Optical device and manufacturing method thereof

By forming and rounding the dielectric layer on the base structure of the optical device, the microlenses are manufactured directly in the chip factory, which solves the problems of long production cycle and poor microlens density and improves optical efficiency.

CN118732098APending Publication Date: 2024-10-01WUHAN XINXIN SEMICON MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410764820.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The production cycle of existing optical devices is long and the density and uniformity of microlenses are poor, resulting in low optical efficiency and difficulty in meeting the requirements of high-performance equipment.

Method used

The first dielectric layer is formed on the base structure, and the opening is formed by removing the part through patterning, dividing the sub-dielectric layer, and rounding the sub-dielectric layer to form the micro-lens. This enables simultaneous manufacturing of micro-lenses in the chip factory and avoids the need for specialized micro-lenses. Factory transfer.

Benefits of technology

The production cycle is shortened, the density and uniformity of the microlenses are improved, and the optical efficiency of the optical device is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118732098A_ABST
    Figure CN118732098A_ABST
Patent Text Reader

Abstract

The invention provides an optical device and a manufacturing method thereof, and the method comprises the steps: forming a first dielectric layer on a substrate structure, removing a part of the first dielectric layer through patterning to form an opening in the first dielectric layer, dividing the first dielectric layer into at least one first sub-dielectric layer through the opening, and the first sub-dielectric layer is rounded to form the micro-lens, so that the micro-lens can be simultaneously manufactured in a chip factory and does not need to be additionally transferred to a special micro-lens factory, the production efficiency can be improved, and the production period can be shortened. Correspondingly, the formed optical device is provided with the micro-lens formed through the semiconductor technology, the compactness and the uniformity of the micro-lens are higher, and therefore higher optical efficiency can be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to an optical device and a manufacturing method thereof. Background Art

[0002] At present, the manufacturing of optical devices (CIS / SPAD, etc.) usually completes the chip manufacturing in the chip factory first, and then sends it to a special microlens factory to make microlenses (ML). Due to the time required for transportation and other turnover, the production cycle of optical devices is relatively long. In addition, the microlenses manufactured by existing processes have poor density and uniformity, and low optical efficiency, which makes it difficult to meet the requirements of high-performance equipment. Summary of the invention

[0003] The object of the present invention is to provide an optical device and a method for manufacturing the same, so as to solve the problems of long production cycle and / or poor density and uniformity of manufactured microlenses and low optical efficiency in existing processes.

[0004] In order to solve the above technical problems, the present invention provides a method for manufacturing an optical device, the method for manufacturing an optical device comprising:

[0005] Providing a base structure;

[0006] forming a first dielectric layer on the base structure; and,

[0007] Part of the first dielectric layer is patterned and removed to form an opening in the first dielectric layer, wherein the opening divides the first dielectric layer into at least one first sub-dielectric layer, and the first sub-dielectric layer is rounded to form a microlens.

[0008] Optionally, in the method for manufacturing the optical device, rounding the first sub-dielectric layer includes:

[0009] A patterned mask layer is formed on the first sub-dielectric layer, and the connection between the surface and the side surface of the first sub-dielectric layer is etched using the patterned mask layer as a mask to form a curved surface.

[0010] Optionally, in the method for manufacturing the optical device, the patterned mask layer exposes an edge surface of the first sub-dielectric layer; and etching a connection between the surface and the side of the first sub-dielectric layer comprises:

[0011] The exposed edge surface of the first sub-dielectric layer is etched.

[0012] Optionally, in the method for manufacturing the optical device, the method for forming the patterned mask layer includes:

[0013] forming a first mask layer on the first dielectric layer;

[0014] Patterning the first mask layer to form a first basic pattern mask layer, and using the first basic pattern mask layer as a mask, etching a portion of the thickness of the first dielectric layer to form the opening;

[0015] The first basic pattern mask layer is constricted to form the patterned mask layer.

[0016] Optionally, in the method for manufacturing the optical device, after etching the connection between the surface and the side of the first sub-dielectric layer, rounding the first sub-dielectric layer further comprises:

[0017] Repeat one or more times: shrink the patterned mask layer to expose the edge surface of the first sub-dielectric layer, and etch the exposed edge surface of the first sub-dielectric layer using the shrunken patterned mask layer as a mask.

[0018] Optionally, in the method for manufacturing the optical device, the patterned mask layer covers the edge surface of the first sub-dielectric layer; and etching the connection between the surface and the side of the first sub-dielectric layer comprises:

[0019] The first sub-dielectric layer is etched. At an edge position of the patterned mask layer, an etching selectivity ratio between the first sub-dielectric layer and the patterned mask layer is less than X:1; at a middle position of the patterned mask layer, an etching selectivity ratio between the first sub-dielectric layer and the patterned mask layer is greater than X:1.

[0020] Optionally, in the method for manufacturing the optical device, forming the patterned mask layer includes:

[0021] forming a second dielectric layer and a second mask layer in sequence on the first dielectric layer;

[0022] The second mask layer is patterned to form a second basic graphic mask layer, and the second dielectric layer is etched using the second basic graphic mask layer as a mask to obtain the graphic mask layer, and a portion of the thickness of the first dielectric layer is etched to form the opening.

[0023] Optionally, in the method for manufacturing the optical device, rounding the first sub-dielectric layer includes:

[0024] A third dielectric layer is formed, wherein the third dielectric layer at least covers the side surface of the first sub-dielectric layer so that a connection between the surface and the side surface of the first sub-dielectric layer forms a curved surface.

[0025] Optionally, in the manufacturing method of the optical device, the first sub-medium layer includes at least two sub-layers, and the cross-sectional width of each sub-layer parallel to the surface of the base structure gradually increases from away from the base structure to close to the base structure;

[0026] Wherein, the third dielectric layer covers the side surfaces of each sub-layer.

[0027] Optionally, in the method for manufacturing the optical device, the opening divides the first dielectric layer into a second sub-dielectric layer, and the first sub-dielectric layer is located on the second sub-dielectric layer.

[0028] Optionally, in the method for manufacturing the optical device, while rounding the first sub-dielectric layer, the second sub-dielectric layer is also patterned and / or rounded.

[0029] The present invention also provides an optical device, comprising: a substrate structure; and a microlens located on the substrate structure, wherein the microlens is formed by patterning and rounding a first dielectric layer located on the substrate structure.

[0030] Optionally, in the optical device, the microlens is made of silicon oxide.

[0031] Optionally, in the optical device, the microlens is formed by using the manufacturing method of the optical device as described above.

[0032] In the optical device and the manufacturing method thereof provided by the present invention, a first dielectric layer is formed on a substrate structure, a portion of the first dielectric layer is removed by patterning to form an opening in the first dielectric layer, the opening divides the first dielectric layer into at least one first sub-dielectric layer, and the first sub-dielectric layer is rounded to form a microlens, whereby the microlens can be manufactured simultaneously in a chip factory without being transferred to a special microlens factory, thereby improving production efficiency and shortening production cycle. Accordingly, the formed optical device has a microlens formed by a semiconductor process, and the microlens has higher density and uniformity, thereby also obtaining higher optical efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figures 1 to 3 It is a cross-sectional schematic diagram of a device structure formed during the process of executing the method for manufacturing an optical device according to the first embodiment of the present invention.

[0034] Figures 4 to 9 It is a partial cross-sectional schematic diagram of a device structure formed in the process of forming a microlens according to the first embodiment of the present invention.

[0035] Figures 10 to 12 It is a cross-sectional schematic diagram of a device structure formed during the process of executing the method for manufacturing an optical device according to the second embodiment of the present invention.

[0036] Figures 13 to 16 It is a partial cross-sectional schematic diagram of a device structure formed in the process of forming a microlens according to the second embodiment of the present invention.

[0037] Figures 17 to 20 It is a cross-sectional schematic diagram of a device structure formed during the process of executing the method for manufacturing an optical device according to the third embodiment of the present invention.

[0038] The reference numerals are described as follows:

[0039] 10-optical device; 100-base structure; 101-logic wafer; 102-pixel wafer; 103-rewiring layer; 110-base dielectric layer; 120-first dielectric layer; 121-opening; 122-first sub-dielectric layer; 123-second sub-dielectric layer; 120A-edge surface; 120B-edge surface; 130-first basic graphic mask layer; 131, 132-graphic mask layers; 140-microlens; R1-radius of curvature.

[0040] 20-optical device; 200-base structure; 201-logic wafer; 202-pixel wafer; 203-rewiring layer; 210-base dielectric layer; 220-first dielectric layer; 221-opening; 222-first sub-dielectric layer; 223-second sub-dielectric layer; 230-second dielectric layer; 231-patterned mask layer; 231A-edge position; 231B-middle position; 240-second basic graphic mask layer; 250-microlens; R2-radius of curvature.

[0041] 30-optical device; 300-base structure; 301-logic wafer; 302-pixel wafer; 303-rewiring layer; 310-base dielectric layer; 320-first dielectric layer; 321-opening; 322-first sub-dielectric layer; 3220-sub-layer; 330-basic graphic mask layer; 340-third dielectric layer; 350-microlens; R3-radius of curvature.

[0042] Note that in the embodiments described below, sometimes the same reference numerals are used in common between different drawings to represent the same parts or parts with the same functions, and their repeated descriptions are omitted. In some cases, similar numbers and letters are used to represent similar items, so once an item is defined in one drawing, it does not need to be further discussed in subsequent drawings. DETAILED DESCRIPTION

[0043] The optical device and the manufacturing method thereof proposed by the present invention are further described in detail below in conjunction with the accompanying drawings and specific embodiments. The advantages and features of the present invention will become more apparent from the following description. It should be noted that the accompanying drawings are all in a very simplified form and are not in precise proportions, and are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention.

[0044] The terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. Unless otherwise defined in the present application document, the technical terms or scientific terms used in the present invention should be the common meaning understood by people with ordinary skills in the field to which the present invention belongs. The words "first", "second" and similar words used in the present specification and claims do not indicate any order, quantity or importance, but are only used to distinguish different components. Similarly, words such as "one" or "one" do not indicate a quantity limit, but indicate that there is at least one. "Multiple" or "several" means two or more. Unless otherwise specified, words such as "upper / upper layer", "lower / lower layer" and the like are only for the convenience of explanation and are not limited to one position or one spatial orientation. Words such as "include" or "comprise" and the like mean that the elements or objects appearing in front of "include" or "comprise" include the elements or objects listed after "include" or "comprise" and their equivalents, and do not exclude other elements or objects. Words such as "connect" or "connected" and the like are not limited to physical or mechanical connections, and can include electrical connections, whether direct or indirect. The singular forms "a", "said" and "the" used in the present specification and the appended claims are also intended to include the plural forms, unless the context clearly indicates otherwise. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more of the associated listed items.

[0045] [Example 1]

[0046] Please refer to Figures 1 to 3 , which is a cross-sectional schematic diagram of a device structure formed during the process of executing the method for manufacturing an optical device according to the first embodiment of the present invention. Figure 1 As shown, a substrate structure 100 is provided, wherein the substrate structure 100 includes: a first wafer 101, a second wafer 102 bonded to the first wafer 101, and a wiring layer 103 located on the second wafer 102, wherein the first wafer 101 is, for example, a logic wafer, and the second wafer 102 is, for example, a pixel wafer. In other embodiments of the present application, the substrate structure 100 may also be other structures, for example, the substrate structure 100 may also include a single wafer structure, the wafer structure includes a logic area, a pixel area, etc., the substrate structure 100 may also include a single or stacked chip, and the substrate structure 100 may also include wafers and chips bonded together; the material of the substrate structure 100 may include semiconductor materials, and may also include non-semiconductor materials, such as glass, ceramics, etc.

[0047] like Figure 2As shown, in the embodiment of the present application, then, a base dielectric layer 110 is formed on the base structure 100, and a first dielectric layer 120 is formed on the base dielectric layer 110. The base dielectric layer 110 can be used as an etching stop layer and can protect the base structure 100. In other embodiments of the present application, the first dielectric layer 120 can also be directly formed on the base structure 100. The base dielectric layer 110 and / or the first dielectric layer 120 are made of organic material or inorganic material. In the present embodiment, the base dielectric layer 110 is made of silicon nitride, which mainly serves as an etching stop layer; the first dielectric layer 120 is made of silicon oxide, which is used to form a microlens. The thickness of the base dielectric layer 110 is, for example, The thickness of the first dielectric layer 120 is, for example, The material and thickness of the base dielectric layer 110 and the first dielectric layer 120 are not limited to the above description, and may be other materials or thicknesses known in the art.

[0048] Please continue to refer to Figure 2 In the embodiment of the present application, a first mask layer (not shown) is then formed on the first dielectric layer 120; the first mask layer is patterned to form a first basic graphic mask layer 130. The first mask layer is any material known in the art, such as a hard mask layer, a photoresist, etc. In the embodiment of the present application, the first mask layer is a photoresist layer, and the first basic graphic mask layer 130 includes, for example, a plurality of photoresist blocks arranged in an array to form a microlens arranged in an array. The thickness of the first basic graphic mask layer 130 can be, for example, The thickness of the first basic pattern mask layer 130 may not be limited to the above range.

[0049] like Figure 3 As shown, in the embodiment of the present application, then, using the first basic graphic mask layer 130 as a mask, a portion of the first dielectric layer 120 is patterned and removed to form an opening 121 in the first dielectric layer 120, and the opening 121 divides the first dielectric layer 120 into at least one first sub-dielectric layer 122, and the first sub-dielectric layer 122 is rounded to form a microlens 140.

[0050] For details, please refer to Figures 4 to 9 , which is a partial cross-sectional schematic diagram of a device structure formed in the process of forming a microlens according to the first embodiment of the present invention. For the sake of clarity, Figures 4 to 9 Only a portion of the base dielectric layer 110 and a portion of the first dielectric layer 120 are shown.

[0051] like Figure 4As shown, here, the first basic pattern mask layer 130 is used as a mask to etch a portion of the first dielectric layer 120, for example, 1 / 20 to 1 / 3 of the thickness of the first dielectric layer 120. The etching thickness can be matched and regulated by the etchant and the etching time. Thus, the opening 121 is formed in the first dielectric layer 120, and a plurality of the first sub-dielectric layers 122 ( Figures 4 to 9 Only one of them is schematically shown in the figure). In the embodiment of the present application, a second sub-dielectric layer 123 is further divided, the first sub-dielectric layer 122 is located on the second sub-dielectric layer 123, the cross-sectional width of the first sub-dielectric layer 122 parallel to the surface of the substrate structure may be less than or equal to or greater than the cross-sectional width of the second sub-dielectric layer 123 parallel to the surface of the substrate structure, and a step may be formed between the first sub-dielectric layer 122 and the second sub-dielectric layer 123.

[0052] Please refer to Figure 2 , Figure 3 and Figure 4 , wherein the number of the divided second sub-dielectric layers 123 may be one or more. Specifically, the opening 121 may include a plurality of first sub-openings (not shown in the figure) extending along the first direction and a plurality of second sub-openings (not shown in the figure) extending along the second direction, wherein the first sub-openings and the second sub-openings intersect and communicate with each other on a surface parallel to the substrate structure 100, wherein the first direction and the second direction are both parallel to the surface of the substrate structure 100 and form an angle, and preferably, the first direction and the second direction are both parallel to the surface of the substrate structure 100 and perpendicular to each other. Thus, a plurality of the first sub-dielectric layers 120 may be divided through the opening 121, wherein the opening 121 may penetrate the first dielectric layer 120 or may not penetrate the first dielectric layer 120, thereby correspondingly dividing one or more second sub-dielectric layers 123.

[0053] Then, if Figure 5 As shown, the first basic pattern mask layer 130 is shrunk to form a patterned mask layer 131 on the first sub-dielectric layer 122. Here, after the shrinking process, the size of the patterned mask layer 131 in the width direction is reduced relative to the first basic pattern mask layer 130, and the size of the patterned mask layer 131 in the thickness direction can also be reduced at the same time, wherein, after the size in the width direction is reduced, the patterned mask layer 131 exposes the edge surface 120A of the first sub-dielectric layer 122.

[0054] Then, if Figure 6As shown, the patterned mask layer 131 is used as a mask to etch the connection between the surface and the side of the first sub-dielectric layer 122 to form a curved surface. Here, the edge surface of the exposed first sub-dielectric layer 122 is etched to round the first sub-dielectric layer 122.

[0055] Please continue to refer to Figure 6 In the embodiment of the present application, while the first sub-dielectric layer 122 is rounded, the second sub-dielectric layer 123 is also patterned. Figure 5 and Figure 6 Here, while the first sub-dielectric layer 122 is rounded by an etching process, the second sub-dielectric layer 123 is also patterned by the same etching process, thereby removing a portion of the thickness of the second sub-dielectric layer 123. By rounding the first sub-dielectric layer 122 and patterning the second sub-dielectric layer 123 at the same time, the thickness of the formed microlens can be adjusted.

[0056] Then, if Figure 7 As shown, the patterned mask layer 131 is shrunk to obtain the shrunk patterned mask layer 132. The shrunk patterned mask layer 132 is reduced in size relative to the patterned mask layer 131 in the width direction, that is, the size relative to the first basic patterned mask layer 130 in the width direction is further reduced, and the shrunk patterned mask layer 132 can also be reduced in thickness direction relative to the patterned mask layer 131 at the same time, that is, the size relative to the first basic patterned mask layer 130 in the thickness direction can also be further reduced, thereby, the shrunk patterned mask layer 132 exposes the edge surface 120B of the first sub-dielectric layer 122, that is, more of the first dielectric layer 120 is exposed.

[0057] like Figure 8As shown, then, the edge surface 120B of the exposed first sub-dielectric layer 122 is etched using the shrunk patterned mask layer 132 as a mask. In the embodiment of the present application, the remaining second sub-dielectric layer 123 can be patterned and / or rounded at the same time, and the etching stops at the surface of the base dielectric layer 110, thereby forming the microlens 140. In other embodiments of the present application, the etching process can stop in the second sub-dielectric layer 123, and the following process steps can be performed one or more times: the patterned mask layer 132 is shrunk to expose the edge surface of the first sub-dielectric layer 122; and the edge surface of the exposed first sub-dielectric layer 122 is etched using the shrunk patterned mask layer as a mask, and the second sub-dielectric layer 123 is also etched at the same time, and finally the etching stops at the surface of the base dielectric layer 110 to form the microlens 140. By performing multiple etching processes on the first dielectric layer 120, the morphology of the formed microlens 140 can be adjusted, for example, the curvature radius R1 of the microlens 140 can be adjusted, thereby improving the quality and reliability of the microlens 140. In the embodiment of the present application, the curvature radius R1 of the microlens 140 is between In other embodiments, the curvature radius R1 of the microlens 140 may be less than or greater than

[0058] In the embodiment of the present application, then, Fig. 9 As shown, the patterned mask layer 132 is removed to expose the microlens 140. For example, the patterned mask layer 132 may be removed by ashing or other processes.

[0059] Please continue to refer to Figure 3 Thus, an optical device 10 is obtained, and the optical device 10 includes: a substrate structure 100; and a microlens 140 located on the substrate structure 100, and the microlens 140 is formed by patterning and rounding the first dielectric layer 120 located on the substrate structure 100. In the embodiment of the present application, the optical device 10 also includes a substrate dielectric layer 110 located on the substrate structure 100, and the microlens 140 is located on the substrate dielectric layer 110.

[0060] In the optical device and manufacturing method thereof provided in the embodiment of the present application, a first dielectric layer 120 is formed on a substrate structure 100, a portion of the first dielectric layer 120 is patterned to remove a portion of the first dielectric layer 120 to form an opening 121 in the first dielectric layer 120, the opening 121 divides the first dielectric layer 120 into at least one first sub-dielectric layer 122, and the first sub-dielectric layer 122 is rounded to form a microlens 140, thereby, the microlens 140 can be manufactured simultaneously in a chip factory without being transferred to a special microlens factory, thereby improving production efficiency and shortening production cycle. Accordingly, the formed optical device 10 has a microlens 140 formed by a semiconductor process, and the microlens 140 has higher compactness and uniformity, thereby also obtaining higher optical efficiency.

[0061] [Example 2]

[0062] Please refer to Figures 10 to 12 , which is a cross-sectional schematic diagram of a device structure formed during the process of executing the method for manufacturing an optical device according to the second embodiment of the present invention. Fig.10 As shown, a substrate structure 200 is provided. In an embodiment of the present application, the substrate structure 200 includes: a first wafer 201, a second wafer 202 bonded to the first wafer 201, and a wiring layer 203 located on the second wafer 202. The first wafer 201 is, for example, a logic wafer, and the second wafer 202 is, for example, a pixel wafer. In other embodiments of the present application, the substrate structure 200 may also be other structures. For example, the substrate structure 200 may also include a single wafer structure, and the wafer structure includes a logic area, a pixel area, etc. The substrate structure 200 may also include a single or stacked chip. The substrate structure 200 may also include wafers and chips bonded together; the material of the substrate structure 200 may include semiconductor materials, and may also include non-semiconductor materials, such as glass, ceramics, etc.

[0063] like Fig.11 As shown, in the embodiment of the present application, then, a base dielectric layer 210 is formed on the base structure 200, and a first dielectric layer 220 is formed on the base dielectric layer 210. The base dielectric layer 210 and / or the first dielectric layer 220 are made of organic materials or inorganic materials. In this embodiment, the base dielectric layer 210 is made of silicon nitride, which mainly serves as an etching stop layer; the first dielectric layer 220 is made of silicon oxide, which is used to form a microlens. The thickness of the base dielectric layer 210 is, for example, The thickness of the first dielectric layer 220 is, for example, The material and thickness of the base dielectric layer 210 and the first dielectric layer 220 are not limited to the above description, and may be other materials or thicknesses known in the art.

[0064] Furthermore, a second dielectric layer 230 is formed on the first dielectric layer 220, and a second mask layer (not shown) is formed on the second dielectric layer 230. The second mask layer is any material known in the art, such as a hard mask layer, a photoresist, etc. In the embodiment of the present application, the second mask layer is a photoresist layer. The thickness of the second dielectric layer 230 is preferably The thickness of the second mask layer may be, for example, Next, the second mask layer is patterned to form a second basic pattern mask layer 240. The second basic pattern mask layer 240 includes, for example, a plurality of photoresist blocks arranged in an array. The thickness of the second mask layer and the thickness of the second dielectric layer 230 may not be limited to the above ranges.

[0065] like Fig.12 Please combine Fig.13 , using the second basic pattern mask layer 240 as a mask, etching the second dielectric layer 230 to obtain a patterned mask layer 231, wherein the material of the patterned mask layer 231 is a dielectric material, that is, the patterned mask layer 231 is a patterned second dielectric layer. Also, etching a portion of the thickness of the first dielectric layer 220 to form an opening 221 in the first dielectric layer 220, wherein the opening 221 divides the first dielectric layer 220 into at least one first sub-dielectric layer 222. In the embodiment of the present application, the opening 221 also divides the first dielectric layer 220 into a second sub-dielectric layer 223, wherein the first sub-dielectric layer 222 is located on the second sub-dielectric layer 223, wherein the cross-sectional width of the first sub-dielectric layer 222 parallel to the surface of the substrate structure may be less than, equal to, or greater than the cross-sectional width of the second sub-dielectric layer 223 parallel to the surface of the substrate structure, and a step may be formed between the first sub-dielectric layer 222 and the second sub-dielectric layer 223. For example, 1 / 10 to 2 / 3 of the thickness of the first dielectric layer 220 is etched to form the opening 221 and divide the first sub-dielectric layer 222 and the second sub-dielectric layer 223 , wherein the etching thickness can be matched and controlled by the etchant and etching time.

[0066] like Fig.14 As shown, in the embodiment of the present application, then, the second basic pattern mask layer 240 is removed to expose the patterned mask layer 231. Specifically, the second basic pattern mask layer 240 can be removed by ashing or other processes.

[0067] Please continue to refer to Fig.14, which is different from the first embodiment, in the embodiment of the present application, the patterned mask layer 231 covers the edge surface of the first sub-dielectric layer 222, that is, here, the patterned mask layer 231 covers the entire surface of the first sub-dielectric layer 222. In the terminology of the present application, the surface specifically refers to the upper surface, and the side surface is described as the side surface. Among them, at the edge position 231A of the patterned mask layer 231, the etching selectivity ratio of the first sub-dielectric layer 222 and the patterned mask layer 231 is less than X:1; at the middle position 231B of the patterned mask layer 231, the etching selectivity ratio of the first sub-dielectric layer 222 and the patterned mask layer 231 is greater than X:1. That is, at the edge position 231A of the patterned mask layer 231, the etching selectivity ratio of the first dielectric layer 220 and the patterned mask layer 231 is less than X: 1; at the middle position 231B of the patterned mask layer 231, the etching selectivity ratio of the first dielectric layer 220 and the patterned mask layer 231 is greater than X: 1. Therefore, in the subsequent etching process, the first sub-dielectric layer 222 corresponding to the edge position 231A will be etched and removed more, while the first sub-dielectric layer 222 corresponding to the middle position 231B will be etched and removed less, so that a microlens with a curved surface can be formed through the etching process.

[0068] Then, if Fig.15 and Fig.16 As shown, the first sub-medium layer 222 is etched using the patterned mask layer 231 as a mask to obtain the microlens 250. In the embodiment of the present application, the second sub-medium layer 223 is also patterned and / or rounded at the same time. Fig.15 As shown, during the process of etching the first dielectric layer 220, the patterned mask layer 231 is also slowly consumed, wherein the consumption rate of the patterned mask layer 231 at the edge position 231A is faster than the consumption rate of the patterned mask layer 231 at the middle position 231B; and the amount of the first sub-dielectric layer 222 or the first dielectric layer 220 corresponding to the edge position 231A etched and removed is greater than the amount of the first sub-dielectric layer 222 or the first dielectric layer 220 corresponding to the middle position 231B, as shown in FIG. Fig.16 As shown, a microlens 250 having a curved surface is formed.

[0069] Preferably, the value of X is between 5 and 20, that is, the value of X is greater than or equal to 5 and less than or equal to 20. Here, by selecting the value of X, the curvature radius R2 of the microlens 250 can be adjusted, wherein the larger the value of X is, the larger the curvature radius R2 of the microlens 250 is.

[0070] Please continue to refer to Fig.12 and Fig.16Accordingly, an optical device 20 is formed, and the optical device 20 includes: a substrate structure 200; and a microlens 250 located on the substrate structure 200, and the microlens 250 is formed by patterning and rounding the first dielectric layer 220 located on the substrate structure 200. In the embodiment of the present application, the optical device 20 also includes a substrate dielectric layer 210 located on the substrate structure 200, and the microlens 140 is located on the substrate dielectric layer 210.

[0071] [Example 3]

[0072] Please refer to Figures 17 to 20 , which is a cross-sectional schematic diagram of a device structure formed during the process of executing the method for manufacturing an optical device according to the third embodiment of the present invention. Fig.17 As shown, a substrate structure 300 is provided. In an embodiment of the present application, the substrate structure 300 includes: a first wafer 301, a second wafer 302 bonded to the first wafer 301, and a wiring layer 303 located on the second wafer 302. The first wafer 301 is, for example, a logic wafer, and the second wafer 302 is, for example, a pixel wafer. In other embodiments of the present application, the substrate structure 300 may also be other structures. For example, the substrate structure 300 may also include a single wafer structure, and the wafer structure includes a logic area, a pixel area, etc. The substrate structure 300 may also include a single or stacked chip. The substrate structure 300 may also include wafers and chips bonded together; the material of the substrate structure 300 may include semiconductor materials, and may also include non-semiconductor materials, such as glass, ceramics, etc.

[0073] like Fig.18 As shown, in the embodiment of the present application, then, a base dielectric layer 310 is formed on the base structure 300, and a first dielectric layer 320 is formed on the base dielectric layer 310. The base dielectric layer 310 and / or the first dielectric layer 320 are made of organic materials or inorganic materials. In this embodiment, the base dielectric layer 310 is made of silicon nitride, which mainly serves as an etching stop layer; the first dielectric layer 320 is made of silicon oxide, which is used to form a microlens. The thickness of the base dielectric layer 310 is, for example, The thickness of the first dielectric layer 320 is, for example, The material and thickness of the base dielectric layer 310 and the first dielectric layer 320 are not limited to the above description, and may be other materials or thicknesses known in the art.

[0074] Please continue to refer to Fig.18, in the embodiment of the present application, then, a third mask layer is formed on the first dielectric layer 320 (not shown in the figure, the first mask layer in the first embodiment, the second mask layer in the second embodiment, and the third mask layer in the third embodiment can be collectively referred to as a mask layer), wherein the third mask layer can be the first mask layer in the first embodiment or the second mask layer in the second embodiment; the third mask layer is patterned to form a basic graphic mask layer 330. Wherein, the third mask layer is any material known in the art, for example, a hard mask layer, a photoresist, etc. In the embodiment of the present application, the third mask layer is a photoresist layer. The basic graphic mask layer 330, for example, includes a plurality of photoresist blocks arranged in an array to form microlenses arranged in an array. Wherein, the thickness of the basic graphic mask layer 330 can be, for example, The thickness of the basic pattern mask layer 330 may not be limited to the above range.

[0075] like Fig.19 As shown, then, using the basic pattern mask layer 330 as a mask, a portion of the first dielectric layer 320 is patterned and removed to form an opening 321 in the first dielectric layer 320. The opening 321 divides the first dielectric layer 320 into at least one first sub-dielectric layer 322. Here, the opening 321 exposes a portion of the base dielectric layer 310, that is, the opening 321 penetrates the first dielectric layer 320 and divides the first dielectric layer 320 into only at least one first sub-dielectric layer 322. In other embodiments, the opening 321 may not expose the base dielectric layer 310, that is, the opening 321 does not penetrate the first dielectric layer 320 and divides the first dielectric layer 320 into a second sub-dielectric layer (not shown). The first sub-dielectric layer 322 is located on the second sub-dielectric layer. The cross-sectional width of the first sub-dielectric layer 322 parallel to the surface of the base structure may be less than, equal to, or greater than the cross-sectional width of the second sub-dielectric layer parallel to the surface of the base structure. A step may be formed between the first sub-dielectric layer 322 and the second sub-dielectric layer.

[0076] Please continue to refer to Fig.19In the embodiment of the present application, the first sub-medium layer 322 includes at least two sub-layers 3220, and the cross-sectional width of each sub-layer 3220 in parallel with the surface of the base structure 300 gradually increases from away from the base structure 300 to close to the base structure 300, and a step may be formed between two adjacent sub-layers 3220, and at least two sub-layers 3220 are formed in a manner well known in the art. Here, three sub-layers 3220 are schematically shown, wherein the cross-sections of the sub-layers 3220 gradually widen from top to bottom, the uppermost sub-layer 3220 exposes the middle sub-layer 3220, and the middle sub-layer 3220 exposes the lowermost sub-layer 3220, thereby forming three step structures.

[0077] Then, if Fig. 20 As shown, a third dielectric layer 340 is formed, and the third dielectric layer 340 at least covers the side of the first sub-dielectric layer 322 so that the connection between the surface and the side of the first sub-dielectric layer 322 forms a curved surface, thereby obtaining a microlens 350. It should be noted that before forming the third dielectric layer 340, due to the limitation of the process itself, when at least two layers of the sub-layers 3220 are formed, the connection between the surface and the side of each layer of the sub-layer 3220 can be a curved surface. In the embodiment of the present application, the third dielectric layer 340 also covers the surface of the first sub-dielectric layer 322, that is, the third dielectric layer 340 covers the surface and side of each sub-layer 3220. Specifically, the third dielectric layer 340 can be formed by a deposition process. The first sub-dielectric layer 322 can be rounded by the third dielectric layer 340, thereby forming a microlens 350 with an arc surface, thereby improving the quality and reliability of the formed microlens 350. In the embodiment of the present application, the third dielectric layer 340 also covers the exposed substrate dielectric layer 310, thereby simplifying the formation process of the microlens 350. In the embodiment of the present application, the curvature radius R3 of the microlens 350 is between In other embodiments, the radius of curvature R3 of the microlens 140 may be less than or greater than

[0078] Accordingly, the present application embodiment also provides an optical device, please continue to refer to Fig. 20 The optical device 30 includes: a substrate structure 300; and a microlens 350 located on the substrate structure 300, wherein the microlens 350 is formed by patterning and rounding a first dielectric layer 320 located on the substrate structure 300 and further covering a third dielectric layer 340. In the embodiment of the present application, the optical device 30 also includes a substrate dielectric layer 310 located on the substrate structure 300, and the microlens 350 is located on the substrate dielectric layer 310.

[0079] In the present application, references to "one embodiment" or "some embodiments" mean that features, structures, or characteristics described in conjunction with the embodiment are included in at least one embodiment, at least some embodiments, of the present application. Therefore, the appearance of the phrases "in one embodiment" or "in some embodiments" in various places of the present application does not necessarily refer to the same or the same embodiments. In addition, in one or more embodiments, features, structures, or characteristics may be combined in any suitable combination and / or sub-combination.

[0080] Although some specific embodiments of the present application have been described in detail by way of example, it will be appreciated by those skilled in the art that the above examples are for illustration only and are not intended to limit the scope of the present application. The various embodiments of the present application may be combined in any manner without departing from the spirit and scope of the present application. It will also be appreciated by those skilled in the art that various modifications may be made to the embodiments without departing from the scope and spirit of the present application. The scope of the present application is defined by the appended claims.

Claims

1. A method for manufacturing an optical device, characterized in that: The method for manufacturing the optical device comprises: Providing a base structure; forming a first dielectric layer on the base structure; and, Part of the first dielectric layer is patterned and removed to form an opening in the first dielectric layer, wherein the opening divides the first dielectric layer into at least one first sub-dielectric layer, and the first sub-dielectric layer is rounded to form a microlens.

2. The method for manufacturing an optical device according to claim 1, wherein: Rounding the first sub-medium layer includes: A patterned mask layer is formed on the first sub-dielectric layer, and the connection between the surface and the side surface of the first sub-dielectric layer is etched using the patterned mask layer as a mask to form a curved surface.

3. The method for manufacturing an optical device according to claim 2, wherein: The patterned mask layer exposes an edge surface of the first sub-dielectric layer; Etching the connection between the surface and the side of the first sub-dielectric layer includes: The exposed edge surface of the first sub-dielectric layer is etched.

4. The method for manufacturing an optical device according to claim 3, wherein: The method for forming the patterned mask layer includes: forming a first mask layer on the first dielectric layer; Patterning the first mask layer to form a first basic pattern mask layer, and using the first basic pattern mask layer as a mask, etching a portion of the thickness of the first dielectric layer to form the opening; The first basic pattern mask layer is constricted to form the patterned mask layer.

5. The method for manufacturing an optical device according to claim 4, wherein: After etching the connection between the surface and the side of the first sub-dielectric layer, rounding the first sub-dielectric layer further comprises: Repeat one or more times: shrink the patterned mask layer to expose the edge surface of the first sub-dielectric layer, and etch the exposed edge surface of the first sub-dielectric layer using the shrunken patterned mask layer as a mask.

6. The method for manufacturing an optical device according to claim 2, wherein: The patterned mask layer covers the edge surface of the first sub-dielectric layer; Etching the connection between the surface and the side of the first sub-dielectric layer includes: Etching the first sub-dielectric layer, wherein at an edge position of the patterned mask layer, an etching selection ratio between the first sub-dielectric layer and the patterned mask layer is less than X:1; At a middle position of the patterned mask layer, an etching selection ratio between the first sub-dielectric layer and the patterned mask layer is greater than X:

1.

7. The method for manufacturing an optical device according to claim 6, wherein: Forming the patterned mask layer includes: forming a second dielectric layer and a second mask layer in sequence on the first dielectric layer; The second mask layer is patterned to form a second basic graphic mask layer, and the second dielectric layer is etched using the second basic graphic mask layer as a mask to obtain the graphic mask layer, and a portion of the thickness of the first dielectric layer is etched to form the opening.

8. The method for manufacturing an optical device according to claim 1, wherein: Rounding the first sub-dielectric layer includes: A third dielectric layer is formed, wherein the third dielectric layer at least covers the side surface of the first sub-dielectric layer so that a connection between the surface and the side surface of the first sub-dielectric layer forms a curved surface.

9. The method for manufacturing an optical device according to claim 8, wherein: The first sub-medium layer includes at least two sub-layers, and the cross-sectional width of each sub-layer parallel to the surface of the base structure gradually increases from a direction away from the base structure to a direction close to the base structure; Wherein, the third dielectric layer covers the side surfaces of each sub-layer.

10. The method for manufacturing an optical device according to any one of claims 1 to 7, wherein: The opening divides the first dielectric layer into a second sub-dielectric layer, and the first sub-dielectric layer is located on the second sub-dielectric layer.

11. The method for manufacturing an optical device according to claim 10, wherein: While the first sub-dielectric layer is rounded, the second sub-dielectric layer is also patterned and / or rounded.

12. An optical device, characterized in that: The optical device comprises: a substrate structure; and a microlens located on the substrate structure, wherein the microlens is formed by patterning and rounding a first dielectric layer located on the substrate structure.

13. The optical device according to claim 12, characterized in that The microlens is made of silicon oxide.

14. The optical device according to claim 12, characterized in that The microlens is formed by the method for manufacturing an optical device according to any one of claims 1 to 11.