy; The corrosion-resistant copper-based nickel-aluminum alloy is a copper-based nickel-aluminum alloy with a nanoporous film layer having a spider-web-like micro-nano La2O3 rough structure attached to the surface.

[0020] In summary, this application has the following beneficial effects: 1. The corrosion in the outdoor environment is generally rain corrosion. When rainwater adheres to the surface of the copper-based nickel-aluminum alloy for a long time, the composite oxide layer of Al2O3, Ni0 and Cu2O is easily broken. However, when La is attached to the surface of the copper-based nickel-aluminum alloy in the form of a spider-web-like micro-nano La2O3 rough structure, the spider-web-like micro-nano La2O3 rough structure will form a bionic hydrophobic layer. In addition, the super-hydrophobic properties of La2O3 itself work together to make the corrosion-resistant copper-based nickel-aluminum alloy have an extremely good hydrophobic effect on rainwater, making it difficult for corrosive media to adhere to the surface of the corrosion-resistant copper-based nickel-aluminum alloy, thereby reducing the possibility of Al2O3, Ni0 and Cu2O composite oxide layer breaking, thereby improving the corrosion resistance of the corrosion-resistant copper-based nickel-aluminum alloy.

[0021] 2. Although the spider-web-like micro-nano La2O3 rough structure can improve the corrosion resistance of copper-based nickel-aluminum alloy by improving its surface hydrophobicity, the connection effect between the spider-web-like micro-nano La2O3 rough structure and the Al2O3, Ni0 and Cu2O composite oxide layer needs to be strengthened. After the corrosion-resistant copper-based nickel-aluminum alloy is used for a long time, the spider-web-like micro-nano La2O3 rough structure is easy to fall off, resulting in the deterioration of its hydrophobicity; After the nanoporous composite film layer is formed on the surface of the copper-based nickel-aluminum alloy, the spider-web-like micro-nano La2O3 rough structure can be inserted into the pores of the nanoporous composite film layer, thereby playing a multi-point supporting and connecting role, effectively reducing the possibility of the spider-web-like micro-nano La2O3 rough structure falling off, and indirectly improving the corrosion resistance of the copper-based nickel-aluminum alloy.

[0022] 3. After the nanoporous composite film is formed, the stability of the composite oxide layers of Al2O3, Ni0 and Cu2O will be reduced to a certain extent. When the Cr element is added, Cr will form a Cr2O3 inner oxide film during the sintering process, and then with the synergistic cooperation of the composite oxide layers of Al2O3, Ni0 and Cu2O, better corrosion resistance will be obtained. When the Zr element is added, the Zr element can slightly improve the strength of the Al2O3, Ni0 and Cu2O composite oxide layer as a whole. While improving the connection effect between the spider-web-like micro-nano La2O3 rough structure and the Al2O3, Ni0 and Cu2O composite oxide layer, it can also improve the corrosion resistance of the copper-based nickel-aluminum alloy. DETAILED DESCRIPTION

[0023] The present application is further described in detail below in conjunction with Examples 1-6 and Comparative Examples 1-2.

[0024] raw material Cu, Ni, Al, Cr and Zr are all commercially available; acetone CAS: 67-64-1; anhydrous ethanol CAS: 64-17-5; oxalic acid CAS: 6153-56-6; lanthanum nitrate CAS: 100587-94-8.

[0025] Example Example 1 A corrosion-resistant copper-based nickel-aluminum alloy comprises the following raw materials in percentage by mass: 23% Ni, 7% Al, 4% La, and the balance is Cu.

[0026] The preparation method of the corrosion-resistant copper-based nickel-aluminum alloy comprises the following steps: Step 1: First, Cu, Ni, and Al are mixed in proportion, then melt-cast, homogenized, and finally immersed in a 3.5% sodium chloride aqueous solution for 4 hours for pre-corrosion to prepare a copper-based nickel-aluminum alloy, with a melting temperature of 1320°C, a heat preservation of 15 minutes, a casting temperature of 1250°C, a homogenized annealing temperature of 950°C, a heat preservation of 3 hours, and cooling with the furnace; Step 2: Cut the copper-based nickel-aluminum alloy into a rectangular electrode of 1.0 cm × 5.0 cm, then wash it with acetone, anhydrous ethanol and deionized water, the volume ratio of acetone, anhydrous ethanol and deionized water is 2:2:6, and then dry it for use; then prepare 200 ml of lanthanum nitrate electrodeposition solution according to the proportion of La, adjust the voltage to 3 V, short-circuit the positive and negative poles of the power supply, adjust the current to 2 mA, connect the graphite electrode to the positive pole of the power supply, connect the copper-based nickel-aluminum alloy to the negative pole of the power supply, and electro-deposit it at a water bath temperature of 25 ° C for 10 minutes, and finally place the product in an environment of pressure -0.1 MPa and temperature 185 ° C for 3 hours to obtain a corrosion-resistant copper-based nickel-aluminum alloy; Among them, the corrosion-resistant copper-based nickel-aluminum alloy is a copper-based nickel-aluminum alloy with a spider-web-like micro-nano La2O3 rough structure attached to the surface.

[0027] Example 2 A corrosion-resistant copper-based nickel-aluminum alloy comprises the following raw materials in percentage by mass: 23% Ni, 7% Al, 4% La, and the balance is Cu.

[0028] The preparation method of the corrosion-resistant copper-based nickel-aluminum alloy comprises the following steps: Step 1: First, Cu, Ni, and Al are mixed in proportion, and then melt-cast and homogenized annealed to prepare a copper-based nickel-aluminum alloy, with a melting temperature of 1320°C, a heat preservation of 15 minutes, and a casting temperature of 1250°C; a homogenization annealing temperature of 950°C, a heat preservation of 3 hours, and cooling with the furnace; Step 2: Cut the copper-based nickel-aluminum alloy into a rectangular electrode of 1.0 cm × 5.0 cm, then wash it with acetone, anhydrous ethanol and deionized water, the volume ratio of acetone, anhydrous ethanol and deionized water is 2:2:6, and then dry it for use; then prepare 200 ml of 5wt% oxalic acid solution, adjust the voltage to 50V, short-circuit the positive and negative poles of the power supply, connect the copper-based nickel-aluminum alloy to the positive pole of the power supply, connect the graphite electrode to the negative pole of the power supply, treat it at a water bath temperature of 0°C for 40 minutes, and finally dry it to obtain a nanoporous film layer copper-based nickel-aluminum alloy; Step 3, the nanoporous film layer copper-based nickel-aluminum alloy is cleaned by acetone, anhydrous ethanol and deionized water, the volume ratio of acetone, anhydrous ethanol and deionized water is 2:2:6, and then dried for use; then 200 ml of lanthanum nitrate electrodeposition solution is prepared according to the proportion of La, the voltage is adjusted to 3V, the positive and negative poles of the power supply are short-circuited, the current is adjusted to 2 mA, the graphite electrode is connected to the positive pole of the power supply, and the copper-based nickel-aluminum alloy is connected to the negative pole of the power supply, and the electrodeposition is carried out at a water bath temperature of 25°C for 10 minutes, and finally the product is placed in an environment of pressure -0.1Mpa and temperature 185°C and dried for 3 hours to obtain a corrosion-resistant copper-based nickel-aluminum alloy; The corrosion-resistant copper-based nickel-aluminum alloy is a copper-based nickel-aluminum alloy with a nanoporous film layer having a spider-web-like micro-nano La2O3 rough structure attached to the surface.

[0029] Example 3 The difference from Example 2 is that the corrosion-resistant copper-based nickel-aluminum alloy also includes trace element Cr; Specifically, the corrosion-resistant copper-based nickel-aluminum alloy includes the following raw materials in percentage by mass: Ni 23%, Al 7%, La 4%, Cr 2%, and the balance is Cu.

[0030] Example 4 The difference from Example 3 is that the corrosion-resistant copper-based nickel-aluminum alloy further includes a trace element Zr; Specifically, the corrosion-resistant copper-based nickel-aluminum alloy includes the following raw materials in percentage by mass: Ni 23%, Al 7%, La 4%, Cr 2%, Zr 1.5%, and the balance is Cu.

[0031] Embodiment 5-6 The difference from Example 4 is that the percentages of the components of the corrosion-resistant copper-based nickel-aluminum alloy are different, as shown in Table 1.

[0032] Table 1 Percentage of each component of the corrosion-resistant copper-based nickel-aluminum alloy of Examples 4-6 Example 4 Example 5 Example 6 Ni 23 20 26 Al 7 8 6 La 4 4 5 Cr 2 2 1 Zr 1.5 1 2 Cu margin margin margin Comparative Example Comparative Example 1 A copper-nickel alloy comprises the following raw materials in percentage by mass: 23% Ni and 77% Cu.

[0033] The preparation method of copper-nickel alloy is: First, Cu and Ni are mixed in proportion, then melt-cast, homogenized annealed, and finally immersed in 3.5% sodium chloride aqueous solution for 4 hours for pre-corrosion to prepare copper-nickel alloy. The melting temperature is 1320℃, the temperature is kept for 15 minutes, and the casting temperature is 1250℃; the homogenized annealing temperature is 950℃, the temperature is kept for 3 hours, and the alloy is cooled with the furnace.

[0034] Comparative Example 2 A copper-based nickel-aluminum alloy comprises the following raw materials in percentage by mass: 23% Ni, 7% Al and 70% Cu.

[0035] The preparation method of copper-based nickel-aluminum alloy is: First, Cu, Al and Ni are mixed in proportion, then melt-cast, homogenized annealed, and finally immersed in 3.5% sodium chloride aqueous solution for 4 hours for pre-corrosion to prepare copper-nickel alloy. The melting temperature is 1320℃, the temperature is kept for 15 minutes, and the casting temperature is 1250℃; the homogenized annealing temperature is 950℃, the temperature is kept for 3 hours, and the alloy is cooled with the furnace.

[0036] Performance testing Detection Methods 1. Corrosion resistance test Three samples were taken out from Examples 1-6 and Comparative Examples 1-2, respectively, and the masses of all samples were weighed and recorded as M0; all samples were then placed vertically, and 10 ml of acid rain simulation liquid was sprayed on the surface of the samples every three days. The pH value of the acid rain simulation liquid was 5, and the ratio of sulfuric acid to nitric acid was 1:1 by mixing sulfuric acid and nitric acid; the experiment lasted for 150 days, and finally the samples were washed and dried with deionized water, and the test mass was weighed and recorded as M1. Finally, the mass loss value was calculated, mass loss value = M0-M1, and the average value was taken.

[0037] 2. Wear resistance test Three samples were taken from Examples 1-6 and Comparative Examples 1-2, and then the sample surfaces were rubbed with 600-mesh sandpaper at a speed of 30 r / min for 10 min, and then the sample mass was weighed and recorded as m0; then all the samples were placed vertically, and 10 ml of acid rain simulation liquid was sprayed on the sample surface every three days, the acid rain simulation liquid pH value = 5, and sulfuric acid and nitric acid were prepared with a ratio of sulfuric acid to nitric acid of 1:1; the experiment lasted for 150 days, and finally washed and dried with deionized water, and the wear test mass was weighed and recorded as m1, and finally the mass loss value after wear was calculated, the mass loss value after wear = m0-m1, and the average value was taken; Finally, the change is calculated, change = mass loss value after wear - mass loss value.

[0038] The test data are shown in Table 2.

[0039] Table 2 Test data table of Examples 1-6 and Comparative Examples 1-2 Mass loss value / mg Change / mg Example 1 0.341 0.579 Example 2 0.349 0.211 Example 3 0.301 0.205 Example 4 0.273 0.180 Example 5 0.278 0.183 Example 6 0.281 0.185 Comparative Example 1 3.112 0.003 Comparative Example 2 1.097 0.778 Referring to Comparative Examples 1-2 and in combination with Table 2, it can be seen that, relative to Comparative Example 1, the mass loss value of Comparative Example 2 is significantly reduced, and the amount of change is also significantly increased, which indicates that the addition of Al can effectively improve the corrosion resistance of the copper-nickel alloy, while wear will cause its corrosion resistance to decrease significantly.

[0040] The reason is that when Al is added to the copper-nickel alloy, a composite oxide layer of Al2O3, Ni0 and Cu2O will gradually form on the surface of the copper-based nickel-aluminum alloy in the early stage of corrosion. The composite oxide layer containing Al2O3 is more stable, thus obtaining better corrosion resistance. However, at the same time, the composite oxide layer of Al2O3, Ni0 and Cu2O is relatively fragile, and the wear operation can easily wear away the composite oxide layer of Al2O3, Ni0 and Cu2O, so that the internal metal cannot be completely isolated from the corrosive medium, and the corrosion resistance of the copper-based nickel-aluminum alloy will also be significantly reduced, resulting in a significant increase in its change amount.

[0041] Referring to Example 1 and Comparative Example 2 and combining with Table 2, it can be seen that relative to Comparative Example 2, the mass loss value and change amount of Example 1 are significantly reduced, which shows that the setting of the spider-web-like micro-nano La2O3 rough structure can effectively improve the corrosion resistance and wear resistance of the corrosion-resistant copper-based nickel-aluminum alloy.

[0042] The reason is that when La is attached to the surface of the copper-based nickel-aluminum alloy in the form of a spider-web-like micro-nano La2O3 rough structure, the spider-web-like micro-nano La2O3 rough structure will form a bionic hydrophobic layer, and the super-hydrophobic properties of La2O3 itself will cooperate to make the corrosion-resistant copper-based nickel-aluminum alloy have an extremely good hydrophobic effect on rainwater, making it difficult for corrosive media to adhere to the surface of the corrosion-resistant copper-based nickel-aluminum alloy, thereby reducing the possibility of Al2O3, Ni0 and Cu2O composite oxide layer breaking, thereby improving the corrosion resistance of the corrosion-resistant copper-based nickel-aluminum alloy. In addition, the spider-web-like micro-nano La2O3 rough structure also has extremely good wear resistance, so that the corrosion-resistant copper-based nickel-aluminum alloy still has extremely good wear resistance after being worn.

[0043] Referring to Examples 1-2 and in combination with Table 2, it can be seen that relative to Example 1, the change value of Example 2 is further reduced, but the mass loss value of Example 2 is slightly increased, which shows that the provision of the nanoporous membrane layer can improve the wear resistance of the corrosion-resistant copper-based nickel alloy, but has a negative impact on the corrosion resistance of the corrosion-resistant copper-based nickel alloy.

[0044] The reason is that the connection effect between the spiderweb-like micro-nano La2O3 rough structure and the Al2O3, Ni0 and Cu2O composite oxide layer needs to be strengthened. After the corrosion-resistant copper-based nickel-aluminum alloy is used for a long time, the spiderweb-like micro-nano La2O3 rough structure is easy to fall off, resulting in the deterioration of its hydrophobic performance.

[0045] After the nanoporous composite film layer is formed on the surface of the copper-based nickel-aluminum alloy, the spider-web-like micro-nano La2O3 rough structure can be inserted into the pores of the nanoporous composite film layer, thereby playing a multi-point supporting and connecting role, effectively reducing the possibility of the spider-web-like micro-nano La2O3 rough structure falling off, and indirectly improving the corrosion resistance of the copper-based nickel-aluminum alloy.

[0046] Referring to Examples 2-3 and in combination with Table 2, it can be seen that, relative to Example 2, the mass wear value of Example 3 is significantly reduced, while the amount of change is basically unchanged, which indicates that the addition of Cr element can effectively improve the corrosion resistance of the corrosion-resistant copper-based nickel-aluminum alloy.

[0047] The reason is that after the Cr element is added, Cr will form a Cr2O3 inner oxide film during the sintering process, and then with the synergistic cooperation of the Al2O3, Ni0 and Cu2O composite oxide layers, better corrosion resistance is obtained.

[0048] Referring to Examples 3-4 and in combination with Table 2, it can be seen that, relative to Example 3, the mass loss value and the change in Example 4 are significantly reduced, which indicates that the addition of Zr can improve the corrosion resistance and wear resistance of the corrosion-resistant copper-based nickel-aluminum alloy to a certain extent.

[0049] The reason is that after the Zr element is added, the Zr element can slightly increase the strength of the Al2O3, Ni0 and Cu2O composite oxide layer as a whole, while improving the connection effect between the spider-web-like micro-nano La2O3 rough structure and the Al2O3, Ni0 and Cu2O composite oxide layer, it can also improve the corrosion resistance of the copper-based nickel-aluminum alloy.

[0050] Referring to Examples 4-6 and in combination with Table 2, it can be seen that relative to Example 4, the mass loss values ​​and changes of Examples 5-6 are slightly improved, which indicates that when the components of the corrosion-resistant copper-based nickel-aluminum alloy adopt the percentages of Example 1, the prepared corrosion-resistant copper-based nickel-aluminum alloy will have better corrosion resistance and wear resistance.

[0051] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A corrosion-resistant copper-based nickel-aluminum alloy, characterized in that: The raw materials include the following mass percentages: Ni 20-26%, Al 6-8%, La 3-5% and trace elements 0-4%, and the balance is Cu.

2. The corrosion-resistant copper-based nickel-aluminum alloy according to claim 1, characterized in that: The La is attached to the surface of the copper-based nickel-aluminum alloy in the form of a spider-web-like micro-nano La2O3 rough structure.

3. The corrosion-resistant copper-based nickel-aluminum alloy according to claim 2, characterized in that: A nanoporous composite membrane layer is formed on the surface of the copper-based nickel-aluminum alloy, and the spider-web-like micro-nano La2O3 rough structure is inserted into the pores of the nanoporous composite membrane layer.

4. The corrosion-resistant copper-based nickel-aluminum alloy according to claim 3, characterized in that: The trace elements include Cr.

5. The corrosion-resistant copper-based nickel-aluminum alloy according to claim 4, characterized in that: The trace elements also include Zr.

6. The corrosion-resistant copper-based nickel-aluminum alloy according to claim 5, characterized in that: The corrosion-resistant copper-based nickel-aluminum alloy comprises the following raw materials in percentage by mass: Ni 20-26%, Al 6-8%, La 3-5%, Cr 1-3% and Zr 1-2%, with the remainder being Cu.

7. A method for preparing the corrosion-resistant copper-based nickel-aluminum alloy according to any one of claims 1 to 2, characterized in that: The following steps are involved: Step 1: First, Cu, Ni, Al and trace elements are mixed in proportion, then melted, homogenized and annealed, and finally immersed in a 3.5% sodium chloride aqueous solution for 3-5 hours for pre-corrosion to prepare a copper-based nickel-aluminum alloy, with a melting temperature of 1300-1400°C, insulation for 10-15 minutes, and a casting temperature of 1250-1300°C; a homogenization annealing temperature of 900-1000°C, insulation for 1-3 hours, and cooling with the furnace; Step 2: Clean the copper-based nickel-aluminum alloy with acetone, anhydrous ethanol and deionized water, and then dry it for use; then prepare lanthanum nitrate electrodeposition solution according to the proportion of La, adjust the voltage to 3V, short-circuit the positive and negative poles of the power supply, adjust the current to 2mA, connect the graphite electrode to the positive pole of the power supply, connect the copper-based nickel-aluminum alloy to the negative pole of the power supply, and electrodeposit for 10 minutes at a water bath temperature of 25°C. Finally, dry the product under a pressure of -0.1Mpa and a temperature of 185°C for 3 hours to obtain a corrosion-resistant copper-based nickel-aluminum alloy; The corrosion-resistant copper-based nickel-aluminum alloy is a copper-based nickel-aluminum alloy with a spider-web-like micro-nano La2O3 rough structure attached to the surface.

8. A method for preparing the corrosion-resistant copper-based nickel-aluminum alloy according to any one of claims 1 to 6, characterized in that: The following steps are involved: Step 1: First, Cu, Ni, Al and trace elements are mixed in proportion, and then melt-cast and homogenize anneal to prepare a copper-based nickel-aluminum alloy, with a melting temperature of 1300-1400°C, insulation for 10-15 minutes, and a casting temperature of 1250-1300°C; the homogenization annealing temperature is 900-1000°C, insulation for 1-3 hours, and cooling with the furnace; Step 2, the copper-based nickel-aluminum alloy is cleaned by acetone, anhydrous ethanol and deionized water, and then dried for standby use; then, an oxalic acid solution with a concentration of 5wt% is prepared, the voltage is adjusted to 50V, the positive and negative electrodes of the power supply are short-circuited, the copper-based nickel-aluminum alloy is connected to the positive electrode of the power supply, the graphite electrode is connected to the negative electrode of the power supply, and the treatment is carried out at a water bath temperature of 0°C for 40min, and finally dried to obtain a nanoporous film layer copper-based nickel-aluminum alloy; Step 3, the nanoporous film layer copper-based nickel-aluminum alloy is cleaned with acetone, anhydrous ethanol and deionized water, and then dried for use; then, a lanthanum nitrate electrodeposition solution is prepared according to the proportion of La, the voltage is adjusted to 3V, the positive and negative electrodes of the power supply are short-circuited, the current is adjusted to 2mA, the graphite electrode is connected to the positive electrode of the power supply, and the nanoporous film layer copper-based nickel-aluminum alloy is connected to the negative electrode of the power supply, and the electrodeposition is carried out at a water bath temperature of 25°C for 10min, and finally the product is placed in an environment of pressure -0.1Mpa and temperature 185°C and dried for 3h to obtain a corrosion-resistant copper-based nickel-aluminum alloy; The corrosion-resistant copper-based nickel-aluminum alloy is a copper-based nickel-aluminum alloy with a nanoporous film layer having a spider-web-like micro-nano La2O3 rough structure attached to the surface.