Post-rolling expansion amount simulation method for 65Mn steel flat roll defect regulation and control

Through the analysis of CCT curve and cooling expansion curve, the cooling process of 65Mn steel was simulated, the expansion change under the action of phase change and cooling rate was determined, the problem of defects of 65Mn steel flat coils was solved, the effective control of flat coils was realized, and the reduction of Defects are prevented from occurring, and the method is simple and low-cost.

CN118731089AActive Publication Date: 2024-10-01NORTH CHINA UNIVERSITY OF SCIENCE AND TECHNOLOGY +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410715617.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-01
Estimated Expiration
2044-06-04

AI Technical Summary

Technical Problem

Quality defects often occur in 65Mn steel flat coils after hot rolling and coiling, resulting in the inability to carry out subsequent uncoiling and cold rolling annealing processes. The main factors include uneven distribution of residual stress inside the steel coil, improper tension adjustment during coiling, and uneven phase transformation. Due to its insufficient stiffness, it is difficult for the existing technology to effectively control the expansion caused by the combined effect of phase change and cooling rate.

Method used

The CCT curve and cooling expansion curve were used to analyze the expansion changes of 65Mn steel in different cooling speed ranges after coiling. The cooling process was simulated by the Gleeble-3500 thermal simulation testing machine, combined with microstructure observation and Vickers hardness testing, to determine the phase transformation and The expansion amount changes under the combined effect of cooling speed, and the appropriate cooling speed is selected to control flat roll defects.

Benefits of technology

The relationship between phase transformation categories and proportions and expansion changes under different cooling rates was successfully determined, and a method for regulating 65Mn steel flat coils was provided to reduce the occurrence of flat coil defects. The test method is simple and low-cost, providing improvement New ideas for flat roll quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118731089A_ABST
    Figure CN118731089A_ABST
Patent Text Reader

Abstract

The invention provides an after-rolling expansion amount simulation method for 65Mn steel flat roll defect regulation and control, which comprises the following steps: cutting 65Mn test steel into a cylinder sample with the diameter phi of 6 * 100mm, and carrying out cooling simulation on the cylinder sample at different cooling speeds; carrying out microscopic structure observation and Vickers hardness detection on the cooled and simulated cylindrical sample, and combining the expansion curve of the cylindrical sample to obtain a CCT curve; according to the CCT curve, the cooling speed range meeting the condition is selected, the cooling expansion curve of the selected cooling speed range is analyzed, and the expansion amount change caused by the independent action of the phase change and the expansion amount change caused by the comprehensive action of the cooling speed in the phase change process are counted, so that the problem of 65 Mn steel flat rolling is solved. According to the method, the CCT curve and the cooling expansion curve are used for analyzing main factors influencing the change of the expansion amount within different cooling speed ranges after the 65Mn steel is coiled, and then the flat coil defect is regulated and controlled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal material plastic processing, and in particular to a method for simulating post-rolling expansion for defect control of a 65Mn steel flat coil. Background Art

[0002] 65Mn high-strength tool steel is widely used in various fields because of its excellent mechanical properties and low price. However, in actual production, flat coil quality defects often occur after hot rolling, which makes it impossible to unwind the hot rolled coil and affects the cold rolling annealing process. The occurrence of flat coils is related to many factors, mainly including uneven residual stress distribution inside the steel coil, inappropriate tension adjustment during coiling, uneven phase change, insufficient self-rigidity, etc. In order to reduce the occurrence of flat coil defects, it can be solved by increasing the strength of the strip, adjusting the coiling tension, and controlling the residence time after coiling. These adjustment methods are mainly based on the fundamental cause of flat coils, that is, after the strip is coiled, a large volume expansion occurs due to phase change, resulting in sliding between layers and loose coiling.

[0003] In addition, in actual cooling, due to the thermal expansion and contraction of steel, volume shrinkage will occur. When the volume shrinkage force cannot resist the phase change expansion force, the strip will have flat coil defects under its own gravity. Therefore, it is very important to study the expansion of the strip under the combined effect of phase change and cooling for the regulation of phase change and cooling rate after coiling, and then inhibit the occurrence of flat coils. The generation of flat coils is mainly affected by the expansion amount under the dual effects of phase change and cooling rate. The former is the factor that causes flat coils, and the latter is the reason for inhibiting the generation of flat coils. In the cooling stage after coiling, due to the different specific volumes of various tissues produced by phase change, the steel coil will produce a large volume expansion with the increase of cooling rate. At the same time, during the cooling process, due to the thermal expansion and contraction characteristics of steel, the faster the cooling rate, the greater the temperature change, and the greater the shrinkage produced in the same time. Finally, under the interaction of two forces with the same trend and opposite action, it is determined whether flat coils occur.

[0004] Therefore, it is necessary to study the changing laws of the expansion and contraction produced at different cooling rates during the cooling process after the strip is coiled, and to determine the dominant relationship between the interaction of the expansion caused by phase change and the contraction caused by cooling on the final volume expansion change of the steel coil at different cooling stages. Summary of the invention

[0005] In order to overcome the shortcomings of the prior art, the purpose of the present invention is to provide a post-coiling expansion simulation method for 65Mn steel flat coil defect control, and use CCT curve and cooling expansion curve to analyze the main factors affecting the expansion change within different cooling rate ranges of 65Mn steel after coiling, thereby realizing the control of flat coil defects.

[0006] To achieve the above object, the present invention provides the following scheme: a method for simulating the post-rolling expansion for defect control of 65Mn steel flat coil, comprising the following steps:

[0007] The 65Mn test steel was cut into cylindrical specimens of φ6×100 mm, and cooling simulations were performed on the cylindrical specimens at different cooling rates;

[0008] Conducting microstructural observation and Vickers hardness testing on the cylindrical specimen after cooling simulation, and obtaining a CCT curve in combination with the expansion curve of the cylindrical specimen;

[0009] According to the CCT curve, a cooling rate range that meets the conditions is selected, and the cooling expansion curve of the selected cooling rate range is analyzed. The expansion changes caused by the phase transformation alone and the expansion changes caused by the combined effect of the cooling rate during the phase transformation process are statistically calculated to solve the 65Mn steel flat coil problem.

[0010] Optionally, the mass percentages of the cylindrical sample are: C: 0.66%, Si: 0.21%, Mn: 0.98%, P: 0.014%, S: 0.007%, Ni: 0.021%, Cr: 0.04%, Cu: 0.021%, and the remainder is Fe.

[0011] Optionally, the cooling simulation process of the cylindrical specimen is:

[0012] Using a Gleeble-3500 thermal simulation tester, the cylindrical sample is heated to the austenitizing temperature at a heating rate of 10°C / s, the heating expansion curve is detected and the critical transition points Ac1 and Ac3 are determined, and the cylindrical sample is kept warm for 5 minutes after the heating is completed to completely austenitize the cylindrical sample, and then the completely austenitized cylindrical sample is cooled to room temperature at cooling rates of 0.5°C / s, 2°C / s, 5°C / s, 10°C / s, 15°C / s, 20°C / s, 30°C / s, and 50°C / s, respectively, to complete the cooling simulation process and obtain the cooling expansion curve;

[0013] The austenitizing temperature is 950° C., and argon gas is introduced into the Gleeble-3500 thermal simulation test machine as a protective atmosphere during the experiment.

[0014] Optionally, the process of obtaining the CCT curve is:

[0015] Cut the middle part of the cylindrical sample after the cooling simulation to obtain a thermocouple welding section, measure the Vickers hardness at multiple positions on both sides of the cut part of the thermocouple welding section and take an average value, then use the tangent method to measure the critical transition point and phase transition point of the heating expansion curve and the cooling expansion curve respectively, and draw the CCT curve by combining the average value of the Vickers hardness, the critical transition point and the phase transition point;

[0016] The abscissa time of the CCT curve starts from when the cylindrical sample is cooled after being kept warm for 5 minutes.

[0017] Optionally, it is characterized in that a cooling rate range that meets the conditions is selected according to the CCT curve, and the cooling expansion curve of the selected cooling rate range is analyzed, and the expansion change caused by the phase change alone and the expansion change caused by the combined effect of the cooling rate during the phase transformation process are statistically calculated, so as to solve the problem of 65Mn steel flat coils as follows:

[0018] According to the optimal structure of 65Mn steel, a cooling rate that meets the conditions is selected on the CCT curve, and the proeutectoid ferrite content of the optimal structure is measured; wherein the optimal structure includes proeutectoid ferrite and pearlite structure, and the cooling rates that meet the conditions are selected to include 0.5°C / s, 2°C / s, 5°C / s and 10°C / s;

[0019] The expansion curve and the degree of change of expansion amount under the cooling rates of 0.5℃ / s, 2℃ / s, 5℃ / s and 10℃ / s due to the phase change alone and the combined effect of cooling rate are determined, and the main factors affecting the expansion amount in each cooling range are compared. Based on the main factors, the problem of 65Mn steel flat coil is solved; among them, each cooling range includes 0.5~2℃ / s, 2~5℃ / s and 5~10℃ / s.

[0020] The present invention discloses the following technical effects by providing a method for simulating the post-rolling expansion for defect control of 65Mn steel flat coils:

[0021] 1. The present invention can determine the relationship between the difference in the content of phase types and their respective proportions caused by 65Mn steel at different cooling rates and the change in expansion caused by the phase transformation alone.

[0022] 2. In the actual cooling process, the phase change and the expansion caused by the comprehensive cooling effect at different cooling rates are different. The present invention provides the expansion change law caused by different cooling rates and the main influencing factors of each cooling stage.

[0023] 3. The present invention determines the corresponding cooling rate range according to the actual cooling rate when phase change occurs and each cooling rate stage in the cooling process, and regulates the main factors causing the expansion within the range, thereby effectively controlling the occurrence of 65Mn steel flat coils.

[0024] 4. The testing method of the present invention is simple, low-cost, and provides a new idea for effectively improving the defects of 65Mn steel flat coils.

[0025] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0027] Figure 1 A flow chart of a method provided by an embodiment of the present invention;

[0028] Figure 2 A schematic diagram of a CCT curve of 65Mn steel provided in an embodiment of the present invention;

[0029] Figure 3 A schematic diagram of a detailed explanation of the CCT curve of 65Mn steel provided in an embodiment of the present invention;

[0030] Figure 4 The percentage of proeutectoid ferrite content that meets the cooling rate requirements provided by the embodiment of the present invention;

[0031] Figure 5 A schematic diagram of the expansion amount change of the cooling expansion curve provided in an embodiment of the present invention;

[0032] Figure 6 A schematic diagram of an expansion curve under the action of phase change alone provided in an embodiment of the present invention;

[0033] Figure 7 A schematic diagram of the change in expansion amount under the action of phase change alone provided by an embodiment of the present invention;

[0034] Figure 8 A schematic diagram of an expansion curve under a comprehensive effect provided by an embodiment of the present invention;

[0035] Fig. 9 A schematic diagram of the change in expansion amount under the combined effects provided by an embodiment of the present invention. DETAILED DESCRIPTION

[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0038] like Figure 1-9As shown, the present invention provides a method for simulating the post-rolling expansion for defect control of 65Mn steel flat coils, which realizes effective control of defects of 65Mn steel flat coils, including the following steps:

[0039] 1. Cut the 65Mn test steel into cylindrical specimens of φ6×100mm, and perform cooling simulations at different cooling rates on the cylindrical specimens. Specifically:

[0040] The mass percentages of the cylindrical sample are: C: 0.66, Si: 0.21, Mn: 0.98, P: 0.014, S: 0.007, Ni: 0.021, Cr: 0.04, Cu: 0.021, and the remaining amount is Fe (mass percentage, %).

[0041] like Figure 1-3 As shown in the figure, the cooling simulation process of the cylindrical sample is as follows: using a Gleeble-3500 thermal simulation testing machine, the cylindrical sample is heated to the austenitizing temperature at a heating rate of 10°C / s, the heating expansion curve is detected and the critical transition points Ac1 and Ac3 are determined, and the heating is maintained for 5 minutes after the heating is completed to make the cylindrical sample completely austenitized, and then the completely austenitized cylindrical sample is cooled to room temperature at cooling rates of 0.5°C / s, 2°C / s, 5°C / s, 10°C / s, 15°C / s, 20°C / s, 30°C / s, and 50°C / s, respectively, to complete the cooling simulation process and obtain the cooling expansion curve.

[0042] The austenitizing temperature is 950° C., and argon gas is introduced into the Gleeble-3500 thermal simulation test machine as a protective atmosphere during the experiment.

[0043] 2. Perform microstructure observation and Vickers hardness test on the cylindrical sample after cooling simulation, and obtain the CCT curve in combination with the expansion curve of the cylindrical sample. Specifically:

[0044] like Figure 1-3 As shown in the figure, the middle part of the cylindrical specimen after the cooling simulation is cut to obtain a thermocouple welding section, the Vickers hardness of multiple positions on both sides of the cut of the thermocouple welding section is measured and the average value is taken, and then the critical transition point (Ac1, Ac3) and the phase transition point (Ms) of the 10°C / s heating expansion curve and the 50°C / s cooling expansion curve are measured by the tangent method, and the CCT curve is plotted in combination with the average Vickers hardness, the critical transition point and the phase transition point.

[0045] The abscissa time of the CCT curve starts from the time when the cylindrical sample is cooled after being kept warm for 5 minutes.

[0046] 3. According to the CCT curve, a cooling rate range that meets the conditions is selected, and the cooling expansion curve of the selected cooling rate range is analyzed to calculate the expansion changes caused by the phase change alone and the expansion changes caused by the combined effect of the cooling rate during the phase transformation process, so as to solve the 65Mn steel flat coil problem. Specifically:

[0047] According to the optimal structure of 65Mn steel, a cooling rate that meets the conditions is selected on the CCT curve, and the proeutectoid ferrite content of the optimal structure is measured to obtain the proeutectoid ferrite content percentage (such as Figure 4 As shown); wherein, the optimal structure includes proeutectoid ferrite and pearlite structure, and the cooling rates that meet the conditions are selected to include 0.5°C / s, 2°C / s, 5°C / s and 10°C / s;

[0048] like Figure 5 As shown, since the change in expansion during the cooling process is affected by the combined effects of phase change and cooling, the change in expansion caused by phase change alone and the change in expansion caused by the combined effects of the two are determined and experimentally analyzed.

[0049] like Figure 6-9 As shown, the present invention determines the expansion curve and the degree of change of expansion under the single effect of phase change and the combined effect of cooling rate at cooling rates of 0.5℃ / s, 2℃ / s, 5℃ / s and 10℃ / s, compares the main factors affecting the expansion in each cooling range, and solves the problem of 65Mn steel flat coil based on the main factors; wherein, each cooling range and its influencing factors include: at a small cooling rate of 0.5-2℃ / s, the shrinkage caused by cooling is dominant; when the cooling rate is increased to the range of 2-5℃ / s, the expansion caused by phase change plays a major role; when the cooling rate reaches 5-10℃ / s, the shrinkage caused by cooling is dominant. Therefore, in order to effectively solve the problem of flat coils, adjustments should be made to its dominant factors within different cooling rate ranges after coiling.

[0050] Therefore, the present invention provides a post-coiling expansion simulation method for controlling defects of 65Mn steel flat coils, and uses CCT curves and cooling expansion curves to analyze the main factors affecting the change in expansion within different cooling rate ranges after 65Mn steel coiling, thereby achieving control of flat coil defects.

[0051] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.

[0052] The principles and implementation methods of the present invention are described in this article using specific examples. The description of the above embodiments is only used to help understand the method and core idea of ​​the present invention. At the same time, for those skilled in the art, according to the idea of ​​the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A method for simulating the post-rolling expansion for defect control of 65Mn steel flat coils, characterized in that: The following steps are involved: The 65Mn test steel was cut into cylindrical specimens of φ6×100 mm, and cooling simulations were performed on the cylindrical specimens at different cooling rates; Conducting microstructural observation and Vickers hardness testing on the cylindrical specimen after cooling simulation, and obtaining a CCT curve in combination with the expansion curve of the cylindrical specimen; According to the CCT curve, a cooling rate range that meets the conditions is selected, and the cooling expansion curve of the selected cooling rate range is analyzed. The expansion changes caused by the phase transformation alone and the expansion changes caused by the combined effect of the cooling rate during the phase transformation process are statistically calculated to solve the 65Mn steel flat coil problem.

2. The method for simulating the post-coiling expansion for defect control of 65Mn steel flat coil according to claim 1, characterized in that: The mass percentages of the cylindrical sample are: C: 0.66%, Si: 0.21%, Mn: 0.98%, P: 0.014%, S: 0.007%, Ni: 0.021%, Cr: 0.04%, Cu: 0.021%, and the remainder is Fe.

3. The method for simulating the post-coiling expansion for defect control of 65Mn steel flat coil according to claim 2, characterized in that: The cooling simulation process of the cylindrical specimen is as follows: Using a Gleeble-3500 thermal simulation tester, the cylindrical sample is heated to the austenitizing temperature at a heating rate of 10°C / s, the heating expansion curve is detected and the critical transition points Ac1 and Ac3 are determined, and the cylindrical sample is kept warm for 5 minutes after the heating is completed to completely austenitize the cylindrical sample, and then the completely austenitized cylindrical sample is cooled to room temperature at cooling rates of 0.5°C / s, 2°C / s, 5°C / s, 10°C / s, 15°C / s, 20°C / s, 30°C / s, and 50°C / s, respectively, to complete the cooling simulation process and obtain the cooling expansion curve; The austenitizing temperature is 950° C., and argon gas is introduced into the Gleeble-3500 thermal simulation test machine as a protective atmosphere during the experiment.

4. The method for simulating the post-coiling expansion for defect control of 65Mn steel flat coil according to claim 3, characterized in that: The process of obtaining the CCT curve is: Cut the middle part of the cylindrical sample after the cooling simulation to obtain a thermocouple welding section, measure the Vickers hardness at multiple positions on both sides of the cut part of the thermocouple welding section and take an average value, then use the tangent method to measure the critical transition point and phase transition point of the heating expansion curve and the cooling expansion curve respectively, and draw the CCT curve by combining the average value of the Vickers hardness, the critical transition point and the phase transition point; The abscissa time of the CCT curve starts from when the cylindrical sample is cooled after being kept warm for 5 minutes.

5. The method for simulating the post-coiling expansion for defect control of 65Mn steel flat coil according to claim 4, characterized in that: According to the CCT curve, a cooling rate range that meets the conditions is selected, and the cooling expansion curve of the selected cooling rate range is analyzed. The expansion changes caused by the phase transformation alone and the expansion changes caused by the combined effect of the cooling rate during the phase transformation process are statistically calculated to solve the 65Mn steel flat coil problem as follows: According to the optimal structure of 65Mn steel, a cooling rate that meets the conditions is selected on the CCT curve, and the proeutectoid ferrite content of the optimal structure is measured; wherein the optimal structure includes proeutectoid ferrite and pearlite structure, and the cooling rates that meet the conditions are selected to include 0.5°C / s, 2°C / s, 5°C / s and 10°C / s; The expansion curve and the degree of change of expansion amount under the cooling rates of 0.5℃ / s, 2℃ / s, 5℃ / s and 10℃ / s due to the phase change alone and the combined effect of cooling rate are determined, and the main factors affecting the expansion amount in each cooling range are compared. Based on the main factors, the problem of 65Mn steel flat coil is solved; among them, each cooling range includes 0.5~2℃ / s, 2~5℃ / s and 5~10℃ / s.

Citation Information

Patent Citations

  • Coiling shape control method for medium-high carbon steel with omega (C) larger than or equal to 0.45%

    CN113441549A

  • Control method for eliminating flat coils of hot-rolled high-strength strip steel

    CN113458152A

  • Flexible production method of thin 65Mn steel

    CN115647075A