A wafer metallization method
Through the wafer metallization method of pretreatment and substrate laying on the chip surface, the chip surface electroplating layer adaptation problem in the prior art is solved, the metal layer thickness and process stability are improved, and the finished product safety is achieved and productivity.
Patent Information
- Application Number
- CN202411231067.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-04
AI Technical Summary
The existing chip surface only has one aluminum layer electroplated to the aluminum wire bonding process. The bonding interface layering phenomenon is the copper wire bonding process. The copper wire bonding process requires specific equipment and sintering equipment, and the finished product safety and production efficiency are low.
A wafer metallization method is adopted, which involves pretreatment before applying solder paste, such as mounting a flexible printing mold on the top of the wafer and removing the mold after sintering; laying the substrate before pressurization after drying, and After sintering, the substrate is removed, and these steps are used to improve the thickness and process stability of the metal layer and reduce the risk of use.
It improves the yield, safety and reliability of the finished product, significantly improves the flow performance and heat dissipation performance of the chip, increases production efficiency, and reduces production costs.
Smart Images

Figure CN118737861B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor technology, and in particular to a wafer metallization method. Background Art
[0002] In recent years, with the rapid development of electric vehicles, higher requirements have been put forward for long driving range and ultra-fast charging of vehicles. The power density, operating temperature and current-carrying capacity of power electronic modules have also increased accordingly, resulting in increasingly complex reliability requirements. Packaging has become the key to improving reliability and performance. However, existing packaging processes (such as solder welding processes) have reached their application limits, and new packaging processes and materials are urgently needed.
[0003] The semiconductor device (chip) and substrate connection technology usually uses specific connection materials to package the electronic components and substrate together to achieve the electrical performance of the electronic components. Obviously, the typical chip and substrate interconnection structure includes electronic components, connection materials, substrate, lead frame (optional), and external circuit. GBT (i.e., high-temperature, high-power electronic device) chips and chip electrode terminals, IGBT chip electrode terminals and diode chips, and chip electrode terminals and insulating linings are usually electrically connected through wire bonding technology, and the chips are interconnected through bonding wires to form a loop. Wire bonding is one of the main ways to achieve electrical interconnection inside IGBT power devices.
[0004] At present, commonly used bonding wires include aluminum wire, gold wire, silver wire, copper wire, aluminum strip, copper sheet and aluminum-clad copper wire. Among them, aluminum wire bonding is the most widely used chip interconnection technology in industry. The aluminum wire bonding technology is mature and inexpensive. Compared with aluminum wire bonding, copper wire bonding can improve the current capacity, electrical conductivity and thermal conductivity of electronic components, thereby extending the life. However, copper is relatively hard, and greater ultrasonic power and pressure are required during the bonding process to cause the copper wire to undergo plastic deformation and then connect to the bottom metal layer. The existing chip surface is only electroplated with a layer of aluminum, which is suitable for the aluminum wire bonding process. If the copper wire is directly bonded, the chip will be cratered. The existing process is to achieve bonding copper wire in a combination of copper foil and welding layer, but there is a bonding interface stratification phenomenon, and the copper wire bonding process requires specific equipment mounting and sintering equipment to complete the bonding with the chip surface; and the finished product is not safe. In addition, this method requires the chip to be solderable, that is, gold-plated or silver-plated, and is only applicable to a single packaged chip rather than the wafer level, so the production efficiency is low. Summary of the invention
[0005] In view of the shortcomings of the prior art described above, the present invention provides a wafer metallization method to solve the above-mentioned existing chip surface only electroplating a layer of aluminum layer, adapted to the aluminum wire bonding process, there is a bonding interface stratification phenomenon, and the copper wire bonding process requires specific equipment mounting and sintering equipment to complete the metal processing process; in addition, the method requires the chip to be solderable, that is, gold-plated or silver-plated, and is only for a single packaged chip, not a wafer level, and the production efficiency is low; in addition, the safety of the finished product is not good, and the withstand voltage value is high; there are also solder pastes, which are sequentially applied through solder paste, drying, pressurization and sintering processes, and then the metal solder in the solder paste is coated on the chip made of the wafer. However, the finished product obtained in this way has technical problems such as poor safety, high withstand voltage value, and low production efficiency.
[0006] After studying the relevant technology, the inventor found that in the prior art, the copper wire bonding process requires specific equipment mounting and sintering equipment to complete the bonding with the chip surface, and the welding layer is hard and non-sticky. Therefore, it often shifts when it is mounted on the chip surface, resulting in the presence of welding layers in other parts of the chip, resulting in a higher withstand voltage value of the finished product and poor safety.
[0007] To achieve the above objectives, the scheme of this application is as follows:
[0008] The present invention provides a wafer metallization method, wherein the wafer is provided with a plurality of bonding pads (referred to as pad areas) for bonding, and the wafer metallization method sequentially comprises the steps of applying solder paste, drying, pressing and sintering, and further comprises: before applying solder paste, performing pretreatment, wherein the pretreatment comprises mounting a first printing mold on the top of the wafer, and removing the first printing mold after sintering, wherein the first printing mold is provided with a plurality of first windows corresponding to the bonding pads one by one, and the area of the first windows is smaller than the area of the bonding pads;
[0009] And / or, it also includes: after drying and before pressurizing, laying a first substrate on the bottom of the wafer, and removing the first substrate after sintering.
[0010] It should be noted that, in the present application, the term "wafer" refers to a wafer with a metal-plated surface or a wafer without a metal-plated surface, and the metal here includes but is not limited to: gold, silver, etc.
[0011] Optionally, the first printing mold is a flexible film.
[0012] Optionally, the material of the flexible film is selected from at least one of polyimide resin (PI for short in English), polytetrafluoroethylene resin, polypropylene resin, polyethylene terephthalate resin (PET for short in English) and polyamide.
[0013] Optionally, the thickness of the flexible film is 100-200 μm, preferably 120-200 μm.
[0014] Optionally, the wafer metallization method further comprises:
[0015] After the first printing mold is mounted on the top of the wafer and before the solder paste is applied, a second printing mold is laid on the first printing mold, and the second printing mold is provided with a plurality of second windows corresponding to the bonding pads one by one, and the area of the second windows is smaller than the area of the first windows.
[0016] Optionally, the second printing mold is a mesh structure.
[0017] Optionally, the thickness of the second printing mold is 100-200 μm, preferably 120-200 μm.
[0018] In the present application, the material of the second printing mold includes but is not limited to: steel, nickel, aluminum, resin, acrylonitrile-styrene-butadiene copolymer (ABS for short), polycarbonate, rubber, silicone, polyester, nylon, silk, etc.
[0019] Optionally, after the first printing mold is mounted on the wafer, the wafer is placed in a printing tool with a second substrate laid on the bottom.
[0020] Optionally, the second substrate has a thickness of 100-200 μm, preferably 120-200 μm.
[0021] Optionally, the material of the second substrate is selected from at least one of polyimide resin (PI for short in English), polytetrafluoroethylene resin (PTFE), polyvinylidene fluoride resin (PVDF), polysulfone resin (PSU), polyethersulfone (PES), polypropylene resin, polyethylene terephthalate resin (PET for short in English), polyetheretherketone (PEEK) and polyamide.
[0022] It should be noted that, in the present application, the area of the second substrate is larger than the area of the bottom of the wafer.
[0023] Optionally, the solder paste includes metal solder and flux.
[0024] In the present application, metal solder includes but is not limited to: copper solder, silver solder, silver-copper solder, tin-silver solder, tin-copper solder, copper-aluminum solder, tin-lead solder, tin-lead-silver solder, tin-lead-bismuth solder, tin-silver-copper solder, etc.
[0025] In the present application, the soldering flux may include a solvent, a surfactant (if necessary), an activator (if necessary), a preservative (if necessary), a co-solvent (if necessary), a film-forming agent (if necessary), and the like.
[0026] Optionally, the drying temperature is 100-150°C, preferably 120-150°C.
[0027] Optionally, the drying time is 5-30 min, preferably 10-30 min.
[0028] Optionally, the material of the first substrate is selected from at least one of polyimide resin (PI for short in English), polytetrafluoroethylene resin (PTFE), polyvinylidene fluoride resin (PVDF), polysulfone resin (PSU), polyethersulfone (PES), polypropylene resin, polyethylene terephthalate resin (PET for short in English), polyetheretherketone (PEEK) and polyamide.
[0029] Optionally, the thickness of the first substrate is 100-1000 μm, preferably 100-500 μm, and more preferably 300-500 μm.
[0030] Optionally, the pressure is increased to 2-10 MPa, preferably 3-10 MPa.
[0031] Optionally, the pressurization duration is 1-5 min, preferably 2-5 min.
[0032] Optionally, the sintering temperature is 250-350°C, preferably 260-350°C.
[0033] Optionally, the sintering time is 20-60 min, preferably 25-60 min.
[0034] Beneficial effects of the present invention:
[0035] The present invention improves the yield, practicality and reliability of the finished product.
[0036] The present invention can prevent scratches on the wafer surface and paste overflow during the printing process by mounting the first printing mold on the bottom of the wafer, thereby increasing the yield (scratches result in poor appearance, and paste overflow results in poor electrical parameters) and improving the safety of the finished product.
[0037] The present invention can increase the thickness of the metal layer, reduce the use risk, and further improve the process stability and increase the yield by laying the second printing mold on the first printing mold after the first printing mold is mounted on the top of the wafer and before the solder paste is applied.
[0038] The present invention can relieve stress by laying a second substrate between a printing tool and the bottom of a wafer, thereby avoiding wafer cracking caused by the printing and pressurizing process.
[0039] The present invention can relieve stress by laying the first substrate on the bottom of the wafer, thereby avoiding wafer cracking caused by printing and pressurization processes.
[0040] The present invention significantly improves the flow performance and heat dissipation performance of the chip made from the finished product and the reliability in the subsequent packaging process.
[0041] In the present application, metallization is performed directly on the wafer rather than the chip, thereby improving production efficiency.
[0042] In the present application, the printing mold is disposable. The present application sets the material of the first printing mold to at least one of polyimide resin (PI for short in English), polytetrafluoroethylene resin (PTFE), polyvinylidene fluoride resin (PVDF), polysulfone resin (PSU), polyethersulfone (PES), polypropylene resin, polyethylene terephthalate resin (PET for short in English), polyetheretherketone (PEEK) and polyamide, and sets the material of the second printing mold to nickel, aluminum, resin, acrylonitrile-styrene-butadiene copolymer (ABS for short in English), polycarbonate, rubber, silicone, polyester, nylon, silk, etc., which can reduce production costs and improve economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 Schematic diagram of wafer, printing tooling and printing pattern.
[0044] Figure 2 This is a picture of the product after bonding in Example 1;
[0045] Figure 3 This is the product picture of the control group 1 after bonding. DETAILED DESCRIPTION
[0046] The following will describe the embodiments of the present invention with reference to the accompanying drawings and preferred embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be understood that the preferred embodiments are only for illustrating the present invention, not for limiting the scope of protection of the present invention.
[0047] It should be noted that the illustrations provided in the following embodiments are only schematic illustrations of the basic concept of the present invention, and thus the drawings only show components related to the present invention rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.
[0048] An embodiment of the present invention provides a wafer metallization method, wherein the wafer is provided with a plurality of bonding pads for bonding. The wafer metallization method sequentially comprises the steps of applying solder paste, drying, pressing and sintering. Before applying the solder paste, the method further comprises: performing pretreatment before applying the solder paste, the pretreatment comprising mounting a first printing mold on the top of the wafer, and removing the first printing mold after sintering, the first printing mold is provided with a plurality of first windows corresponding to the bonding areas one by one, the area of the first windows is smaller than the area of the bonding pads, the first printing mold is a flexible film with a thickness of 100-200 μm, and the material of the flexible film is selected from at least one of polyimide resin, polytetrafluoroethylene resin, polypropylene resin, polyethylene terephthalate resin and polyamide;
[0049] Then, the wafer is placed in a printing tool with a second substrate on the bottom, wherein the material of the second substrate is selected from at least one of polyimide resin, polytetrafluoroethylene resin, polypropylene resin, polyethylene terephthalate resin and polyamide, and the thickness of the second substrate is 100-200 μm;
[0050] And / or, after drying and before pressurization, the method further comprises: laying a first substrate on the bottom of the wafer, and removing the first substrate after sintering, wherein the material of the first substrate is selected from at least one of polyimide resin, polytetrafluoroethylene resin, polypropylene resin, polyethylene terephthalate resin and polyamide, and the thickness of the first substrate is 100-1000 μm;
[0051] The drying temperature is 100-150℃ and the drying time is 5-30min;
[0052] Pressurize to 2-10MPa for 1-5min;
[0053] The sintering temperature is 250-350°C, and the sintering time is 20-60 minutes.
[0054] In another embodiment of the present invention, after the first printing mold is mounted on the top of the wafer and before the solder paste is applied, it also includes: laying a second printing mold on the first printing mold, the second printing mold has a plurality of second windows corresponding to the bonding areas one by one, the area of the second window is smaller than the area of the first window, and the thickness of the second printing mold is 100-200μm.
[0055] In the following description, numerous details are discussed to provide a more thorough explanation of embodiments of the present invention; however, it is apparent to one skilled in the art that embodiments of the present invention may be practiced without these specific details.
[0056] Example 1
[0057] A wafer metallization method, the specific steps are as follows:
[0058] A first printing mold is mounted on the top of a wafer (the wafer refers to a wafer with a gold-plated surface, that is, a wafer with a solderable surface, and the wafer is provided with a plurality of bonding pads (i.e., pad areas) for bonding, the first printing mold is provided with a plurality of first windows corresponding to the pad areas one by one, the area of the first windows is smaller than the area of the pad areas, the first printing mold is selected from a PI film (i.e., a polyimide film), and the thickness of the first printing mold is 150 μm;
[0059] like Figure 1 As shown, the wafer is then placed in a printing tool, a second substrate is laid between the printing tool and the bottom of the wafer, the thickness of the second substrate is 150 μm, and the material of the second substrate is selected from PET film (i.e. polyester resin film);
[0060] Copper solder paste (i.e., the metal solder is copper, the flux is a solvent, and the solder paste is commercially available) is evenly coated on the first printing mold, and the wafer is placed in a 120° C. oven and dried in a nitrogen atmosphere for 15 minutes;
[0061] Lay the first substrate on the bottom of the wafer. The material of the first substrate is selected from PI film. The area of the first substrate is slightly larger than the area of the wafer. The thickness of the first substrate is 500 μm. The applied pressure is 5 MPa. The duration of the applied pressure is 1 min.
[0062] The wafer was transferred to a sintering device and kept at 350°C in a formic acid atmosphere for 30 minutes to obtain a wafer with a pre-coated copper layer on the top (the thickness of the copper layer was 80 μm, tested by a thickness detector). After sintering, the first printing mold and the first substrate were removed, and the bottom of the wafer was encapsulated with a blue film (commercially available) and a patch ring (commercially available).
[0063] Example 2
[0064] A wafer metallization method, the specific steps are as follows:
[0065] A first printing mold is mounted on the top of a wafer (the wafer is a wafer with a silver-plated surface, i.e., a wafer with a solderable surface, and the wafer is provided with a plurality of bonding pads (i.e., pad areas) for bonding), the first printing mold is provided with a plurality of windows corresponding to the pad areas one by one, the area of the first window is smaller than the area of the pad area, the first printing mold is selected from a PI film (i.e., a polyimide film), and the thickness of the first printing mold is 200 μm;
[0066] like Figure 1 As shown, the wafer is then placed in a printing tool, and a second substrate is laid between the printing tool and the bottom of the wafer. The thickness of the second substrate is 200 μm, and the material of the second substrate is selected from PET film (i.e. polyester resin film);
[0067] Copper solder paste (i.e., the metal solder is copper, the flux is a solvent, and the solder paste is commercially available) is evenly coated on the first printing mold, and the wafer is placed in a 150° C. oven and dried in a nitrogen atmosphere for 20 minutes;
[0068] Lay the first substrate on the bottom of the wafer. The material of the first substrate is selected from PI film. The area of the first substrate is slightly larger than the area of the wafer. The thickness of the first substrate is 300 μm. The applied pressure is 5 MPa. The duration of the applied pressure is 1 min.
[0069] The wafer was transferred to a sintering device and kept at 300°C in a formic acid atmosphere for 60 minutes to obtain a wafer with a pre-coated copper layer on the top (the thickness of the copper layer was 120 μm, tested by a thickness detector). After sintering, the first printing mold and the first substrate were removed, and the bottom of the wafer was encapsulated with a blue film (commercially available) and a patch ring (commercially available).
[0070] Example 3
[0071] A wafer metallization method, the specific steps are as follows:
[0072] A first printing mold is mounted on the top of a wafer (the wafer is a wafer with a gold-plated surface, i.e., a wafer with a solderable surface, and the wafer is provided with a plurality of bonding pads (i.e., pad areas) for bonding), the first printing mold is selected from a PI film (i.e., a polyimide film), the first printing mold is provided with a plurality of windows corresponding to the pad areas one by one, the area of the first window is smaller than the area of the pad area, and the thickness of the first printing mold is 50 μm;
[0073] Subsequently, a second printing mold is laid on the first printing mold. The second printing mold is provided with a plurality of second windows corresponding to the bonding areas one by one. The area of the second windows is slightly smaller than the area of the first windows. The thickness of the second printing mold is 450 μm. The second printing mold uses a steel mesh.
[0074] Next, the wafer is placed in a printing tool, and a second substrate is laid between the printing tool and the bottom of the wafer. The thickness of the second substrate is 200 μm, and the material of the second substrate is selected from PET film (i.e. polyester resin film);
[0075] Copper solder paste (i.e., the metal solder is copper, the flux is a solvent, and the solder paste is commercially available) is evenly coated on the first printing mold, and the wafer is placed in a 120° C. oven and dried in a nitrogen atmosphere for 15 minutes;
[0076] Lay the first substrate on the bottom of the wafer. The material of the first substrate is selected from PI film. The area of the first substrate is slightly larger than the area of the wafer. The thickness of the first substrate is 500 μm. The applied pressure is 5 MPa. The duration of the applied pressure is 1 min.
[0077] The wafer was transferred to a sintering device and kept at 350°C in a formic acid atmosphere for 30 minutes to obtain a wafer with a pre-coated copper layer on the top (the thickness of the copper layer was 200 μm, tested by a thickness detector). After sintering, the first printing mold and the first substrate were removed, and the bottom of the wafer was encapsulated with a blue film (commercially available) and a patch ring (commercially available).
[0078] Example 4
[0079] A wafer metallization method, the specific steps are as follows:
[0080] A first printing mold is mounted on the top of a wafer (the wafer is an aluminum-plated wafer, that is, a wafer whose surface cannot be connected to copper paste or silver paste, and the wafer is provided with a plurality of bonding pads (i.e., pad area) for bonding), the first printing mold is selected from a PI film (i.e., a polyimide film), the first printing mold is provided with a plurality of windows corresponding to the pad area, the area of the first window is smaller than the area of the pad area, and the thickness of the first printing mold is 50 μm;
[0081] Subsequently, a second printing mold is laid on the first printing mold. The second printing mold is provided with a plurality of second windows corresponding to the bonding areas one by one. The area of the second windows is slightly smaller than the area of the first windows. The thickness of the second printing mold is 450 μm. The second printing mold uses a steel mesh.
[0082] Next, the wafer is placed in a printing tool, and a second substrate is laid between the printing tool and the bottom of the wafer. The thickness of the second substrate is 200 μm, and the material of the second substrate is selected from PET film (i.e. polyester resin film);
[0083] Evenly apply aluminum-copper solder paste (i.e., the metal solder is copper, the flux is solvent, and the solder paste is commercially available) on the first printing mold, and place the wafer in a 120° C. oven and dry it in a nitrogen atmosphere for 20 minutes;
[0084] Laying a first substrate on the bottom of the wafer, the material of the first substrate is selected from PI film, the area of the first substrate is slightly larger than the area of the wafer, the thickness of the first substrate is 500 μm, the pressure applied is 5 MPa, and the duration of the applied pressure is 3 minutes;
[0085] The wafer was transferred to a sintering device and kept at 350°C in a formic acid atmosphere for 60 minutes to obtain a wafer with a pre-coated copper layer on the top (the thickness of the copper layer was 200 μm, tested by a thickness detector). After sintering, the first printing mold and the first substrate were removed, and the bottom of the wafer was encapsulated with a blue film (commercially available) and a patch ring (commercially available).
[0086] Comparative Example 1
[0087] The difference between this comparative example and Example 1 is that the first printing mold is not mounted on the top of the wafer.
[0088] Comparative Example 2
[0089] The difference between this comparative example and Example 1 is that the second substrate is not laid between the printing tooling and the bottom of the wafer.
[0090] During the process, the wafer cracked.
[0091] Comparative Example 3
[0092] The difference between this comparative example and Example 1 is that the first substrate is not laid on the bottom of the wafer.
[0093] During the process, the wafer cracked.
[0094] Comparative Example 4
[0095] The difference between this comparative example and Example 4 is that the thickness of the first printing mold is 500 μm, the second printing steel mesh is not laid on the first printing mold, and an attempt is made to bond the copper bonding wire to the metal layer on the top of the wafer.
[0096] During the process, the copper bonding wire cannot bond to the metal layer on top of the wafer due to the uneven surface of the metal layer on the wafer.
[0097] Performance Testing
[0098] The withstand voltage values of the finished products obtained in Examples 1-4, i.e., Comparative Example 1, were tested, and the results are shown in Table 1;
[0099] The method for testing the withstand voltage value is as follows: place the wafer on a high-voltage probe station, locate each pole of the chip through a microscope, start the test from 100V, increase 100V each time, record the current, and once the current exceeds the preset breakdown threshold (such as 1mA), this voltage value is the breakdown voltage;
[0100] The finished products of Examples 1-4 and Comparative Example 1 were cut into chips, and the cut chips were bonded to copper wires respectively. A control group 1 was set up. The control group 1 was: DTS (i.e., copper foil with pre-coated silver paste) was directly bonded to the copper wire, and the appearance of the bonded products was observed. The bonded products of Example 1 were as follows: Figure 2 As shown;
[0101] The push-pull force of the bonded product was tested using a push-pull force testing machine. The results are shown in Table 1.
[0102] Table 1 Test results
[0103]
[0104] It can be seen from Table 1 that the withstand voltage values of the finished products obtained in Examples 1-4 are ≥ 1200 V. This result shows that the present invention improves the safety of the finished products.
[0105] As shown in Table 1, compared with Comparative Example 1 (the first printing mold is not mounted on the bottom of the wafer), the withstand voltage value of Example 1 (the first printing mold is mounted on the bottom of the wafer) is significantly increased. This result shows that the present invention can prevent scratches on the wafer surface and paste overflow during the printing process by mounting the first printing mold on the bottom of the wafer, thereby increasing the yield (scratches have a poor appearance, and paste overflow causes poor electrical parameters) and improving the safety of the finished product.
[0106] From the above embodiments and comparative examples, it can be seen that in comparative example 2 (no second substrate was laid between the printing tool and the bottom of the wafer), the wafer was broken during the preparation process, while the wafer of embodiment 1 (a second substrate was laid between the printing tool and the bottom of the wafer, and the second substrate was specifically a PET film) was successfully metallized. This result shows that the present invention can relieve stress by laying a second substrate between the printing tool and the bottom of the wafer, thereby avoiding wafer cracking caused by the printing and pressurization process.
[0107] It can be seen from the above embodiments and comparative examples that, compared with comparative example 3 (the first substrate is not laid on the bottom of the wafer), the wafer of embodiment 1 (the first substrate is laid on the bottom of the wafer) is successfully metallized. This result shows that the present invention can relieve stress by laying the first substrate on the bottom of the wafer, thereby avoiding wafer cracking caused by the printing and pressurization process.
[0108] The finished products of Examples 1-4 were cut into chips respectively, and the maximum junction temperature of the chips was tested. The results are shown in Table 2.
[0109] The test method of the maximum junction temperature of the chip is as follows: using comsol software to establish bonding models of chips cut from wafers treated in Examples 1-4 and Comparative Example 1 and different bonding wires, and using the same software to establish a bonding model of chips cut from untreated wafers from the same source as Example 1 and aluminum wires as Control Group 2, wherein the chip thickness is 0.12 μm, the solder layer thickness at the bottom of the chip is 0.1 μm, the material is tin, the substrate is made of copper, the difference at the top of the chip is whether a metal layer is used, the bonding wire material is copper or aluminum, and the bonding wire diameter is 15 mil;
[0110] The chip is set as a heat source and operates continuously with a fixed loss of 50W. The copper substrate is set as a convection heat transfer boundary, and the other surfaces are insulation surfaces. Comsol software is used to calculate the maximum surface temperature of the chip (i.e., the maximum junction temperature of the chip).
[0111] Table 2 Chip maximum junction temperature test results
[0112]
[0113] As shown in Table 2, the maximum junction temperature of the chips made from the finished products of Examples 1-4 is significantly reduced compared to Control Group 2. This result shows that the present invention significantly improves the flow performance, heat dissipation performance and reliability of the chips made from the finished products in the subsequent packaging process.
[0114] It can be seen from the above embodiments and comparative examples that in the process of comparative example 4 (the thickness of the first printing mold is 500μm, and the second printing mold is not laid on the first printing mold), the copper bonding wire cannot be bonded to the metal layer on the top of the wafer due to the uneven metal layer on the surface of the wafer, while the bonding wire in embodiment 4 (the second printing mold is laid on the first printing mold, the thickness of the first printing mold is 50μm, and the thickness of the second printing mold is 450μm) can be bonded to the metal layer on the top of the wafer. This result shows that the present invention can increase the thickness of the metal layer, reduce the use risk, and thus improve the process stability and increase the yield by laying the second printing mold on the first printing mold before applying the solder paste.
[0115] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present invention. Therefore, all equivalent modifications or changes made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for metallizing a wafer, wherein the wafer is provided with a plurality of bonding pads for bonding, and the method for metallizing the wafer sequentially comprises the steps of applying solder paste, drying, pressing and sintering, It is characterized in that Also includes: Before applying the solder paste, pretreatment is performed, the pretreatment comprising mounting a first printing mold on the top of the wafer and removing the first printing mold after sintering, the first printing mold is provided with a plurality of first windows corresponding to the bonding pads one by one, the area of the first windows is smaller than the area of the bonding pads, the first printing mold is a flexible film, the material of the flexible film is selected from at least one of polyimide resin, polytetrafluoroethylene resin, polyvinylidene fluoride resin, polysulfone resin, polyethersulfone, polypropylene resin, polyethylene terephthalate resin, polyetheretherketone and polyamide, and the thickness of the flexible film is 100-200 μm; And / or, it also includes: after drying and before pressurizing, laying a first substrate on the bottom of the wafer, and removing the first substrate after sintering.
2. The method for metallizing a wafer as claimed in claim 1, It is characterized in that Also includes: After the first printing mold is mounted on the top of the wafer and before the solder paste is applied, a second printing mold is laid on the first printing mold, and the second printing mold is provided with a plurality of second windows corresponding to the bonding pads one by one, and the area of the second windows is smaller than the area of the first windows.
3. The method for metallizing a wafer as claimed in claim 2, It is characterized in that The second printing mold is a mesh structure.
4. The method for metallizing a wafer as claimed in claim 1, It is characterized in that After mounting the first printing mold on the wafer, the wafer is placed in a printing tool with a second substrate laid on the bottom.
5. The method for metallizing a wafer as claimed in claim 4, It is characterized in that The material of the second substrate is selected from at least one of polyimide resin, polytetrafluoroethylene resin, polyvinylidene fluoride resin, polysulfone resin, polyethersulfone, polypropylene resin, polyethylene terephthalate resin, polyetheretherketone and polyamide; And / or, the second substrate has a thickness of 100-200 μm.
6. The method for metallizing a wafer as claimed in claim 1, It is characterized in that The material of the first substrate is selected from at least one of polyimide resin, polytetrafluoroethylene resin, polyvinylidene fluoride resin, polysulfone resin, polyethersulfone, polypropylene resin, polyethylene terephthalate resin, polyetheretherketone and polyamide; And / or, the first substrate has a thickness of 100-1000 μm.
7. The method for metallizing a wafer as claimed in claim 1, It is characterized in that The drying temperature is 100-150°C; And / or, the drying time is 5-30 min.
8. The method for metallizing a wafer as claimed in claim 1, It is characterized in that Pressurize to 2-10MPa; And / or, the pressurization duration is 1-5 min.
Citation Information
Patent Citations
Sintering materials and attachment methods using same
CN106660120A
Sintered silver cushion block with low modulus and high thermal conductivity and manufacturing device and method thereof
CN115116867A