Selective stencil mask and stencil printing method

Through the use of selective stencil masks, the problems of solder bump bridging and non-wetting in the traditional stencil printing process are solved, the quality and wettability of solder bumps are improved, and the yield rate of semiconductor products is improved.

CN118732383APending Publication Date: 2024-10-01STATS CHIPPAC LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310326565.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The traditional stencil printing process is prone to solder bump bridging and non-wetting solder joints when the solder bump pitch is small, resulting in a decrease in the yield of semiconductor products.

Method used

Using a selective stencil mask with a printing area and a blocking area, the fluid material is deposited onto the substrate through the hole array in the printing area, and a gap is formed by contacting the support member with the substrate to avoid exerting pressure on the existing solder bumps and ensuring fluid flow Selective printing of materials.

Benefits of technology

It improves the quality and wettability of solder bumps, reduces the occurrence of solder bump bridging and non-wetted solder joints, and improves the yield rate of semiconductor products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118732383A_ABST
    Figure CN118732383A_ABST
Patent Text Reader

Abstract

The invention provides a selective stencil mask and a stencil printing method. A stencil mask for printing a fluid material onto a substrate, and comprising: a stencil member comprising: at least one printing area wherein each printing area has an array of apertures allowing the fluid material to flow through and deposit onto the substrate; and a barrier region configured to prevent a flow of fluid material therethrough; the present invention relates to a mask apparatus including a template member, and a support member attached to the template member and configured to contact a substrate and create a gap between the template member and the substrate when a template mask is placed on the substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates generally to semiconductor manufacturing technology, and more particularly to a stencil mask and a stencil printing method. Background Art

[0002] The semiconductor industry has been facing the challenge of complex integration as consumers want their electronic products to be smaller, faster, and higher performing, as well as to integrate more and more functions into a single device. People want to have a large chip size with high bump count and fine bump pitch, such as less than 100μm. However, using the currently available flip-chip flux dipping process, these chips often have non-wetting solder joints in the peripheral area of ​​the chip due to chip bending, and bump bridging problems in the center area of ​​the chip.

[0003] Therefore, there is a need for an improved stencil mask and stencil printing method. Summary of the invention

[0004] One object of the present application is to provide a stencil mask that can improve the quality of solder bumps on a substrate when the stencil mask is used in a stencil printing process.

[0005] According to one aspect of the present application, a template mask for printing a fluid material onto a substrate is provided, the template mask comprising: a template member, the template member comprising: at least one printing area, each printing area having an array of holes that allow the fluid material to flow through and be deposited onto the substrate; and a blocking area, the blocking area being configured to prevent the fluid material from flowing therethrough; and a support member, the support member being attached to the template member and being configured such that when the template mask is placed on the substrate, the support member contacts the substrate and creates a gap between the template member and the substrate.

[0006] According to another aspect of the present application, a template printing method is provided, comprising: providing a substrate, the substrate comprising at least one printing location; providing a template mask, the template mask comprising: a template member, the template member comprising at least one printing area, each printing area having a hole array allowing a fluid material to flow therethrough, and a blocking area for preventing the fluid material from flowing therethrough; and a support member attached to the template member; placing the template mask on the substrate, creating a gap between the template member and the substrate through the support member, and aligning the at least one printing area with the at least one printing location, respectively; depositing the fluid material onto the substrate through the at least one printing area, so that the fluid material flows through the at least one hole array to at least one printing location.

[0007] According to another aspect of the present application, a method for forming a semiconductor package is provided, including: providing a first substrate and a second substrate; forming a first plurality of solder bumps in a first region of the first substrate using a first template mask; forming a second plurality of solder bumps in a second region of the first substrate using a second template mask; forming solder bumps on the second substrate; aligning the first plurality of solder bumps and the second plurality of solder bumps on the first substrate with the solder bumps on the second substrate to connect the first substrate and the second substrate; and reflowing the first plurality of solder bumps and the second plurality of solder bumps on the first substrate and the solder bumps on the second substrate.

[0008] According to another aspect of the present application, a method for forming a template mask is provided, comprising: providing a substrate; forming a first photoresist pattern having a first opening on the substrate; filling a first electroplating material in the first opening of the first photoresist pattern; forming a second photoresist pattern having a second opening on the first photoresist pattern; filling a second electroplating material in the second opening of the second photoresist pattern; and removing the first photoresist pattern and the second photoresist pattern on the substrate.

[0009] According to another aspect of the present application, a method for forming a semiconductor package is provided, comprising: providing a first substrate and a second substrate; forming a first plurality of solder bumps in a first region of the first substrate and forming a second plurality of solder bumps in a second region of the first substrate using a first template mask; depositing flux onto the second plurality of solder bumps using a second template mask; forming solder bumps on the second substrate; aligning the first plurality of solder bumps and the second plurality of solder bumps on the first substrate with the solder bumps on the second substrate to connect the first substrate and the second substrate; and reflowing the first plurality of solder bumps and the second plurality of solder bumps on the first substrate and the solder bumps on the second substrate.

[0010] It should be understood that the foregoing general description and the following detailed description are exemplary and illustrative only, rather than limiting the present invention. In addition, the accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments of the present invention and together with the description serve to explain the principles of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] The drawings cited herein constitute a part of the specification. The features shown in the drawings illustrate only some embodiments of the present application, not all embodiments of the present application, unless otherwise explicitly stated in the detailed description, and readers of the specification should not make contrary suggestions.

[0012] Figure 1A , 1B 1C and 1C respectively show a substrate with a template mask attached according to an embodiment of the present application.

[0013] Figures 2A to 2E A process for forming a bond between two substrates is shown according to one embodiment of the present application.

[0014] Figures 3A to 3H A process for forming a stencil mask is shown according to one embodiment of the present application.

[0015] Figures 4A to 4B According to one embodiment of the present application, a method for forming a stencil mask is shown.

[0016] Figure 5A and 5B A substrate to which a stencil mask is attached is respectively shown according to one embodiment of the present application.

[0017] Figures 6A to 6E A process for forming a bond between two substrates is shown according to one embodiment of the present application.

[0018] The same reference numbers will be used throughout the drawings to refer to the same or like parts. DETAILED DESCRIPTION

[0019] The following detailed description of exemplary embodiments of the present application refers to the accompanying drawings that form a part of the description. The accompanying drawings show specific exemplary embodiments in which the present application can be practiced. The detailed description, including the accompanying drawings, describes these embodiments in sufficient detail to enable those skilled in the art to practice the present application. Those skilled in the art may further utilize other embodiments of the present application and make logical, mechanical, etc. changes without departing from the spirit or scope of the present application. Therefore, readers of the following detailed description should not interpret the description in a restrictive manner, and only limit the scope of the embodiments of the present application with the appended claims.

[0020] In this application, the use of the singular includes the plural unless otherwise expressly stated. In this application, the use of "or" means "and / or" unless otherwise expressly stated. In addition, the use of the term "includes" and other forms such as "includes" and "comprising" are not limiting. In addition, unless otherwise expressly stated, terms such as "element" or "component" cover elements and components that include one unit, as well as elements and components that include more than one subunit. In addition, the section headings used herein are for organizational purposes only and should not be construed as limiting the subject matter described.

[0021] As used herein, spatially relative terms, such as "below," "below," "above," "above," "up," "upper side," "lower side," "left side," "right side," "horizontal," "vertical," "lateral," and the like, may be used herein to facilitate description of the relationship of one element or feature to another element or feature as shown in the accompanying drawings. In addition to the orientation depicted in the figures, spatially relative terms are intended to cover different orientations of the device in use or operation. The device may be oriented in other ways (rotated 90 degrees or in other orientations), and the spatially relative descriptors used herein may likewise be interpreted accordingly. It should be understood that when an element is referred to as being "connected to" or "coupled to" another element, it may be directly connected to or coupled to the other element, or there may be intermediate elements.

[0022] The inventors of the present application have found that, due to the small solder bump spacing, the substrate produced by the conventional stencil printing process may produce solder bump bridging in the central area of ​​the substrate, and non-wetting solder bumps in the peripheral area of ​​the substrate due to substrate warping during the reflow process. Both solder bump bridging and non-wetting solder bumps reduce the yield of semiconductor products manufactured using the conventional stencil printing process and are therefore undesirable. Various measures have been taken to try to solve these problems. For example, deep flux dipping and scraper printing in specific non-wetting edge areas are generally used to overcome these problems. However, these methods may result in more solder bump bridging or produce undesirable extrusion pressure on the substrate.

[0023] In order to further improve the traditional stencil printing process, a new stencil mask and a stencil printing process using the stencil mask are proposed for printing a fluid material onto a printed circuit board, a semiconductor die or a semiconductor package. The stencil mask is a selective stencil mask having a printing area and a blocking area. The blocking area usually has no holes, so no fluid material can flow through the blocking area in the stencil mask. In addition, the printing area has holes that allow the fluid material to flow through and deposit on the substrate. Using this stencil mask, the fluid material can be selectively printed onto the substrate, for example, in an area where a solder bump with a first pitch is required; in addition, other areas of the substrate can use another stencil mask or use another type of solder forming process to print solder bumps with a second pitch. Since the solder bumps in the two areas of the substrate are formed by different stencil masks or even different processes, different amounts of fluid materials can be used for the solder bumps in different areas to allow better wetting of the solder bumps and different pitches.

[0024] According to an embodiment of the present application, Figure 1A , 1B 1C and 1C respectively show the substrate 101 with the template mask 111 attached. Figure 1A is a top view of the substrate 101 . Figure 1B and Figure 1C Along Figure 1A The cross-sectional view of the substrate 101 before and after the fluid material is deposited onto the substrate 101 through the template mask 111 is shown along line AA′.

[0025] Reference Figure 1A and 1B , the stencil mask 111 is placed on a substrate 101 such as a semiconductor package or a printed circuit board. The substrate 101 has various conductive patterns 103, such as a redistribution layer (RDL). In the present embodiment, the substrate 101 is partially formed with solder bumps 105, for example, at the center position of the substrate 101, and the solder bumps 105 can be electrically connected to each conductive pattern 103. It can be understood that the center position can be relatively closer to the center of the substrate 101 than the peripheral position of the substrate 101. However, it is not required that the center position should be at the center of the substrate 101. In some embodiments, the solder bumps 105 formed on the substrate 101 can be pre-formed using another stencil printing process or another type of solder bump forming process. Therefore, the stencil printing process can be performed in the remaining portion of the substrate 101 where the solder bumps are not formed using the stencil mask 111, that is, in the bump-free area. It can be understood that in some other embodiments, the solder bumps 105 in the bump area of ​​the substrate 101 can be formed using another stencil mask and stencil printing process at a later stage.

[0026] Specifically, the stencil mask 111 includes a stencil member 113 and a support member 115 for supporting the stencil member 113. In this embodiment, the stencil member 113 is in the form of a generally flat plate with a hole 117 passing through a specific area. Corresponding to the substrate 101 on which the solder bump is not fully formed, the stencil member 113 includes at least one printing area 113a having a hole and a blocking area 115 without a hole. In some embodiments, the printing area 113a may be distributed across the substrate 101, wherein each printing area has an array of holes. The support member 115 is attached to the stencil member 113, for example, below the stencil member 113. In some embodiments, the stencil member 113 and the support member 115 may be formed together as a single piece using a single process, or may be formed separately using two processes and then connected to each other.

[0027] like Figure 1A and 1BAs shown, when the template mask 111 is placed on the substrate 101, the support member 115 can contact the substrate 101 and generate a gap 119 between the template member 113 and the substrate 101. The printing area 113a with the hole 117 can allow a fluid material such as solder to flow through and be deposited on the substrate 101. In this way, the solder bumps on the substrate 101 can be formed in different batches and processes to have different characteristics, such as different sizes, spacings and / or fluid materials. Differently, the gap 119 between the template member 113 and the substrate 101 can accommodate the solder bumps already formed on the substrate 101. With the generated gap 119, the template member 113 will not apply any pressure to the previously formed solder bump 105 and will not cause any damage to it. Due to the gap printing effect, the printability of the fluid material is also improved. That is, during the printing process, the fluid material can be easily swept to the desired position of the template member 111 by the scraper.

[0028] like Figure 1A and 1B As shown, support member 115 includes a plurality of support bars. In some embodiments, support member 115 may include a plurality of support pins or other similar structures. When template mask 111 is placed on substrate 101, support bars may be disposed at locations of substrate 101 where solder bumps 105 were not previously formed, i.e., in bump-free areas. Thus, support bars provide anchor points for template member 113 on substrate 101. Figure 1B As shown, the support member 115 may have support bars not only under the blocking area 113b, but also under the partial printing area 113a, as long as they do not interfere with the formation of the solder bumps to be formed. For example, some support bars may be arranged near the edge of the template member 113 or at the edge of the template member 113, but may not be arranged directly below the hole 117. Preferably, the support bars may be distributed roughly evenly on the template member 113 to avoid excessive stress on the template mask at some specific locations when the scraper sweeps the fluid material along the template mask 111. It is understood that the height of the support bar should be greater than the height of the solder bump 105 that has been formed and the solder bump to be formed, so as not to damage the solder bump. In some embodiments, the support bar may be 20μm to 5mm higher than the maximum height of the solder bump.

[0029] In some embodiments, for example Figure 1A In the embodiment shown, the blocking area 113b is located at the center of the template member 113, and the printing area 113a is located at the periphery of the template member 113 and surrounds the blocking area 113b. In some other embodiments, the printing area 113a can be in the form of several separate areas separated by the blocking area 113b and have corresponding hole arrays 117.

[0030] refer to Figure 1C , which shows a cross-sectional view of the substrate 101 after performing a stencil printing process, wherein the printing area 113a is located at the peripheral position of the template member 113, and a fluid material such as solder can flow through the template member 113 and be deposited to the peripheral position of the substrate 101 through the hole array 117, thereby forming the desired solder bump 107. At the same time, the blocking area 113b can prevent the fluid material from flowing therethrough and being deposited to the central position of the substrate 101. Through the selective stencil mask, a sufficient amount of fluid material can be deposited at the peripheral position of the substrate 101 without applying additional fluid material at the central position of the substrate 101. In this way, the solder bump 107 at the peripheral position of the substrate 101 can have a sufficient amount of fluid material, thereby providing a sufficient wetting angle for the solder bump during reflow, and at the same time, any undesirable solder bump bridging can be prevented from forming for the solder bump 105 at the central position of the substrate 101, because a smaller amount of fluid material can be used in the previous stencil printing process for forming the solder bump 105.

[0031] The template mask 111 can be made of stainless steel, nickel, copper or other suitable materials. In addition, the template mask 111 can be used to print any desired fluid material onto any other type of substrate, such as glass plate, steel plate, printed circuit board, semiconductor substrate, semiconductor grain or semiconductor package, etc. For example, the substrate 101 can be a PCB, a laminated interposer, a strip interposer, a lead frame or other suitable substrates. The substrate 101 can include one or more insulating or passivation layers, one or more conductive vias formed through the insulating layer, and one or more conductive layers formed on or between the insulating layers. The substrate 101 can include one or more pre-impregnated polytetrafluoroethylene, FR-4, FR-1, CEM-1 or CEM-3 and a combination of phenolic cotton paper, epoxy resin, resin, glass fiber, frosted glass, polyester or other reinforcing fibers or fabrics. The substrate 101 can also be a multilayer flexible laminate, ceramic, copper-plated laminate, glass or semiconductor wafer, and the semiconductor wafer can contain one or more transistors, diodes and other circuit elements to realize analog circuits or digital circuits. The substrate 101 may include one or more conductive layers or redistribution layers (RDL) formed using sputtering, electrolytic plating, electroless plating, or other suitable deposition processes. The conductive layer may be one or more layers of Al, Cu, Sn, Ni, Au, Ag, Ti, W, or other suitable conductive materials. In some embodiments, one or more conductive patterns may be exposed to the surface of the substrate 101 and subsequently connected to one or more external electronic components.

[0032] According to one embodiment of the present application, Figures 2A to 2EA process for forming a bond between two substrates is shown. In some embodiments, the process can be used in a process for forming a semiconductor package including two substrates.

[0033] like Figure 2A As shown, a first substrate 201 may be provided, which may have a first plurality of solder bumps 205 in a central region of the substrate 201. For example, the first plurality of solder bumps 205 may be formed using a first stencil printing process, which may allow a fine pitch of 90 μm or even less. A portion of the upper surface of the substrate 201, typically in a peripheral region of the substrate 201, may be free of solder bumps, so that some of the conductive pattern 203 may be exposed.

[0034] Afterwards, if Figure 2B As shown, the first substrate 201 may be subjected to a second template printing process to form a second plurality of solder bumps 207 in the peripheral region of the substrate 201. The second plurality of solder bumps 207 may cover the exposed conductive patterns 203 and be electrically connected to the conductive patterns. In this embodiment, the second template printing process may use reference Figures 1A to 1C The second stencil printing process can be implemented using a stencil mask as shown in the embodiment of . Because it is a different process from the first stencil printing process, the second stencil printing process can be implemented using a different configuration. For example, the aperture size of the stencil mask, the amount of solder of the second plurality of solder bumps 207, and / or the spacing of the second plurality of solder bumps can be different from those parameters of the first plurality of solder bumps 205. As described above, the stencil mask used in the second stencil printing process provides gaps that can accommodate the first plurality of solder bumps 205 and protect them from damage and contamination during the second stencil printing process.

[0035] Next, if Figure 2C As shown, a second substrate 221 may be provided. The second substrate 221 may have solder bumps 223 corresponding to and facing the first and second plurality of solder bumps 205 and 207. The second substrate 221 may be joined to the first substrate 201 through the solder bumps 205, 207, and 223. In some embodiments, the solder bumps 223 may have a substantially uniform shape and size, and flux may be formed thereon by a dipping process. In addition, as shown in FIG. Figure 2D As shown, the second substrate 221 is placed on the first substrate 201 and the solder bumps 223 are aligned with and in contact with corresponding solder bumps in the first and second pluralities of solder bumps 205 and 207 .

[0036] Next, if Figure 2EAs shown, a reflow process can be performed on the connected substrates 201 and 221 to reflow the solder material therebetween. It can be understood that even if the periphery of the second substrate 221 above is warped due to heat, the solder bumps on the peripheries of the two substrates 201 and 221 will not be disconnected or insufficiently wetted due to the presence of a large amount of solder that remains wetted.

[0037] Understandably, Figures 2A to 2E The process shown is exemplary only and modifications, changes or additions may be made to the process. Figure 2A In the embodiment, the substrate 201 may have other regions without solder bumps in addition to the exposed conductive pattern 203 in the peripheral region of the substrate 201. Figure 2A In an alternative embodiment, the first plurality of solder bumps 205 may be formed after the second plurality of solder bumps 207 .

[0038] The stencil mask according to the embodiments of the present application can be formed using any suitable means. In some preferred embodiments, the stencil mask can be formed using an in-situ formation process, i.e., directly formed on a substrate that will subsequently be subjected to a stencil printing process using the stencil mask. It will be appreciated that in some alternative embodiments, the stencil mask can be formed separately from the substrate and then attached to the substrate prior to the stencil printing process.

[0039] According to an embodiment of the present application, Figures 3A to 3H A process for forming a stencil mask is shown.

[0040] like Figure 3A As shown, a substrate 301 is provided. The substrate 301 is formed with a first photoresist 341. In some embodiments, the first photoresist 341 can be a positive photoresist or a negative photoresist, with slightly different subsequent processes and photomasks. In the present embodiment, the first photoresist 341 is a positive photoresist. A first photomask 351 is placed above the substrate 301, which has an opaque area 353 and a transparent area 355, such as a window or opening that allows light to pass through. Light radiation, such as ultraviolet light, can be emitted to the substrate 301 through the first photomask 351. In this way, the first photoresist 341 on the substrate 343 can be selectively exposed to form two parts, namely, an exposed part 341 and an unexposed part 343. The first photoresist 341 can be further developed by a developing solution so that the exposed part 341 can be removed from the substrate 301, as shown in FIG. Figure 3B shown.

[0041] Afterwards, if Figure 3C As shown, the substrate 301 may be subjected to a first electroplating process to form a first electroplating block 315, which is filled in the location where the exposed photoresist portion 341 is located. The first electroplating block 315 forms a supporting member of the template mask, for example Figures 1A to 1CNext, a second photoresist 361 is further formed on the substrate 301, the first electroplating block 315 and the remaining portion of the first photoresist layer 341, as shown in FIG. Figure 3D shown.

[0042] Next, if Figure 3E As shown, the second photoresist layer 361 is patterned using a second photomask 371. Figure 3A The patterning of the first photoresist layer 341 is similar to that shown in FIG. Specifically, light radiation can be emitted to the substrate 301 through the second photomask 371, which exposes most of the second photoresist layer 361, leaving only a portion 363 thereof unexposed. Figure 3F As shown, the second photoresist layer 361 may be further developed using a developer to remove most of the exposed portion of the second photoresist layer 361 , leaving only the unexposed portion 363 on the substrate 301 .

[0043] Afterwards, if Figure 3G As shown, the substrate 301 can be subjected to a second electroplating process to form a second electroplating block 313 to fill the position of the exposed photoresist portion 361. The second electroplating block 313 forms a template component of the template mask, for example Figures 1A to 1C The template member 113 shown in FIG. Next, as Figure 3H As shown in FIG. 1 , the photoresist remaining on the substrate 301 can be completely removed from the substrate 301, leaving the first electroplating block 313 and the second electroplating block 315 on the substrate 301. In this way, the following is obtained: Figures 1A to 1C Stencil mask 311 of stencil mask 111 is shown. In some embodiments, stencil mask 311 can be further released from substrate 301 for further stencil printing process.

[0044] According to another embodiment of the present application, Figures 4A to 4B A method for forming a template mask is shown. Figure 4A As shown, the template member 413 and the support member 415 can be formed separately. In some embodiments, the template member 413 can be formed by an etching process or a laser cutting process. In some embodiments, the template member can be etched by a chemical etching or dry etching process. In some embodiments, the template member can be etched by a laser cutting process. The laser cutting process can be automatically controlled using a computer or similar electronic device, so the size and depth of the etched portion can be accurate. The support member 415 can be formed using a similar process such as laser cutting or any other suitable process. Then as shown in FIG. Figure 4B As shown, the template member 413 and the support member 415 can be aligned with each other and attached to each other. For example, an adhesive material can be used to connect the two together.

[0045] although Figures 1A to 1C and Figures 2A to 2E Some embodiments are shown that combine two template printing processes for forming two groups of solder bumps respectively. In some alternative embodiments such as the following, a portion of the solder bumps on the substrate can be enhanced by depositing an additional amount of fluid material thereon, which can also reduce or avoid non-wetting defects.

[0046] According to one embodiment of the present application, Figure 5A and 5B A substrate 501 with a stencil mask 511 attached is shown respectively. In particular, Figure 5A is a cross-sectional view of substrate 501 before a fluid material is deposited onto substrate 501 through stencil mask 511 . Figure 5B is a cross-sectional view of substrate 501 after a fluid material is deposited onto substrate 501 through stencil mask 511 .

[0047] like Figure 5A and Figure 5A As shown, Figures 1A to 1C Unlike the embodiment shown in , solder bumps are formed in the peripheral region 513a and the central region 513b of the substrate 501. However, since the aforementioned problem of die warpage may occur in the subsequent bonding process or any other similar problem, it is desirable to apply a fluid material such as flux or other material that can improve the wetting of the solder bumps in the peripheral region 513 of the substrate 501. Therefore, using a material similar to Figures 1A to 1C 5. The selective stencil mask 511 of the stencil mask 111 shown in FIG. The stencil mask 511 includes a stencil member 513 and a support member 515. The stencil member 513 includes at least one printing area aligned with the peripheral area 513a and a non-porous blocking area aligned with the central area 513b. Each printing area has an array of holes 517 that allow fluid material to flow therethrough.

[0048] like Figure 5B As shown, after the selective template printing process is performed on the substrate 501 using the template mask 511, a fluid material 507 such as flux can flow through the holes 517 in the peripheral area 513a and deposit on the solder bumps 505 formed in the previous printing process to ensure that there is enough flux on the solder bumps 505 in the peripheral area 513a of the substrate 501. In this way, in the subsequent bonding process between the substrate 501 and another substrate (not shown), the bumps 505 with additional flux in the peripheral area 513a can be well wetted with the solder bumps on the other substrate, even if the other substrate may be warped at its periphery during, for example, a reflow process. It is understood that the amount of fluid materials such as flux printed during the printing process can be adjusted or controlled according to actual needs.

[0049] According to an embodiment of the present application, Figures 6A to 6EA process for forming a bond between two substrates is shown. In some embodiments, the process can be used in a process for forming a semiconductor package including two substrates.

[0050] As shown Fig. 6A As shown, a first substrate 601 may be provided, which may have solder bumps 605 in both the central region and the peripheral region of the substrate 601. For example, a plurality of solder bumps 605 may be formed using a first stencil printing process, which may allow a fine pitch of 90 μm or even less.

[0051] Afterwards, if Figure 6B As shown, a second template printing process may be performed on the first substrate 601 to deposit a fluid material such as flux on a portion of the solder bump 605 in the peripheral region of the substrate 601. In this embodiment, the second template printing process may use a reference Figures 1A to 1C or Figures 5A to 5B The second stencil printing process can be implemented using a stencil mask as shown in the embodiment of . Because it is a different process from the first stencil printing process, the second stencil printing process can be implemented using a different configuration. For example, the aperture size and spacing of the stencil mask may be different from that of the first stencil printing process. The stencil mask used in the second stencil printing process provides a gap that can accommodate the solder bumps 605 in the central area of ​​the substrate 601 and protect them from damage and contamination during the second stencil printing process.

[0052] Next, if Figure 6C As shown, a second substrate 621 may be provided. The second substrate 621 may have a solder bump 623, which corresponds to and faces the solder bump 605 on the substrate 601. The second substrate 621 may be joined to the first substrate 601 via the solder bumps 605 and 623. In some embodiments, the solder bump 623 on the second substrate 621 may be deposited with flux 625, for example, using a dipping process. In addition, as shown in FIG. Fig.6D As shown, the second substrate 621 is placed on the first substrate 601, and the solder bumps 623 are aligned and contacted with the corresponding solder bumps 605, and are filled with flux 607 and flux 625. The flux, especially the additional flux 607 in the peripheral area of ​​the substrate, can improve the wetting between the solder bumps on the substrates 601 and 621, thereby reducing the defects of the formed package.

[0053] Next, if Fig. 6E As shown, a reflow process can be performed on the connected substrates 601 and 621 to reflow the fluid material between them. It can be understood that even if the upper substrate 621 is warped at its periphery due to heat, the solder bumps at the peripheries of the two substrates 601 and 621 will not be disconnected or insufficiently wetted because there is enough flux to maintain wetting.

[0054] Understandably, Figures 6A to 6E The process shown in is only exemplary and modifications, changes or additions may be made to the process. Figure 6B In the embodiment, substrate 601 may have other areas that may require additional flux for solder bumps that have been formed therein, i.e., areas where non-wetting may occur during subsequent bonding processes. Furthermore, in alternative embodiments, additional fluid material may be deposited on substrate 601 prior to base-level deposition of solder bumps 605, such as Fig. 6A shown.

[0055] The discussion herein includes a number of illustrative drawings that show portions of a stencil mask and a stencil printing method based on the stencil mask. For clarity of illustration, these figures do not show all aspects of each example component. Any example component and / or method provided herein may share any or all features with any or all other components and / or methods provided herein.

[0056] Various embodiments have been described herein with reference to the accompanying drawings. However, it is apparent that various modifications and changes may be made thereto, and additional embodiments may be implemented without departing from the broader scope of the invention as set forth in the appended claims. In addition, other embodiments will be apparent to those skilled in the art by considering the specification and practice of one or more embodiments of the invention disclosed herein. Therefore, the present application and the embodiments herein are intended to be considered merely exemplary, with the true scope and spirit of the invention being indicated by the list of the appended exemplary claims.

Claims

1. A template mask for printing a fluid material onto a substrate, characterized in that The template mask comprises: A template component, comprising: at least one printing region, wherein each printing region has an array of holes that allow the fluid material to flow through and be deposited onto a substrate; and a barrier region for preventing fluid material from flowing therethrough; and A support member is attached to the template member and is configured to contact the substrate and create a gap between the template member and the substrate when a template mask is placed on the substrate.

2. The template mask according to claim 1, characterized in that: The at least one printing area is located at a peripheral position of the template member.

3. The template mask according to claim 1, characterized in that: The blocking area is located at the center of the template member.

4. The template mask according to claim 1, characterized in that: The support member includes a plurality of support bars or support pins.

5. The template mask according to claim 1, characterized in that: The template mask is formed by: providing a template mask substrate; forming a first photoresist pattern having a first opening on a template mask substrate; filling a first electroplating material into the first opening of the first photoresist pattern; forming a second photoresist pattern having a second opening on the first photoresist pattern; filling the second opening of the second photoresist pattern with a second electroplating material; and The first and second photoresist patterns are removed from the template mask substrate.

6. A template printing method comprising: providing a substrate comprising at least one printing site; A template mask is provided, wherein the template mask comprises: a template member including at least one printed area, each printed area having an array of holes for allowing a fluid material to flow therethrough, and a blocking area for preventing the fluid material from flowing therethrough; and a support member attached to the formwork member; placing the stencil mask on the substrate, creating a gap between the stencil member and the substrate by the support member, and aligning the at least one printing area with the at least one printing location, respectively; and The fluid material is deposited onto the substrate through the at least one printing area such that the fluid material flows through the at least one array of holes onto at least one printing location.

7. The method according to claim 6, characterized in that After depositing the fluid material onto the substrate, the method further comprises: The stencil mask is removed from the substrate.

8. The method according to claim 6, characterized in that The at least one printing portion is located at a peripheral position of the substrate, and the at least one printing area is located at a peripheral position of the template member.

9. The method according to claim 8, characterized in that The blocking area is located at the center of the template member.

10. The method according to claim 6, characterized in that The substrate also includes solder bumps, and the solder bumps are formed using another stencil printing process with another stencil mask.

11. The method according to claim 10, characterized in that Solder bumps in the print area are deposited with fluid material flowing through the at least one array of holes.

12. The method according to claim 6, characterized in that The pitch of the solder bumps in the printing area is greater than the pitch of the solder bumps outside the printing area.

13. The method according to claim 6, characterized in that After the depositing step, the size of the solder bumps in the printed area is larger than the size of the solder bumps outside the printed area.

14. The method according to claim 6, characterized in that The fluid material includes flux.

15. A method for forming a semiconductor package, comprising: Providing a first substrate and a second substrate; forming a first plurality of solder bumps in a first region of the first substrate using a first stencil mask; forming a second plurality of solder bumps in a second region of the first substrate using a second stencil mask; forming solder bumps on the second substrate; aligning a first plurality of solder bumps and a second plurality of solder bumps on the first substrate with solder bumps on the second substrate to connect the first substrate and the second substrate; and The first and second pluralities of solder bumps on the first substrate and the solder bumps on the second substrate are reflowed.

16. The method according to claim 15, characterized in that The first area is located at a central position of the first substrate, and the second area is located at a peripheral position of the first substrate.

17. The method according to claim 15, characterized in that The first plurality of solder bumps has a smaller pitch than the second plurality of solder bumps.

18. The method according to claim 15, characterized in that The first plurality of solder bumps have a size smaller than a size of the second plurality of solder bumps.

19. The method according to claim 14, characterized in that The second template mask comprises: a stencil member comprising a printed area having an array of holes, the printed area allowing solder material to flow therethrough and aligned with the second area of ​​the first substrate when the second stencil mask is placed on the first substrate; a blocking area for preventing solder from flowing therethrough when the second stencil mask is placed on the first substrate and aligned with the first area of ​​the first substrate; and A support member is attached to the template member and is configured to contact the first substrate and create a gap between the second template member and the first substrate when a template mask is placed on the substrate.

20. A method for forming a semiconductor package, comprising: Providing a first substrate and a second substrate; forming a first plurality of solder bumps in a first region of the first substrate and forming a second plurality of solder bumps in a second region of the first substrate using a first stencil mask; depositing flux onto the second plurality of solder bumps using a second stencil mask; forming solder bumps on the second substrate; aligning a first plurality of solder bumps and a second plurality of solder bumps on the first substrate with solder bumps on the second substrate to connect the first substrate and the second substrate; and The first and second pluralities of solder bumps on the first substrate and the solder bumps on the second substrate are reflowed.

21. The method of claim 20, wherein: The first area is located at a central position of the first substrate, and the second area is located at a peripheral position of the first substrate.

22. The method according to claim 20, characterized in that The first plurality of solder bumps has a pitch smaller than a pitch of the second plurality of solder bumps.

23. The method according to claim 20, characterized in that The first plurality of solder bumps have a size smaller than a size of the second plurality of solder bumps.

24. The method according to claim 20, characterized in that The second template mask comprises: a stencil member comprising a printed area having an array of holes, the printed area allowing flux to flow therethrough and aligned with the second area of ​​the first substrate when the second stencil mask is placed on the first substrate; and a blocking area for preventing flux from flowing therethrough when the second stencil mask is placed on the first substrate and aligned with the first area of ​​the first substrate; and A support member is attached to the template member and is configured to contact the first substrate and create a gap between the second template member and the first substrate when a template mask is placed on the substrate.

25. The method of claim 20, before aligning the first plurality of solder bumps and the second plurality of solder bumps on the first substrate with solder bumps on the second substrate to connect the first substrate and the second substrate; the method further comprising: A solder flux is formed on the solder bumps on the second substrate using a dipping process.

26. A method for forming a stencil mask, comprising: providing a substrate; forming a first photoresist pattern having a first opening on the substrate; filling a first electroplating material into the first opening of the first photoresist pattern; forming a second photoresist pattern having a second opening on the first photoresist pattern; filling a second electroplating material in the second opening of the second photoresist pattern; and The first photoresist pattern and the second photoresist pattern on the substrate are removed.