Waterproof flame-retardant fabric and preparation method thereof

Through the mixed melting of basalt and zirconium phosphate and the maleic anhydride grafted nanometal copper technology, the modified polytetrafluoroethylene fiber weaving solves the problem of both flame retardant and waterproof properties of the fabric and achieves efficient flame retardant and waterproof effects.

CN118727262AInactive Publication Date: 2024-10-01XIANGCHENG YONGTU CLOTHING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410631640.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-21
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

It is difficult for existing fabrics to improve the flame retardant properties while also taking into account the waterproof properties, especially because the dispersion and compatibility of a single phosphorus flame retardant in the matrix is ​​insufficient.

Method used

The mixed masterbatch is prepared by mixing and melting basalt and zirconium phosphate, and the mixed filler is prepared by grafting nano-metal copper with maleic anhydride. The modified polytetrafluoroethylene fiber is woven and combined with programmed temperature control segmented continuous sintering technology to form an ultra-fine fiber network. shape structure.

Benefits of technology

It achieves both high-efficiency flame-retardant and waterproof properties of the fabric. By improving the mechanical structure of the basalt and increasing the activity of the fiber surface, the flame-retardant and waterproof properties are improved, making the fabric have lasting flame-retardant effects and super-hydrophobic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004850444030000081
    Figure BDA0004850444030000081
Patent Text Reader

Abstract

The invention discloses a waterproof flame-retardant fabric and a preparation method thereof, and relates to the field of fabrics. According to the preparation method, basalt and zirconium phosphate are mixed, melted and granulated to improve a crystal structure, and then mixed master batches are soaked in a solution of ammonium phosphate to improve the bonding strength of the master batches in polymer fibers; then, the mixed master batch is subjected to ammonia fumigation and oxidation, an efficient flame retardant with the volume obviously increased and the phosphorus-nitrogen synergistic flame retardant effect is formed in the fiber, and therefore the lasting flame retardant performance is obtained. Secondly, nano metal copper is grafted with mixed master batches and maleic anhydride, the flame retardant property is improved, and meanwhile, a super-hydrophobic coarse structure is formed by micron-level mixed master batches and nano-level metal copper, so that the waterproof performance of the fiber is more optimized; in the spinning process, temperature-controlled segmented continuous sintering is adopted to form a bead-like superfine fiber net structure, so that the woven fabric achieves a super-hydrophobic effect. The prepared fabric has waterproof and flame-retardant effects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fabrics, in particular to a waterproof and flame-retardant fabric and a preparation method thereof. Background Art

[0002] The combustion performance of indoor textiles and soft furniture has a significant impact on the occurrence and spread of fire. In order to protect personal and property safety, developed countries and regions such as the United States, the European Union, and Canada began to regulate in the form of legislation as early as the 1950s, and have continuously upgraded and improved it. China is also paying more and more attention to the flame retardant functionality of fabrics.

[0003] In the field of fabrics, traditional flame retardant properties usually come from the addition of cumin chicken. For example, phosphorus-based flame retardants have gradually become the preferred flame retardants in flame retardant modification due to their high efficiency, low smoke, and non-toxicity. However, the modification of a single phosphorus-based flame retardant often requires a higher phosphorus content to achieve the flame retardant and droplet suppression effects of the material, which also faces the problem of how to improve the reactivity of the flame retardant or the dispersibility and compatibility in the matrix. Therefore, through the addition of a variety of flame retardant elements or flame retardants, such as carbon nanotubes, inorganic nanomaterials, metal oxides and other synergistic flame retardants, a better synergistic flame retardant effect is formed with phosphorus-containing flame retardants.

[0004] How to make the fabric highly flame retardant while taking into account waterproof performance is the research direction of the present invention. The above purpose is achieved by compounding flame retardant fillers and polymer fiber raw materials. The present invention provides a waterproof flame retardant fabric and a preparation method thereof. Summary of the invention

[0005] The purpose of the present invention is to provide a waterproof and flame-retardant fabric and a preparation method thereof, so as to solve the problems existing in the prior art.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions: a waterproof and flame-retardant fabric, which is made of mixed masterbatch prepared from basalt, and woven from mixed filler modified polytetrafluoroethylene fibers prepared by maleic anhydride grafting nano-metal copper.

[0007] Furthermore, the mixed masterbatch is obtained by mixing basalt and zirconium phosphate, melting and granulating, and then soaking and fumigating with ammonia.

[0008] Furthermore, the modified polytetrafluoroethylene fiber is sintered continuously in stages with programmed temperature control during the spinning process to form a beaded ultrafine fiber mesh structure.

[0009] Furthermore, a method for preparing a waterproof and flame-retardant fabric comprises the following preparation steps:

[0010] (1) Crush and mix basalt ore and zirconium phosphate in a mass ratio of 100:1-5 to obtain mixed particles with an average particle size of 50 μm; melt the mixed particles at 1400°C to form a spinning melt; draw the spinning melt and granulate it to obtain a basalt masterbatch with a diameter of 20 μm; immerse the basalt masterbatch in an aqueous solution containing 3wt% ammonium phosphate for 1 hour, take it out and dry it at room temperature for 2 hours to obtain an activated basalt masterbatch; fumigate the activated basalt masterbatch with ammonia at 30-70°C for 10-20 minutes; and immerse the activated basalt masterbatch in a clean ammonia-filled space of 1.0-2.0m 3 Under the conditions, the ammonia flow rate is 200-600L / min; after the ammonia fumigation is completed, it is immersed in the oxidation solution at 25°C for 20-60min, and the solid is taken and dried at 60°C for 24h to obtain the mixed masterbatch;

[0011] (2) Add maleic anhydride to NN dimethylformamide, stir and mix to dissolve, add the mixed masterbatch, and heat to react at 98°C for 3 hours, wherein the weight ratio of the mixed masterbatch, maleic anhydride and NN dimethylformamide is 1:3:4; wash the grafted masterbatch with deionized water and acetone, and then dry it at 45°C for 2 hours, add it to the prepared metal salt solution, the mass ratio of the mixed masterbatch to the metal salt solution is 1:10, stir and react at 30°C at 60 rpm for 2 hours, take out the solid, wash it with deionized water 3 times, and dry it at 45°C for 2 hours to obtain a mixed filler;

[0012] (3) dissolving polyvinyl alcohol in water to prepare a uniform solution with a mass concentration of 30%; stirring 20-24 parts of polytetrafluoroethylene, 10-20 parts of water, 10-12 parts of emulsifier and 8-10 parts of initiator at 60° C. and 200 rpm for 2 hours to form a polytetrafluoroethylene emulsion; then adding the polytetrafluoroethylene emulsion to the uniform solution with stirring at 60 rpm, and then adding 4-8 parts of mixed filler, stirring at 40° C. and 200 rpm for 2-4 hours to obtain a spinning solution, spinning the spinning solution using a screw extruder, cooling, and stretching to obtain polytetrafluoroethylene fiber, wherein the cooling temperature is 16-18° C., the melting temperature in the screw extruder is 250° C.-270° C., and the stretching rate is 2-4 times;

[0013] (4) placing the polytetrafluoroethylene fiber in a high temperature furnace and sintering it under the condition of continuous flow of atmosphere; the sintering adopts program temperature control and continuous sintering, keeping the temperature at 90℃-120℃ for 30-120min, heating from 90℃-120℃ to 250℃-300℃ at a rate of 4-10℃ / min, and keeping the temperature at 250℃-300℃ for 30-120min; heating from 250℃-300℃ to 370℃-410℃ at a rate of 2-8℃ / min, and keeping the temperature at 370℃-410℃ for 20-120min; after cooling to room temperature, weaving the modified polytetrafluoroethylene fiber into a 150g / cm 2 fabric.

[0014] Furthermore, the oxidizing liquid in step (1) is a hydrogen peroxide aqueous solution with a mass fraction of 0.1-0.5%.

[0015] Furthermore, the metal salt solution in step (2) is a copper sulfate aqueous solution with a molar concentration of 0.09 mol / L.

[0016] Furthermore, in step (3), the emulsifier is ammonium perfluorooctanoate and the initiator is persulfate.

[0017] Furthermore, in step (3), the dry weight ratio of polyvinyl alcohol to polytetrafluoroethylene is 1:1-20.

[0018] Furthermore, the diameter of the polytetrafluoroethylene fiber spun in step (3) is 50-80 μm.

[0019] Furthermore, the flowing atmosphere in step (4) is nitrogen.

[0020] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0021] The present invention uses basalt to prepare mixed masterbatch, and uses maleic anhydride grafted nano-metal copper to prepare mixed filler modified polytetrafluoroethylene fiber to weave fabrics to achieve waterproof and flame retardant effects.

[0022] Firstly, basalt and zirconium phosphate are mixed and melt-drawn to prepare a mixed masterbatch, and then the mixed basalt masterbatch is immersed in an ammonium phosphate solution for pretreatment; zirconium phosphate is mixed in the masterbatch to improve the crystal structure of basalt and thus improve the mechanical structure of the basalt mixed masterbatch, and the micron-level masterbatch is immersed in ammonium phosphate, and the phosphate ions increase the surface roughness of the masterbatch and can improve its surface activity, thereby increasing the bonding strength of the masterbatch in the polymer fiber and chemically bonding it with the free groups in polytetrafluoroethylene; then the mixed masterbatch is fumigated and oxidized with ammonia, and intermittent processing is used to infiltrate ammonia into the interior of the masterbatch, so that ammonia and phosphate ions are cross-linked inside the fiber, and a high-efficiency flame retardant with phosphorus-nitrogen synergistic flame retardant effect with a significantly increased volume that cannot be washed out or is difficult to wash out is formed inside the fiber, and the flame retardant performance is made more stable after oxidation, thereby obtaining a long-lasting flame retardant performance.

[0023] Secondly, a mixed filler modified polytetrafluoroethylene fiber is prepared by grafting nano-metal copper with a mixed masterbatch and maleic anhydride. The carboxyl group is grafted with metal ions to load the surface of the fiber with metal ions, thereby improving the flame retardant properties of the polytetrafluoroethylene fiber. At the same time, the micron-level mixed masterbatch and the nano-level metal copper form a super-hydrophobic rough structure, which optimizes the waterproof performance of the fiber. After spinning, a program-controlled temperature-controlled segmented continuous sintering is adopted, and the polytetrafluoroethylene particles begin to reorient and arrange. Then, the carrier decomposes at the right time, and the polytetrafluoroethylene fiber is further oriented and rearranged to form a beaded ultrafine fiber mesh structure, so that the woven fabric achieves a super-hydrophobic effect. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0025] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the test methods of various indicators of a waterproof and flame-retardant fabric prepared in the following examples as follows:

[0026] Flame retardancy: The test is carried out using the test method described in "GB / T 5455 Textiles burning performance test: vertical method".

[0027] Waterproofness: Determined according to GB / T 4745-2012 “Testing and evaluation of the waterproof performance of textiles - Water contact method”.

[0028] Example 1

[0029] (1) Crush and mix basalt ore and zirconium phosphate in a mass ratio of 100:1 to obtain mixed particles with an average particle size of 50 μm; melt the mixed particles at 1400°C to form a spinning melt; draw the spinning melt and granulate it to obtain a basalt masterbatch with a diameter of 20 μm; immerse the basalt masterbatch in an aqueous solution containing 3 wt% of ammonium phosphate for 1 hour, take it out and dry it at room temperature for 2 hours to obtain an activated basalt masterbatch; fumigate the activated basalt masterbatch with ammonia at 30°C for 10 minutes; and immerse the basalt masterbatch in a clean ammonia-filled space of 1.0 m 3 Under the conditions, the ammonia flow rate is 200L / min; after the ammonia fumigation is completed, it is immersed in a 0.1% hydrogen peroxide aqueous solution at 25°C for 20 minutes, and the solid is taken and dried at 60°C for 24 hours to obtain a mixed masterbatch;

[0030] (2) Add maleic anhydride to NN dimethylformamide, stir and dissolve, add the mixed masterbatch, and heat at 98°C for 3 hours, wherein the weight ratio of the mixed masterbatch, maleic anhydride and NN dimethylformamide is 1:3:4; wash the grafted masterbatch with deionized water and acetone, and then dry it at 45°C for 2 hours, add it to the prepared copper sulfate aqueous solution with a molar concentration of 0.09 mol / L, the mass ratio of the mixed masterbatch to the metal salt solution is 1:10, stir and react at 30°C at 60 rpm for 2 hours, take out the solid, wash it with deionized water 3 times, and dry it at 45°C for 2 hours to obtain a mixed filler;

[0031] (3) dissolving polyvinyl alcohol in water to prepare a uniform solution with a mass concentration of 30%; stirring 20 parts of polytetrafluoroethylene, 10 parts of water, 10 parts of ammonium perfluorooctanoate and 8 parts of persulfate at 60°C at 200 rpm for 2 hours to form a polytetrafluoroethylene emulsion; then adding the polytetrafluoroethylene emulsion to the uniform solution at 60 rpm, with a dry weight ratio of polyvinyl alcohol to polytetrafluoroethylene of 1:1; then adding 4 parts of mixed filler, stirring at 40°C at 200 rpm for 2 hours to obtain a spinning solution, spinning the spinning solution using a screw extruder, cooling, and stretching to obtain polytetrafluoroethylene fiber, wherein the cooling temperature is 16°C, the melting temperature in the screw extruder is 250°C, the stretching rate is 2 times, and the fiber diameter is 50 μm;

[0032] (4) The polytetrafluoroethylene fiber is placed in a high-temperature furnace and sintered under the condition of continuous flow of nitrogen atmosphere; the sintering adopts program temperature control and segmented continuous sintering, keeping the temperature at 90°C for 30 minutes, heating from 90°C to 250°C at a rate of 4°C / min, and keeping the temperature at 250°C for 30 minutes; heating from 250°C to 370°C at a rate of 2°C / min, and keeping the temperature at 370°C for 20 minutes; after cooling to room temperature, the modified polytetrafluoroethylene fiber is woven into a 150 g / cm 2 fabric.

[0033] Example 2

[0034] (1) Crush and mix basalt ore and zirconium phosphate in a mass ratio of 100:3 to obtain mixed particles with an average particle size of 50 μm; melt the mixed particles at 1400°C to form a spinning melt; draw the spinning melt and granulate it to obtain a basalt masterbatch with a diameter of 20 μm; immerse the basalt masterbatch in an aqueous solution containing 3 wt% ammonium phosphate for 1 hour, take out and dry it at room temperature for 2 hours to obtain an activated basalt masterbatch; fumigate the activated basalt masterbatch with ammonia at 50°C for 15 minutes; and immerse the basalt masterbatch in a clean ammonia-filled space of 1.5 m 3 Under the conditions, the ammonia flow rate is 400L / min; after the ammonia fumigation is completed, it is immersed in a 0.3% hydrogen peroxide aqueous solution at 25°C for 40 minutes, and the solid is taken and dried at 60°C for 24 hours to obtain a mixed masterbatch;

[0035] (2) Add maleic anhydride to NN dimethylformamide, stir and dissolve, add the mixed masterbatch, and heat at 98°C for 3 hours, wherein the weight ratio of the mixed masterbatch, maleic anhydride and NN dimethylformamide is 1:3:4; wash the grafted masterbatch with deionized water and acetone, and then dry it at 45°C for 2 hours, add it to the prepared copper sulfate aqueous solution with a molar concentration of 0.09 mol / L, the mass ratio of the mixed masterbatch to the metal salt solution is 1:10, stir and react at 30°C at 60 rpm for 2 hours, take out the solid, wash it with deionized water 3 times, and dry it at 45°C for 2 hours to obtain a mixed filler;

[0036] (3) dissolving polyvinyl alcohol in water to prepare a uniform solution with a mass concentration of 30%; stirring 22 parts of polytetrafluoroethylene, 15 parts of water, 11 parts of ammonium perfluorooctanoate and 9 parts of persulfate at 60°C at 200 rpm for 2 hours to form a polytetrafluoroethylene emulsion; then adding the polytetrafluoroethylene emulsion to the uniform solution at 60 rpm, with a dry weight ratio of polyvinyl alcohol to polytetrafluoroethylene of 1:10; then adding 6 parts of mixed filler, stirring at 40°C at 200 rpm for 3 hours to obtain a spinning solution, spinning the spinning solution using a screw extruder, cooling, and stretching to obtain polytetrafluoroethylene fiber, wherein the cooling temperature is 17°C, the melting temperature in the screw extruder is 260°C, the stretching rate is 3 times, and the fiber diameter is 65 μm;

[0037] (4) The polytetrafluoroethylene fiber is placed in a high-temperature furnace and sintered under the condition of continuous flow of nitrogen atmosphere; the sintering adopts program temperature control and segmented continuous sintering, keeping the temperature at 105°C for 75 minutes, heating from 105°C to 275°C at a rate of 7°C / min, and keeping the temperature at 275°C for 75 minutes; heating from 275°C to 390°C at a rate of 5°C / min, and keeping the temperature at 390°C for 70 minutes; after cooling to room temperature, the modified polytetrafluoroethylene fiber is woven into a 150 g / cm 2 fabric.

[0038] Example 3

[0039] (1) Crush and mix basalt ore and zirconium phosphate in a mass ratio of 100:5 to obtain mixed particles with an average particle size of 50 μm; melt the mixed particles at 1400°C to form a spinning melt; draw the spinning melt and granulate it to obtain a basalt masterbatch with a diameter of 20 μm; immerse the basalt masterbatch in an aqueous solution containing 3 wt% of ammonium phosphate for 1 hour, take out and dry it at room temperature for 2 hours to obtain an activated basalt masterbatch; fumigate the activated basalt masterbatch with ammonia at 70°C for 20 minutes; and immerse the basalt masterbatch in a clean ammonia-filled space of 2.0 m 3 Under the conditions, the ammonia flow rate is 600L / min; after the ammonia fumigation is completed, it is immersed in a 0.5% hydrogen peroxide aqueous solution at 25°C for 60 minutes, and the solid is taken and dried at 60°C for 24 hours to obtain a mixed masterbatch;

[0040] (2) Add maleic anhydride to NN dimethylformamide, stir and dissolve, add the mixed masterbatch, and heat at 98°C for 3 hours, wherein the weight ratio of the mixed masterbatch, maleic anhydride and NN dimethylformamide is 1:3:4; wash the grafted masterbatch with deionized water and acetone, and then dry it at 45°C for 2 hours, add it to the prepared copper sulfate aqueous solution with a molar concentration of 0.09 mol / L, the mass ratio of the mixed masterbatch to the metal salt solution is 1:10, stir and react at 30°C at 60 rpm for 2 hours, take out the solid, wash it with deionized water 3 times, and dry it at 45°C for 2 hours to obtain a mixed filler;

[0041] (3) dissolving polyvinyl alcohol in water to prepare a uniform solution with a mass concentration of 30%; stirring 24 parts of polytetrafluoroethylene, 20 parts of water, 12 parts of ammonium perfluorooctanoate and 10 parts of persulfate at 60°C at 200 rpm for 2 hours to form a polytetrafluoroethylene emulsion; then adding the polytetrafluoroethylene emulsion to the uniform solution at 60 rpm, with a dry weight ratio of polyvinyl alcohol to polytetrafluoroethylene of 1:20; then adding 8 parts of mixed filler, stirring at 40°C at 200 rpm for 4 hours to obtain a spinning solution, spinning the spinning solution using a screw extruder, cooling, and stretching to obtain polytetrafluoroethylene fiber, wherein the cooling temperature is 18°C, the melting temperature in the screw extruder is 270°C, the stretching rate is 4 times, and the fiber diameter is 80 μm;

[0042] (4) The polytetrafluoroethylene fiber is placed in a high-temperature furnace and sintered under the condition of continuous flow of nitrogen atmosphere; the sintering adopts program temperature control and segmented continuous sintering, keeping the temperature at 120°C for 120 minutes, heating from 120°C to 300°C at a rate of 10°C / min, and keeping the temperature at 300°C for 120 minutes; heating from 300°C to 410°C at a rate of 8°C / min, and keeping the temperature at 410°C for 120 minutes; after cooling to room temperature, the modified polytetrafluoroethylene fiber is woven into a 150 g / cm 2 fabric.

[0043] Comparative Example 1

[0044] The difference between Comparative Example 1 and Example 2 is that there is no step (1), and step (2) is changed to: maleic anhydride is added to NN dimethylformamide, mixed and stirred to dissolve, nano copper powder is added thereto, and heated to react at a temperature of 98°C for 3h, wherein the weight ratio of nano copper powder, maleic anhydride and NN dimethylformamide is 1:3:4; the grafted masterbatch is washed with deionized water and acetone, and then dried at a temperature of 45°C for 2h to obtain a mixed filler; the remaining steps are the same as those in Example 2.

[0045] Comparative Example 2

[0046] The difference between Comparative Example 2 and Example 2 lies in the difference in step (1), where step (1) is changed to: basalt ore and zirconium phosphate in a mass ratio of 100:3 are crushed and mixed to obtain mixed particles with an average particle size of 50 μm; the mixed particles are melted at 1400°C to form a spinning melt; the spinning melt is drawn and granulated to obtain a basalt masterbatch with a diameter of 20 μm; the basalt masterbatch is fumigated with ammonia at 50°C for 15 minutes; and a net ammonia space of 1.5 m is filled. 3 Under the conditions, the ammonia flow rate is 400L / min; after the ammonia fumigation is completed, it is immersed in a 0.3% by mass hydrogen peroxide aqueous solution at 25°C for 40 minutes, the solid is taken, and dried at 60°C for 24 hours to obtain a mixed masterbatch; the remaining steps are the same as in Example 2.

[0047] Comparative Example 3

[0048] The difference between Comparative Example 3 and Example 2 lies in the difference in step (1), where step (1) is modified as follows: basalt ore and zirconium phosphate in a mass ratio of 100:3 are crushed and mixed to obtain mixed particles with an average particle size of 50 μm; the mixed particles are melted at 1400° C. to form a spinning melt; the spinning melt is drawn and granulated to obtain a basalt masterbatch with a diameter of 20 μm; the basalt masterbatch is immersed in an aqueous solution containing 3 wt % of ammonium phosphate for 1 hour, taken out and dried at room temperature for 2 hours to obtain an activated basalt masterbatch; the activated basalt masterbatch is immersed in an aqueous solution of hydrogen peroxide with a mass fraction of 0.3% for 40 minutes, the solid is taken, and dried at 60° C. for 24 hours to obtain a mixed masterbatch; the remaining steps are the same as those in Example 2.

[0049] Comparative Example 4

[0050] The difference between Comparative Example 4 and Example 2 lies in the difference in step (1), where step (1) is modified as follows: basalt ore and zirconium phosphate in a mass ratio of 100:3 are crushed and mixed to obtain mixed particles with an average particle size of 50 μm; the mixed particles are melted at 1400° C. to form a spinning melt; the spinning melt is drawn and granulated to obtain a basalt masterbatch with a diameter of 20 μm; the basalt masterbatch is immersed in an aqueous solution containing 3 wt % of ammonium phosphate for 1 hour, taken out and dried at room temperature for 2 hours to obtain an activated basalt masterbatch; the activated basalt masterbatch is fumigated with ammonia at 50° C. for 15 minutes; and a net ammonia space of 1.5 m 3 Under the conditions, the ammonia flow rate is 400 L / min, and a mixed masterbatch is obtained; the remaining steps are the same as those in Example 2.

[0051] Comparative Example 5

[0052] The difference between Comparative Example 5 and Example 2 is that step (2) is different. Step (2) is changed to: add maleic anhydride to NN dimethylformamide, mix and stir to dissolve, add the mixed masterbatch thereto, and heat to react at 98°C for 3h, wherein the weight ratio of the mixed masterbatch, maleic anhydride and NN dimethylformamide is 1:3:4; wash the grafted masterbatch with deionized water and acetone, and then dry it at 45°C for 2h to obtain a mixed filler; the remaining steps are the same as Example 2.

[0053] Comparative Example 6

[0054] The difference between Comparative Example 6 and Example 2 is that step (4) is different. Step (4) is changed to: weave polytetrafluoroethylene fiber into a 150 g / cm 2 The remaining steps are the same as in Example 2.

[0055] Effect example

[0056] Table 1 below shows the performance analysis results of a waterproof and flame-retardant fabric using Examples 1 to 3 of the present invention and Comparative Examples 1 to 6.

[0057] Table 1

[0058]

[0059] From the comparison of the flame retardancy experimental data of the embodiment and the comparative example, it can be found that the present invention prepares a mixed masterbatch by melt drawing and granulation of basalt and zirconium phosphate, and then immerses the mixed basalt mixed masterbatch in an ammonium phosphate solution for pretreatment; zirconium phosphate is mixed in the masterbatch to improve the crystal structure of basalt and thus improve the mechanical structure of the basalt mixed masterbatch, and the micron-level masterbatch is immersed in ammonium phosphate, and the phosphate ions increase the surface roughness of the masterbatch while improving its surface activity, thereby improving the bonding strength of the masterbatch in the polymer fiber and chemically bonding it with the free groups in polytetrafluoroethylene; then the mixed masterbatch is fumigated and oxidized with ammonia, and intermittent processing is used to infiltrate ammonia into the interior of the masterbatch, so that ammonia and phosphate ions are cross-linked inside the fiber, and a high-efficiency flame retardant with phosphorus-nitrogen synergistic flame retardant effect with a significantly increased volume formed inside the fiber that cannot be washed out or is difficult to wash out, and the flame retardant performance is made more stable after oxidation, thereby obtaining a lasting flame retardant performance. The present invention then grafts nano-metal copper with mixed masterbatch and maleic anhydride to prepare mixed filler modified polytetrafluoroethylene fiber, and grafts metal ions with carboxyl groups to load metal ions on the surface of the fiber, thereby improving the flame retardant performance of the polytetrafluoroethylene fiber. From the comparison of the experimental data of the waterproofness of the embodiment and the comparative example, it can be found that the present invention forms a super-hydrophobic rough structure with micron-level mixed masterbatch and nano-level metal copper, so that the waterproof performance of the fiber is more optimized; after spinning, the program temperature is controlled and the segmented continuous sintering is adopted, and the polytetrafluoroethylene particles begin to re-orient and arrange, and then the carrier is decomposed at the right time, and the polytetrafluoroethylene fiber is further oriented and rearranged to form a beaded ultrafine fiber mesh structure, so that the woven fabric achieves a super-hydrophobic effect.

[0060] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A waterproof and flame-retardant fabric, It is characterized in that The fabric is prepared by preparing a mixed masterbatch from basalt, and braiding a mixed filler modified polytetrafluoroethylene fiber prepared by grafting nano-metal copper with maleic anhydride.

2. The waterproof and flame-retardant fabric according to claim 1, It is characterized in that The mixed masterbatch is prepared by mixing basalt and zirconium phosphate, melting and granulating the mixture, and then soaking and fumigating the mixture with ammonia.

3. The waterproof and flame-retardant fabric according to claim 1, It is characterized in that The modified polytetrafluoroethylene fiber is prepared by adopting program-controlled temperature and segmented continuous sintering during the spinning process to form a beaded ultrafine fiber mesh structure.

4. A method for preparing a waterproof and flame-retardant fabric, It is characterized in that The method comprises the following preparation steps: (1) Crush and mix basalt ore and zirconium phosphate in a mass ratio of 100:1-5 to obtain mixed particles with an average particle size of 50 μm; melt the mixed particles at 1400°C to form a spinning melt; draw the spinning melt and granulate it to obtain a basalt masterbatch with a diameter of 20 μm; immerse the basalt masterbatch in an aqueous solution containing 3wt% ammonium phosphate for 1 hour, take it out and dry it at room temperature for 2 hours to obtain an activated basalt masterbatch; fumigate the activated basalt masterbatch with ammonia at 30-70°C for 10-20 minutes; and immerse the activated basalt masterbatch in a clean ammonia-filled space of 1.0-2.0m 3 Under the conditions, the ammonia flow rate is 200-600L / min; after the ammonia fumigation is completed, it is immersed in the oxidation solution at 25°C for 20-60min, and the solid is taken and dried at 60°C for 24h to obtain the mixed masterbatch; (2) Add maleic anhydride to NN dimethylformamide, stir and mix to dissolve, add the mixed masterbatch, and heat to react at 98°C for 3 hours, wherein the weight ratio of the mixed masterbatch, maleic anhydride and NN dimethylformamide is 1:3:4; wash the grafted masterbatch with deionized water and acetone, and then dry it at 45°C for 2 hours, add it to the prepared metal salt solution, the mass ratio of the mixed masterbatch to the metal salt solution is 1:10, stir and react at 30°C at 60 rpm for 2 hours, take out the solid, wash it with deionized water 3 times, and dry it at 45°C for 2 hours to obtain a mixed filler; (3) dissolving polyvinyl alcohol in water to prepare a uniform solution with a mass concentration of 30%; stirring 20-24 parts of polytetrafluoroethylene, 10-20 parts of water, 10-12 parts of emulsifier and 8-10 parts of initiator at 60° C. and 200 rpm for 2 hours to form a polytetrafluoroethylene emulsion; then adding the polytetrafluoroethylene emulsion to the uniform solution with stirring at 60 rpm, and then adding 4-8 parts of mixed filler, stirring at 40° C. and 200 rpm for 2-4 hours to obtain a spinning solution, spinning the spinning solution using a screw extruder, cooling, and stretching to obtain polytetrafluoroethylene fiber, wherein the cooling temperature is 16-18° C., the melting temperature in the screw extruder is 250° C.-270° C., and the stretching rate is 2-4 times; (4) placing the polytetrafluoroethylene fiber in a high temperature furnace and sintering it under the condition of continuous flow of atmosphere; the sintering adopts program temperature control and continuous sintering, keeping the temperature at 90℃-120℃ for 30-120min, heating from 90℃-120℃ to 250℃-300℃ at a rate of 4-10℃ / min, and keeping the temperature at 250℃-300℃ for 30-120min; heating from 250℃-300℃ to 370℃-410℃ at a rate of 2-8℃ / min, and keeping the temperature at 370℃-410℃ for 20-120min; after cooling to room temperature, weaving the modified polytetrafluoroethylene fiber into a 150g / cm 2 fabric.

5. A method for preparing a waterproof and flame-retardant fabric according to claim 4, It is characterized in that The oxidizing liquid in step (1) is a hydrogen peroxide aqueous solution with a mass fraction of 0.1-0.5%.

6. The method for preparing a waterproof and flame-retardant fabric according to claim 4, It is characterized in that The metal salt solution in step (2) is a copper sulfate aqueous solution with a molar concentration of 0.09 mol / L.

7. The method for preparing a waterproof and flame-retardant fabric according to claim 4, It is characterized in that In the step (3), the emulsifier is ammonium perfluorooctanoate and the initiator is persulfate.

8. The method for preparing a waterproof and flame-retardant fabric according to claim 4, It is characterized in that In the step (3), the dry weight ratio of polyvinyl alcohol to polytetrafluoroethylene is 1:1-20.

9. The method for preparing a waterproof and flame-retardant fabric according to claim 4, It is characterized in that The diameter of the polytetrafluoroethylene fiber spun in the step (3) is 50-80 μm.

10. The method for preparing a waterproof and flame-retardant fabric according to claim 4, It is characterized in that The flowing atmosphere in step (4) is nitrogen.