Stainless steel strip for electronic products and preparation process thereof
Through anodizing treatment and nano-alumina modification, combined with hexafluorotitanic acid and chitosan, the corrosion problem of stainless steel strips in special environments is solved, and its corrosion resistance and mechanical properties are significantly improved.
Patent Information
- Application Number
- CN202411217317.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-02
AI Technical Summary
Traditional stainless steel belts are prone to corrosion and oxidation under special environments such as high humidity, high temperature, acid and alkalinity, which affects its service life and performance stability, and need to improve corrosion resistance.
The stainless steel strip is surface treated by anodizing method, including alkali washing, pickling washing and annealing treatment, modified nano aluminum trioxide is used to combine with organic framework materials, and hexafluorotitanic acid and shell polyester are added to the anodized electrolyte. Sugar, forming a dense oxide film to improve corrosion resistance.
The corrosion resistance and mechanical properties of stainless steel strips are significantly improved. By combining modified nano aluminum trioxide and chitosan, a more uniform and dense oxide film is formed, which enhances its resistance to corrosive substances.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of stainless steel strips, in particular to a stainless steel strip for electronic products and a preparation process thereof. Background Art
[0002] With the widespread application and intelligent development of electronic products, higher requirements are put forward for the metal materials used in electronic products, especially in terms of corrosion resistance and mechanical properties. As a common metal material, stainless steel strip is widely used in the manufacture of electronic products such as mobile phones, laptops, smart watches, etc. due to its good corrosion resistance, mechanical strength and beautiful appearance.
[0003] However, in some special environments, such as high humidity, high temperature, acidity and alkalinity, traditional stainless steel strips may still corrode and oxidize, affecting their service life and performance stability. Therefore, in order to improve the corrosion resistance of stainless steel strips in electronic products, it is particularly important to develop a corrosion-resistant stainless steel strip with excellent performance and its preparation process.
[0004] In order to solve the above problems and improve the corrosion resistance of the stainless steel strip, the present invention provides a stainless steel strip for electronic products and a preparation process thereof. Summary of the invention
[0005] The object of the present invention is to provide a stainless steel strip for electronic products and a preparation process thereof, so as to solve the problems raised in the above background technology.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] A process for preparing a stainless steel strip for electronic products comprises the following steps:
[0008] Step 1: Take the steel strip, place it in an alkaline washing solution at 55-60°C, immerse it for 5-10 minutes, take it out, wash it, and dry it to obtain the alkaline washed steel strip;
[0009] Step 2: Take the alkali-washed steel strip, place it in a pickling solution at a temperature of 40-45°C, immerse it for 20-25 minutes, take it out, wash it, and dry it to obtain the pickled steel strip. After pickling, anneal it at 730-750°C for 40-45 seconds to obtain the pre-treated steel strip;
[0010] Step 3: Anodizing the pretreated steel strip to obtain a stainless steel strip for electronic products;
[0011] The electrolyte used for anodizing includes the following components: deionized water, sulfuric acid, phytic acid, hexafluorotitanic acid, disodium ethylenediaminetetraacetic acid, nano-aluminum oxide composite material, and aluminum sol.
[0012] Preferably, the preparation method of the nano-aluminum oxide composite material comprises the following steps:
[0013] S1: Take amino nano-aluminum trioxide, L-ornithine acetate, and anhydrous N,N-dimethylformamide, stir them evenly in an ice bath, then react them for 70-74 hours under nitrogen protection, centrifuge, wash, and dry to obtain modified nano-aluminum trioxide;
[0014] S2: Take organic framework material, acetonitrile, N,N-dimethylformamide, and modified nano-aluminum oxide, raise the temperature to 45-50° C., react for 22-26 hours, wash, filter, and dry to obtain a nano-aluminum oxide composite material.
[0015] More optimally, the preparation method of the amino-modified nano-aluminum oxide is as follows: take nano-aluminum oxide and anhydrous ethanol, ultrasonically disperse to obtain a nano-aluminum oxide suspension; take anhydrous ethanol and deionized water, stir evenly, add glacial acetic acid, adjust the pH value to 5, drop 3-aminopropyltriethoxysilane, stir evenly, then drop the nano-aluminum oxide suspension, react at 25-35°C for 22-26h, centrifuge, wash, freeze, and dry to obtain the amino-modified nano-aluminum oxide.
[0016] More optimally, the preparation method of the organic framework material is: take sodium fumarate and deionized water, stir evenly to obtain a sodium fumarate solution; take aluminum nitrate nonahydrate and deionized water, stir evenly, add the sodium fumarate solution dropwise, continue stirring for 10-15 minutes, filter, wash, and dry to obtain the organic framework material.
[0017] More optimally, the preparation method of the aluminum sol is: take deionized water, heat it to 80-85°C, add aluminum isopropoxide and nitric acid, stir for 1-2 minutes every 20-30 minutes, react for 7-9 hours, add chitosan, stir evenly, and obtain aluminum sol.
[0018] More optimally, the alkaline washing solution includes the following components: sodium hydroxide, sodium carbonate, and sodium dodecyl sulfate.
[0019] More optimally, the pickling solution includes the following components: sodium dodecyl sulfate, benzotriazole, and hydrochloric acid.
[0020] More optimally, the working conditions of the anodization are: an AC power supply of 1 kW, a constant current of 0.3-0.5 A, a frequency of 100-120 Hz, and a time of 10-15 min.
[0021] More optimally, the steel strip comprises the following components, in percentage by mass: 0.30-0.7wt% Mn, 0.25-0.30wt% Si, 0.15-0.20wt% C, 0.01-0.045wt% S, 0.02-0.045wt% P, 0.1-0.25wt% Cr, 0.1-0.25wt% Ni, and the balance is Fe.
[0022] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0023] (1) The present invention uses an anodic oxidation method to perform surface treatment on a stainless steel strip, thereby improving the corrosion resistance and mechanical properties of the stainless steel strip. First, the stainless steel strip is pre-treated by pickling and alkali washing, and then anodized.
[0024] The present invention uses L-ornithine acetate to modify nano aluminum oxide. L-ornithine acetate has a strong arc suppression ability, and can make the oxide film generated on the surface of the stainless steel strip more dense and have fine holes, thereby improving the corrosion resistance of the oxide film. Then the modified nano aluminum oxide is compounded with an organic framework material. The organic framework has a good pore structure. The modified nano aluminum oxide is compounded with the organic framework material to increase its specific surface area, and the oxide film is more uniform and dense, which effectively increases the tortuosity of corrosive substances entering the surface of the aluminum alloy body, thereby improving the corrosion resistance of the stainless steel strip.
[0025] (2) The present invention adds chitosan to the aluminum sol. Chitosan has good corrosion resistance. At the same time, the present invention adds hexafluorotitanic acid to the anodizing electrolyte. The addition of chitosan promotes the deposition of titanium element, so that titanium element is deposited on the surface of the stainless steel strip, further enhancing the corrosion resistance of the stainless steel strip. DETAILED DESCRIPTION
[0026] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] There is no special restriction on the purchase manufacturers of all raw materials involved in the present invention, and exemplary examples include: Nano-alumina: can be purchased from Sumitomo Chemical of Japan, α-Al2O3 particles, with a particle size of less than 500 nm.
[0028] Embodiment 1: A process for preparing a stainless steel strip for electronic products, comprising the following steps:
[0029] Step 1:
[0030] The steel strip is placed in an alkaline washing solution at 57° C. for 7 minutes, taken out, washed, and dried to obtain an alkaline washed steel strip; the alkaline washing solution comprises the following components: 10 g / L sodium hydroxide, 20 g / L sodium carbonate, and 1 g / L sodium dodecyl sulfate;
[0031] The steel strip comprises the following components, in percentage by mass: 0.5wt% Mn, 0.27wt% Si, 0.18wt% C, 0.03wt% S, 0.04wt% P, 0.2wt% Cr, 0.2wt% Ni, and the balance is Fe;
[0032] Step 2:
[0033] The alkali-washed steel strip is placed in a pickling solution at a temperature of 42°C for 23 minutes, taken out, washed, and dried to obtain a pickled steel strip. After pickling, the steel strip is annealed at 740°C for 43 seconds to obtain a pretreated steel strip. The pickling solution includes the following components: 0.08 g / L sodium dodecyl sulfonate, 2 g / L benzotriazole, and 32% hydrochloric acid. The concentration of the pickling solution is 80 g / L.
[0034] Step 3:
[0035] Anodizing the pretreated steel strip to obtain a stainless steel strip for electronic products;
[0036] The working conditions of anodization are: AC power supply of 1 kW, constant current of 0.3 A, frequency of 100 Hz, and time of 12 min; the electrolyte used for anodization is: 100 mL of deionized water as solvent, including 0.5 g of sulfuric acid, 0.8 g of phytic acid, 0.2 g of hexafluorotitanic acid, 5 g of disodium ethylenediaminetetraacetate, 0.1 g of nano-aluminum oxide composite material, and 1 g of aluminum sol;
[0037] Step 4: Preparation of nano-aluminum oxide composite materials:
[0038] S1: Preparation of organic framework materials:
[0039] Take 8g of sodium fumarate and 125mL of deionized water, stir evenly to obtain a sodium fumarate solution; take 9.5g of aluminum nitrate nonahydrate and 125mL of deionized water, stir evenly, add the sodium fumarate solution dropwise, continue stirring for 12min, filter, wash, and dry to obtain an organic framework material;
[0040] S2: Preparation of modified nano-alumina:
[0041] Take 4g of nano-aluminum trioxide and 200mL of anhydrous ethanol, and perform ultrasonic dispersion to obtain a nano-aluminum trioxide suspension; take 160mL of anhydrous ethanol and 20mL of deionized water, stir evenly, add glacial acetic acid, adjust the pH value to 5, drop 7g of 3-aminopropyltriethoxysilane, stir evenly, then drop the nano-aluminum trioxide suspension, react at 30°C for 24h, centrifuge, wash, freeze, and dry to obtain amino nano-aluminum trioxide;
[0042] Take 3g of amino-modified nano-aluminum trioxide, 1.2g of L-ornithine acetate, and 100mL of anhydrous N,N-dimethylformamide, stir evenly in an ice bath, then react for 72h under nitrogen protection, centrifuge, wash, and dry to obtain modified nano-aluminum trioxide;
[0043] S3: Take 0.5g of organic framework material, 15mL of acetonitrile, 0.5mL of N,N-dimethylformamide, and 0.2g of modified nano-aluminum trioxide, heat to 47°C, react for 24h, wash, filter, and dry to obtain a nano-aluminum trioxide composite material;
[0044] Step 5: Preparation of aluminum sol:
[0045] Take 100 mL of deionized water, heat it to 83°C, add 12 g of aluminum isopropoxide and 11 mL of 1 mol / L nitric acid, stir for 1.5 min every 27 min, react for 8 h, add 2 g of chitosan, stir evenly to obtain aluminum sol.
[0046] Embodiment 2: A process for preparing a stainless steel strip for electronic products, comprising the following steps:
[0047] Step 1:
[0048] The steel strip is placed in an alkaline washing solution at 57° C. for 7 minutes, taken out, washed, and dried to obtain an alkaline washed steel strip; the alkaline washing solution comprises the following components: 10 g / L sodium hydroxide, 20 g / L sodium carbonate, and 1 g / L sodium dodecyl sulfate;
[0049] The steel strip comprises the following components, in percentage by mass: 0.30wt% Mn, 0.25wt% Si, 0.15wt% C, 0.01wt% S, 0.03wt% P, 0.1wt% Cr, 0.1wt% Ni, and the balance is Fe;
[0050] Step 2:
[0051] The alkali-washed steel strip is placed in a pickling solution at a temperature of 40°C for immersion for 20 minutes, taken out, washed, and dried to obtain a pickled steel strip. After pickling, the steel strip is annealed at 730°C for 40 seconds to obtain a pretreated steel strip. The pickling solution includes the following components: 0.08 g / L sodium dodecyl sulfonate, 2 g / L benzotriazole, and 32% hydrochloric acid. The concentration of the pickling solution is 80 g / L.
[0052] Step 3:
[0053] Anodizing the pretreated steel strip to obtain a stainless steel strip for electronic products;
[0054] The working conditions of anodization are: AC power supply of 1 kW, constant current of 0.3 A, frequency of 100 Hz, and time of 10 min; the electrolyte used for anodization is: 100 mL of deionized water as solvent, including 0.5 g of sulfuric acid, 0.8 g of phytic acid, 0.2 g of hexafluorotitanic acid, 5 g of disodium ethylenediaminetetraacetate, 0.1 g of nano-aluminum oxide composite material, and 1 g of aluminum sol;
[0055] Step 4: Preparation of nano-aluminum oxide composite materials:
[0056] S1: Preparation of organic framework materials:
[0057] Take 8g of sodium fumarate and 125mL of deionized water, stir evenly to obtain a sodium fumarate solution; take 9.5g of aluminum nitrate nonahydrate and 125mL of deionized water, stir evenly, add the sodium fumarate solution dropwise, continue stirring for 10min, filter, wash, and dry to obtain an organic framework material;
[0058] S2: Preparation of modified nano-alumina:
[0059] Take 4g of nano-aluminum trioxide and 200mL of anhydrous ethanol, and perform ultrasonic dispersion to obtain a nano-aluminum trioxide suspension; take 160mL of anhydrous ethanol and 20mL of deionized water, stir evenly, add glacial acetic acid, adjust the pH value to 5, drop 7g of 3-aminopropyltriethoxysilane, stir evenly, then drop the nano-aluminum trioxide suspension, react at 25°C for 22h, centrifuge, wash, freeze, and dry to obtain amino nano-aluminum trioxide;
[0060] Take 3g of amino-modified nano-aluminum trioxide, 1.2g of L-ornithine acetate, and 100mL of anhydrous N,N-dimethylformamide, stir evenly in an ice bath, then react for 70h under nitrogen protection, centrifuge, wash, and dry to obtain modified nano-aluminum trioxide;
[0061] S3: Take 0.5g of organic framework material, 15mL of acetonitrile, 0.5mL of N,N-dimethylformamide, and 0.2g of modified nano-aluminum oxide, heat to 45°C, react for 22h, wash, filter, and dry to obtain a nano-aluminum oxide composite material;
[0062] Step 5: Preparation of aluminum sol:
[0063] Take 100 mL of deionized water, heat it to 80°C, add 12 g of aluminum isopropoxide and 11 mL of 1 mol / L nitric acid, stir for 1 min every 20 min, react for 7 h, add 2 g of chitosan, stir evenly to obtain aluminum sol.
[0064] Embodiment 3: A process for preparing a stainless steel strip for electronic products, comprising the following steps:
[0065] Step 1:
[0066] The steel strip is placed in an alkaline washing solution at 60° C. for 10 minutes, taken out, washed, and dried to obtain an alkaline washed steel strip; the alkaline washing solution comprises the following components: 10 g / L sodium hydroxide, 20 g / L sodium carbonate, and 1 g / L sodium dodecyl sulfate;
[0067] The steel strip comprises the following components, in percentage by mass: 0.7wt% of Mn, 0.30wt% of Si, 0.20wt% of C, 0.045wt% of S, 0.045wt% of P, 0.25wt% of Cr, 0.25wt% of Ni, and the balance is Fe;
[0068] Step 2:
[0069] The alkali-washed steel strip is placed in a pickling solution at a temperature of 45°C, immersed for 25 minutes, taken out, washed, and dried to obtain a pickled steel strip. After pickling, the steel strip is annealed at 750°C for 45 seconds to obtain a pretreated steel strip. The pickling solution includes the following components: 0.08 g / L sodium dodecyl sulfonate, 2 g / L benzotriazole, and 32% hydrochloric acid. The concentration of the pickling solution is 80 g / L.
[0070] Step 3:
[0071] Anodizing the pretreated steel strip to obtain a stainless steel strip for electronic products;
[0072] The working conditions of anodization are: AC power supply of 1 kW, constant current of 0.3 A, frequency of 100 Hz, and time of 15 min; the electrolyte used for anodization is: 100 mL of deionized water as solvent, including 0.5 g of sulfuric acid, 0.8 g of phytic acid, 0.2 g of hexafluorotitanic acid, 5 g of disodium ethylenediaminetetraacetate, 0.1 g of nano-aluminum trioxide composite material, and 1 g of aluminum sol;
[0073] Step 4: Preparation of nano-aluminum oxide composite materials:
[0074] S1: Preparation of organic framework materials:
[0075] Take 8g of sodium fumarate and 125mL of deionized water, stir evenly to obtain a sodium fumarate solution; take 9.5g of aluminum nitrate nonahydrate and 125mL of deionized water, stir evenly, add the sodium fumarate solution dropwise, continue stirring for 15min, filter, wash, and dry to obtain an organic framework material;
[0076] S2: Preparation of modified nano-alumina:
[0077] Take 4g of nano-aluminum trioxide and 200mL of anhydrous ethanol, and perform ultrasonic dispersion to obtain a nano-aluminum trioxide suspension; take 160mL of anhydrous ethanol and 20mL of deionized water, stir evenly, add glacial acetic acid, adjust the pH value to 5, drop 7g of 3-aminopropyltriethoxysilane, stir evenly, then drop the nano-aluminum trioxide suspension, react at 35°C for 26h, centrifuge, wash, freeze, and dry to obtain amino nano-aluminum trioxide;
[0078] Take 3g of amino-modified nano-alumina, 1.2g of L-ornithine acetate, and 100mL of anhydrous N,N-dimethylformamide, stir evenly in an ice bath, then react for 74h under nitrogen protection, centrifuge, wash, and dry to obtain modified nano-alumina;
[0079] S3: Take 0.5g of organic framework material, 15mL of acetonitrile, 0.5mL of N,N-dimethylformamide, and 0.2g of modified nano-aluminum oxide, heat to 50°C, react for 26h, wash, filter, and dry to obtain a nano-aluminum oxide composite material;
[0080] Step 5: Preparation of aluminum sol:
[0081] Take 100 mL of deionized water, heat it to 85°C, add 12 g of aluminum isopropoxide and 11 mL of 1 mol / L nitric acid, stir for 2 min every 30 min, react for 9 h, add 2 g of chitosan, stir evenly to obtain aluminum sol.
[0082] Comparative Example 1: L-ornithine acetate is not used to modify the nano-aluminum oxide, and the rest is the same as Example 1:
[0083] Step 1:
[0084] The steel strip is placed in an alkaline washing solution at 57° C. for 7 minutes, taken out, washed, and dried to obtain an alkaline washed steel strip; the alkaline washing solution comprises the following components: 10 g / L sodium hydroxide, 20 g / L sodium carbonate, and 1 g / L sodium dodecyl sulfate;
[0085] The steel strip comprises the following components, in percentage by mass: 0.5wt% Mn, 0.27wt% Si, 0.18wt% C, 0.03wt% S, 0.04wt% P, 0.2wt% Cr, 0.2wt% Ni, and the balance is Fe;
[0086] Step 2:
[0087] The alkali-washed steel strip is placed in a pickling solution at a temperature of 42°C for 23 minutes, taken out, washed, and dried to obtain a pickled steel strip. After pickling, the steel strip is annealed at 740°C for 43 seconds to obtain a pretreated steel strip. The pickling solution includes the following components: 0.08 g / L sodium dodecyl sulfonate, 2 g / L benzotriazole, and 32% hydrochloric acid. The concentration of the pickling solution is 80 g / L.
[0088] Step 3:
[0089] Anodizing the pretreated steel strip to obtain a stainless steel strip for electronic products;
[0090] The working conditions of anodization are: AC power supply of 1 kW, constant current of 0.3 A, frequency of 100 Hz, and time of 12 min; the electrolyte used for anodization is: 100 mL of deionized water as solvent, including 0.5 g of sulfuric acid, 0.8 g of phytic acid, 0.2 g of hexafluorotitanic acid, 5 g of disodium ethylenediaminetetraacetate, 0.1 g of nano-aluminum oxide composite material, and 1 g of aluminum sol;
[0091] Step 4: Preparation of nano-aluminum oxide composite materials:
[0092] S1: Preparation of organic framework materials:
[0093] Take 8g of sodium fumarate and 125mL of deionized water, stir evenly to obtain a sodium fumarate solution; take 9.5g of aluminum nitrate nonahydrate and 125mL of deionized water, stir evenly, add the sodium fumarate solution dropwise, continue stirring for 12min, filter, wash, and dry to obtain an organic framework material;
[0094] S2: Preparation of modified nano-alumina:
[0095] Take 4g of nano-aluminum trioxide and 200mL of anhydrous ethanol, and perform ultrasonic dispersion to obtain a nano-aluminum trioxide suspension; take 160mL of anhydrous ethanol and 20mL of deionized water, stir evenly, add glacial acetic acid, adjust the pH value to 5, drop 7g of 3-aminopropyltriethoxysilane, stir evenly, then drop the nano-aluminum trioxide suspension, react at 30°C for 24h, centrifuge, wash, freeze, and dry to obtain amino nano-aluminum trioxide;
[0096] S3: Take 0.5g of organic framework material, 15mL of acetonitrile, 0.5mL of N,N-dimethylformamide, and 0.2g of amino-modified nano-aluminum oxide, heat to 47°C, react for 24h, wash, filter, and dry to obtain a nano-aluminum oxide composite material;
[0097] Step 5: Preparation of aluminum sol:
[0098] Take 100 mL of deionized water, heat it to 83°C, add 12 g of aluminum isopropoxide and 11 mL of 1 mol / L nitric acid, stir for 1.5 min every 27 min, react for 8 h, add 2 g of chitosan, stir evenly to obtain aluminum sol.
[0099] Comparative Example 2: Hexafluorotitanic acid was not added to the anodizing electrolyte, and the rest was the same as Example 1:
[0100] Step 1:
[0101] The steel strip is placed in an alkaline washing solution at 57° C. for 7 minutes, taken out, washed, and dried to obtain an alkaline washed steel strip; the alkaline washing solution comprises the following components: 10 g / L sodium hydroxide, 20 g / L sodium carbonate, and 1 g / L sodium dodecyl sulfate;
[0102] The steel strip comprises the following components, in percentage by mass: 0.5wt% Mn, 0.27wt% Si, 0.18wt% C, 0.03wt% S, 0.04wt% P, 0.2wt% Cr, 0.2wt% Ni, and the balance is Fe;
[0103] Step 2:
[0104] The alkali-washed steel strip is placed in a pickling solution at a temperature of 42°C for 23 minutes, taken out, washed, and dried to obtain a pickled steel strip. After pickling, the steel strip is annealed at 740°C for 43 seconds to obtain a pretreated steel strip. The pickling solution includes the following components: 0.08 g / L sodium dodecyl sulfonate, 2 g / L benzotriazole, and 32% hydrochloric acid. The concentration of the pickling solution is 80 g / L.
[0105] Step 3:
[0106] Anodizing the pretreated steel strip to obtain a stainless steel strip for electronic products;
[0107] The working conditions of anodization are: AC power supply of 1 kW, constant current of 0.3 A, frequency of 100 Hz, and time of 12 min; the electrolyte used for anodization is: 100 mL of deionized water as solvent, including 0.5 g of sulfuric acid, 0.8 g of phytic acid, 5 g of disodium ethylenediaminetetraacetic acid, 0.1 g of nano-aluminum oxide composite material, and 1 g of aluminum sol;
[0108] Step 4: Preparation of nano-aluminum oxide composite materials:
[0109] S1: Preparation of organic framework materials:
[0110] Take 8g of sodium fumarate and 125mL of deionized water, stir evenly to obtain a sodium fumarate solution; take 9.5g of aluminum nitrate nonahydrate and 125mL of deionized water, stir evenly, add the sodium fumarate solution dropwise, continue stirring for 12min, filter, wash, and dry to obtain an organic framework material;
[0111] S2: Preparation of modified nano-alumina:
[0112] Take 4g of nano-aluminum trioxide and 200mL of anhydrous ethanol, and perform ultrasonic dispersion to obtain a nano-aluminum trioxide suspension; take 160mL of anhydrous ethanol and 20mL of deionized water, stir evenly, add glacial acetic acid, adjust the pH value to 5, drop 7g of 3-aminopropyltriethoxysilane, stir evenly, then drop the nano-aluminum trioxide suspension, react at 30°C for 24h, centrifuge, wash, freeze, and dry to obtain amino nano-aluminum trioxide;
[0113] Take 3g of amino-modified nano-aluminum trioxide, 1.2g of L-ornithine acetate, and 100mL of anhydrous N,N-dimethylformamide, stir evenly in an ice bath, then react for 72h under nitrogen protection, centrifuge, wash, and dry to obtain modified nano-aluminum trioxide;
[0114] S3: Take 0.5g of organic framework material, 15mL of acetonitrile, 0.5mL of N,N-dimethylformamide, and 0.2g of modified nano-aluminum trioxide, heat to 47°C, react for 24h, wash, filter, and dry to obtain a nano-aluminum trioxide composite material;
[0115] Step 5: Preparation of aluminum sol:
[0116] Take 100 mL of deionized water, heat it to 83°C, add 12 g of aluminum isopropoxide and 11 mL of 1 mol / L nitric acid, stir for 1.5 min every 27 min, react for 8 h, add 2 g of chitosan, stir evenly to obtain aluminum sol.
[0117] Comparative Example 3: Chitosan was not added to the aluminum sol, and the rest was the same as in Example 1:
[0118] Step 1:
[0119] The steel strip is placed in an alkaline washing solution at 57° C. for 7 minutes, taken out, washed, and dried to obtain an alkaline washed steel strip; the alkaline washing solution comprises the following components: 10 g / L sodium hydroxide, 20 g / L sodium carbonate, and 1 g / L sodium dodecyl sulfate;
[0120] The steel strip comprises the following components, in percentage by mass: 0.5wt% Mn, 0.27wt% Si, 0.18wt% C, 0.03wt% S, 0.04wt% P, 0.2wt% Cr, 0.2wt% Ni, and the balance is Fe;
[0121] Step 2:
[0122] The alkali-washed steel strip is placed in a pickling solution at a temperature of 42°C for 23 minutes, taken out, washed, and dried to obtain a pickled steel strip. After pickling, the steel strip is annealed at 740°C for 43 seconds to obtain a pretreated steel strip. The pickling solution includes the following components: 0.08 g / L sodium dodecyl sulfonate, 2 g / L benzotriazole, and 32% hydrochloric acid. The concentration of the pickling solution is 80 g / L.
[0123] Step 3:
[0124] Anodizing the pretreated steel strip to obtain a stainless steel strip for electronic products;
[0125] The working conditions of anodization are: AC power supply of 1 kW, constant current of 0.3 A, frequency of 100 Hz, and time of 12 min; the electrolyte used for anodization is: 100 mL of deionized water as solvent, including 0.5 g of sulfuric acid, 0.8 g of phytic acid, 0.2 g of hexafluorotitanic acid, 5 g of disodium ethylenediaminetetraacetate, 0.1 g of nano-aluminum oxide composite material, and 1 g of aluminum sol;
[0126] Step 4: Preparation of nano-aluminum oxide composite materials:
[0127] S1: Preparation of organic framework materials:
[0128] Take 8g of sodium fumarate and 125mL of deionized water, stir evenly to obtain a sodium fumarate solution; take 9.5g of aluminum nitrate nonahydrate and 125mL of deionized water, stir evenly, add the sodium fumarate solution dropwise, continue stirring for 12min, filter, wash, and dry to obtain an organic framework material;
[0129] S2: Preparation of modified nano-alumina:
[0130] Take 4g of nano-aluminum trioxide and 200mL of anhydrous ethanol, and perform ultrasonic dispersion to obtain a nano-aluminum trioxide suspension; take 160mL of anhydrous ethanol and 20mL of deionized water, stir evenly, add glacial acetic acid, adjust the pH value to 5, drop 7g of 3-aminopropyltriethoxysilane, stir evenly, then drop the nano-aluminum trioxide suspension, react at 30°C for 24h, centrifuge, wash, freeze, and dry to obtain amino nano-aluminum trioxide;
[0131] Take 3g of amino-modified nano-aluminum trioxide, 1.2g of L-ornithine acetate, and 100mL of anhydrous N,N-dimethylformamide, stir evenly in an ice bath, then react for 72h under nitrogen protection, centrifuge, wash, and dry to obtain modified nano-aluminum trioxide;
[0132] S3: Take 0.5g of organic framework material, 15mL of acetonitrile, 0.5mL of N,N-dimethylformamide, and 0.2g of modified nano-aluminum trioxide, heat to 47°C, react for 24h, wash, filter, and dry to obtain a nano-aluminum trioxide composite material;
[0133] Step 5: Preparation of aluminum sol:
[0134] Take 100 mL of deionized water, heat it to 83°C, add 12 g of aluminum isopropoxide and 11 mL of 1 mol / L nitric acid, stir for 1.5 min every 27 min, react for 8 h, stir evenly, and obtain aluminum sol.
[0135] experiment:
[0136] The performance test was carried out using the stainless steel strips for electronic products prepared in Examples 1-3 and Comparative Examples 1-3. The sample was used as the working electrode, the calomel electrode was used as the reference electrode, the platinum electrode was used as the auxiliary electrode, the electrochemical etching solution was a 3.5% sodium chloride aqueous solution, the scanning potential speed was 2 mv / s, and the sample area was 1 cm 2 , detect the corrosion current density of the stainless steel strip; take GB / T6459-86 as the reference standard, conduct acetic acid salt spray test on the sample, pH value is 3.2, test temperature is 35℃, deposition amount is 1.5ml / h, test time is 96h, detect the corrosion rate of the sample, and the data obtained are as follows:
[0137]
[0138] Conclusion: From the comparison of the data in the table, it can be seen that in Example 1, L-ornithine acetate is not used to modify the nano-aluminum oxide, and the corrosion resistance of the oxide film is deteriorated. In Example 2, hexafluorotitanic acid is not added to the anodizing electrolyte, and the corrosion resistance of the stainless steel strip is deteriorated. In Example 3, chitosan is not added to the aluminum sol, and the corrosion resistance of the stainless steel strip is deteriorated. In Examples 1-3, chitosan is added to the aluminum sol, and chitosan has good corrosion resistance. At the same time, hexafluorotitanic acid is added to the anodizing electrolyte. The addition of chitosan promotes the deposition of titanium, so that titanium is deposited on the surface of the stainless steel strip, further enhancing the corrosion resistance of the stainless steel strip. Examples 1-3 also use L-ornithine acetate to modify the nano-aluminum oxide. L-ornithine acetate has a strong arc suppression ability, which can make the oxide film generated on the surface of the stainless steel strip more dense and with smaller pores, thereby improving the corrosion resistance of the oxide film.
[0139] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A process for preparing a stainless steel strip for electronic products, characterized in that: The following steps are involved: Step 1: Take the steel strip, place it in an alkaline washing solution at 55-60°C, immerse it for 5-10 minutes, take it out, wash it, and dry it to obtain the alkaline washed steel strip; Step 2: Take the alkali-washed steel strip, place it in a pickling solution at a temperature of 40-45°C, immerse it for 20-25 minutes, take it out, wash it, and dry it to obtain the pickled steel strip. After pickling, anneal it at 730-750°C for 40-45 seconds to obtain the pre-treated steel strip; Step 3: Anodizing the pretreated steel strip to obtain a stainless steel strip for electronic products; The electrolyte used for anodizing includes the following components: deionized water, sulfuric acid, phytic acid, hexafluorotitanic acid, disodium ethylenediaminetetraacetic acid, nano-aluminum trioxide composite material, aluminum sol; The preparation method of the nano aluminum oxide composite material comprises the following steps: S1: Take amino nano-aluminum trioxide, L-ornithine acetate, and anhydrous N,N-dimethylformamide, stir them evenly in an ice bath, then react them for 70-74 hours under nitrogen protection, centrifuge, wash, and dry to obtain modified nano-aluminum trioxide; S2: Take organic framework material, acetonitrile, N,N-dimethylformamide, and modified nano-aluminum oxide, raise the temperature to 45-50°C, react for 22-26 hours, wash, filter, and dry to obtain a nano-aluminum oxide composite material; The preparation method of the aluminum sol is as follows: take deionized water, heat it to 80-85° C., add aluminum isopropoxide and nitric acid, stir for 1-2 minutes every 20-30 minutes, react for 7-9 hours, add chitosan, stir evenly, and obtain the aluminum sol.
2. The process for preparing a stainless steel strip for electronic products according to claim 1, characterized in that: The preparation method of the amino-modified nano-aluminum oxide comprises the following steps: taking nano-aluminum oxide and anhydrous ethanol, performing ultrasonic dispersion to obtain a nano-aluminum oxide suspension; taking anhydrous ethanol and deionized water, stirring evenly, adding glacial acetic acid, adjusting the pH value to 5, dripping 3-aminopropyltriethoxysilane, stirring evenly, then dripping the nano-aluminum oxide suspension, reacting at 25-35° C. for 22-26 hours, centrifuging, washing, freezing, and drying to obtain the amino-modified nano-aluminum oxide.
3. The process for preparing a stainless steel strip for electronic products according to claim 1, characterized in that: The preparation method of the organic framework material is as follows: sodium fumarate and deionized water are taken, stirred evenly to obtain a sodium fumarate solution; aluminum nitrate nonahydrate and deionized water are taken, stirred evenly, the sodium fumarate solution is added dropwise, stirring is continued for 10-15 minutes, filtering, washing and drying to obtain the organic framework material.
4. The process for preparing a stainless steel strip for electronic products according to claim 1, characterized in that: The alkaline washing solution comprises the following components: sodium hydroxide, sodium carbonate and sodium dodecyl sulfate.
5. The process for preparing a stainless steel strip for electronic products according to claim 1, characterized in that: The pickling solution comprises the following components: sodium dodecyl sulfonate, benzotriazole and hydrochloric acid.
6. The process for preparing a stainless steel strip for electronic products according to claim 1, characterized in that: The working conditions of the anodization are: an AC power supply of 1 kW, a constant current of 0.3-0.5 A, a frequency of 100-120 Hz, and a time of 10-15 min.
7. The process for preparing a stainless steel strip for electronic products according to claim 1, characterized in that: The steel strip is composed of the following components, calculated by mass percentage: 0.30-0.7wt% Mn, 0.25-0.30wt% Si, 0.15-0.20wt% C, 0.01-0.045wt% S, 0.02-0.045wt% P, 0.1-0.25wt% Cr, 0.1-0.25wt% Ni, and the balance is Fe.
8. A stainless steel strip for electronic products prepared according to the process for preparing a stainless steel strip for electronic products according to any one of claims 1 to 7.