Sodium ferric sulfate positive electrode material and preparation method thereof, positive plate, sodium ion battery and electric equipment
By extracting Na2Fe2-x-y-z-nCoxAlyMnzCan(SO4)3@Ti2O3@C structure sodium iron sulfate cathode material from hematite, using Ti2O3 and carbon coating layer to improve the material stability and conductivity, solving the problem of Na2Fe2(SO4)3 The problem of poor material stability has been achieved, and efficient sodium-ion battery performance and cost reduction have been achieved.
Patent Information
- Application Number
- CN202410845502.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-27
AI Technical Summary
The existing Na2Fe2(SO4)3 material has poor material stability, strong water absorption, and poor conductivity, which makes its industrial application difficult. Moreover, the existing preparation method relies on finished sodium sources, sulfur sources, and iron sources, which increases the cost. There are no reports on the direct synthesis of sodium iron sulfate cathode materials from ore raw materials.
Using hematite as raw material, it is dissolved in an acid solution and mixed with a reducing carbon source and a sodium source, dried and calcined to form a sodium iron sulfate cathode material with a structure of Na2Fe2-x-y-z-nCoxAlyMnzCan(SO4)3@Ti2O3@C, using Ti2O3 The coating layer and carbon coating layer improve the stability and conductivity of the material, and are doped and modified by Al, Mn, Ca, and Co elements present in the ore.
It improves the cycle stability and conductivity of the sodium iron sulfate cathode material, reduces production costs, simplifies the process flow, enhances the environmental stability and electrochemical performance of the material, and achieves high capacity retention and excellent battery performance.
Smart Images

Figure CN118738334A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of new energy technology, and in particular to a sodium iron sulfate positive electrode material and a preparation method thereof, a positive electrode sheet, a sodium ion battery and electrical equipment. Background Art
[0002] At present, the most studied positive electrode materials for sodium-ion batteries include transition metal layered oxides, Prussian blue analogs, polyanion compounds, etc. Among them, polyanion materials have the advantages of good cycle stability and thermal stability compared with other types of materials.
[0003] High energy density iron-based polyanion cathode materials have attracted extensive attention from researchers in recent years. As an excellent low-cost iron-based cathode material, Na2Fe2(SO4)3 has a reversible platform of up to 3.8V and a theoretical specific capacity of 121mAh / g, which is rare in polyanion materials. It lays a solid foundation for high energy density. From the perspective of electrochemical performance, Na2Fe2(SO4)3 material is a promising cathode material with a long cycle life.
[0004] However, the existing Na2Fe2(SO4)3 material has poor material stability, absorbs water and dissociates when exposed to air, and its inherent poor conductivity makes its industrial application difficult. Moreover, the preparation methods of Na2Fe2(SO4)3 in the prior art are all based on mixing finished sodium source, sulfur source, and iron source in a certain way and then sintering them into the required positive electrode material. Purchasing raw materials such as sodium source, iron source, and carbon source for synthesis and preparation has increased costs to a certain extent. There is currently no report on the synthesis and preparation of sodium iron sulfate positive electrode materials from ore raw materials. Summary of the invention
[0005] The purpose of the present application is to provide a sodium iron sulfate positive electrode material and a preparation method thereof, a positive electrode sheet, a sodium ion battery, and an electrical device to solve the above-mentioned problems.
[0006] To achieve the above objectives, this application adopts the following technical solutions:
[0007] The first aspect of the present application provides a sodium iron sulfate positive electrode material, the chemical formula of which is Na2Fe 2-x-y-z-n Co x Al y Mn z Ca n (SO4)3@Ti2O3@C, where, 0<x+y+z+n<0.5, 0.0005<x<0.485, 0.0005<y<0.485, 0.0005<z<0.485, 0.0005<n<0.485, Na2Fe 2-x-y-z-nCo x Al y Mn z Ca n (SO4)3 is the core, Ti2O3 is the first coating layer covering the core, and C is the second coating layer covering the first coating layer.
[0008] The second aspect of the present application also provides a method for preparing a sodium iron sulfate positive electrode material, comprising:
[0009] Dissolving hematite with an acid solution to obtain a first solution;
[0010] mixing the first solution with a reducing carbon source, a sodium source, and a sulfur source to obtain a second solution;
[0011] Drying the second solution to obtain a precursor;
[0012] The precursor is calcined to obtain a sodium iron sulfate positive electrode material.
[0013] The third aspect of the present application also provides a sodium iron sulfate positive electrode material, which is prepared by the preparation method of the sodium iron sulfate positive electrode material of the second aspect mentioned above.
[0014] The fourth aspect of the present application also provides a positive electrode sheet, comprising the sodium iron sulfate positive electrode material of the first aspect or the third aspect.
[0015] The fifth aspect of the present application also provides a sodium ion battery, comprising the positive electrode sheet of the fourth aspect.
[0016] The sixth aspect of the present application also provides an electrical device, including the sodium ion battery of the fifth aspect mentioned above.
[0017] Compared with the prior art, the beneficial effects of this application include:
[0018] The sodium iron sulfate positive electrode material of the present application utilizes elements such as Al, Mn, Ca, and Co to achieve doping modification of the sodium iron sulfate positive electrode material, forming a multi-entropy structure, which improves the ionic conductivity and electronic conductivity of the sodium iron sulfate positive electrode material, thereby improving the cycle stability of the sodium iron sulfate positive electrode material. At the same time, Ti2O3 is used to coat the material, which is beneficial to reduce its water absorption and improve its air stability. The carbon coating layer of the sodium iron sulfate positive electrode material of the present application can achieve complete coating of the material, improve the electronic conductivity of the material, alleviate phase change, and improve the stability of the material.
[0019] The preparation method of the sodium iron sulfate positive electrode material provided in the present application uses hematite as a raw material to directly synthesize and prepare the sodium iron sulfate positive electrode material, realizes the doping and modification of the material by trace impurity elements in the ore after a one-step acid dissolution, effectively utilizes the associated Al, Mn, Ca, and Co elements in the ore to dope and modify it, and realizes the coating of the material by Ti2O3 at the same time, improves the environmental stability of the material, eliminates the ore impurity removal process, shortens the process flow, and effectively reduces the production cost. The preparation method introduces a reducing carbon source during the acid dissolution process, which can reduce the metal elements to the corresponding valence state on the one hand, and realizes the coating of the material during the subsequent drying and sintering process on the other hand, avoiding direct contact between the electrolyte and the material, and improving the electrochemical performance of the material.
[0020] The positive electrode sheet and sodium ion battery prepared by the sodium iron sulfate positive electrode material of the present application have good cycle performance and high capacity retention rate; the electrical performance of the electrical equipment is excellent. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.
[0022] Figure 1 The process flow chart of the preparation method of the sodium iron sulfate positive electrode material of Example 1;
[0023] Figure 2 The charge and discharge curve of the sodium ion battery prepared from the sodium iron sulfate positive electrode material of Example 1;
[0024] Figure 3 This is a cycle diagram of a sodium ion battery prepared from the sodium iron sulfate positive electrode material of Example 1;
[0025] Figure 4 This is a SEM image of the sodium iron sulfate positive electrode material of Example 2;
[0026] Figure 5 This is a SEM image of the sodium iron sulfate positive electrode material of Comparative Example 3;
[0027] Figure 6 This is the XRD diagram of the sodium iron sulfate positive electrode material of Example 3. DETAILED DESCRIPTION
[0028] As used herein:
[0029] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0030] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.
[0031] The first aspect of the present application provides a sodium iron sulfate positive electrode material, the chemical formula of which is Na2Fe 2-x-y-z-n Co x Al y Mn z Ca n (SO4)3@Ti2O3@C, where, 0<x+y+z+n<0.5, 0.0005<x<0.485, 0.0005<y<0.485, 0.0005<z<0.485, 0.0005<n<0.485, Na2Fe 2-x-y-z-n Co x Al y Mn z Ca n (SO4)3 is the core, Ti2O3 is the first coating layer covering the core, and C is the second coating layer covering the first coating layer.
[0032] wherein x, y, z, and n may be, for example, 0.0007, 0.001, 0.003, 0.005, 0.007, 0.01, 0.012, 0.013, 0.014, 0.02, 0.05, 0.08, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, or 0.45, respectively.
[0033] In some embodiments, the average thickness of the second coating layer is 0.5 to 5 nm, for example, it can be 0.5 nm, 1 nm, 1.5 nm, 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, 4.5 nm or 5 nm; the mass of the Ti element in the first coating layer relative to the sodium iron sulfate positive electrode material is 500 to 4000 ppm, for example, it can be 500 ppm, 700 ppm, 900 ppm, 1000 ppm, 1200 ppm, 1500 ppm, 1800 ppm, 2000 ppm, 2200 ppm, 2500 ppm, 2700 ppm, 2800 ppm, 3000 ppm, 3500 ppm, 4000 ppm or any value between 500 and 4000 ppm.
[0034] The second aspect of the present application also provides a method for preparing a sodium iron sulfate positive electrode material, comprising:
[0035] Dissolving hematite with an acid solution to obtain a first solution;
[0036] mixing the first solution with a reducing carbon source, a sodium source, and a sulfur source to obtain a second solution;
[0037] Drying the second solution to obtain a precursor;
[0038] The precursor is calcined to obtain a sodium iron sulfate positive electrode material.
[0039] The preparation method of the sodium iron sulfate positive electrode material provided in the present application uses hematite as a raw material to directly synthesize and prepare the sodium iron sulfate positive electrode material, shortening the process flow and effectively reducing the production cost. The preparation method introduces a reducing carbon source during the acid dissolution process, which can reduce the metal element to the corresponding valence state on the one hand, and on the other hand, it can achieve coating of the material during the subsequent drying and sintering process, avoiding direct contact between the electrolyte and the material.
[0040] In some embodiments, the acid solution includes a mixture of one or more of phosphoric acid, perchloric acid, dichromic acid, iodic acid, hydroiodic acid, hydrosulfuric acid, boric acid, hydrochloric acid, sulfuric acid, sulfurous acid, nitric acid, hydrofluoric acid, and acetic acid, wherein nitric acid and sulfuric acid are not used at the same time.
[0041] Wherein, the concentration of sulfuric acid is 0.01-6 mol / L, for example, it can be 0.01 mol / L, 0.1 mol / L, 0.5 mol / L, 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L or 6 mol / L; the concentration of hydrofluoric acid is 0.01-0.4 mol / L, for example, it can be 0.01 mol / L, 0.05 mol / L, 0.1 mol / L, 0.15 mol / L, 0.2 mol / L, 0.25 mol / L, 0.3 mol / L, 0.35 mol / L or 0.4 mol / L.
[0042] In some embodiments, the reaction temperature for dissolving the hematite with an acid solution is 0°C to 40°C, for example, the reaction time for dissolving the hematite with an acid solution is 6 to 12 hours, for example, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours or 12 hours, and the pH of the first solution is 4 to 11, and the pH of the first solution can be, for example, 4, 5, 6, 7, 8, 9, 10 or 11.
[0043] In some embodiments, the reducing carbon source includes any one or more of citric acid, oxalic acid, oleic acid, pyromellitic acid, glucose, ethylene glycol, polyethylene glycol, formaldehyde, ascorbic acid, and pyrrole. The reducing carbon source of the present application not only realizes the reduction of the metal elements of hematite, but also realizes the complete coating of the sodium iron sulfate positive electrode material in the later stage, improves the electronic conductivity of the material, alleviates the phase change, and improves the stability of the material.
[0044] In some embodiments, the sodium source includes any one or more of sodium carbonate, sodium sulfate, sodium oxalate, sodium acetate, sodium alginate, and sodium citrate.
[0045] In some embodiments, the sulfur source includes any one or more of sulfuric acid, sulfur dioxide, sulfur trioxide, sodium sulfate, sodium sulfite, ammonium sulfate, and sodium thiosulfate.
[0046] The sodium source and the sulfur source can be the same substance. For example, if both the sodium source and the sulfur source are sodium sulfate, then only sodium sulfate needs to be added when adding the sodium source and the sulfur source. If the sodium source and the sulfur source are different substances, then the sodium source substance and the sulfur source substance can be added separately.
[0047] When the sulfur source is sulfuric acid, if the acid solution used in the dissolving step includes sulfuric acid, sulfuric acid may not be added in the step of adding the sulfur source.
[0048] In some embodiments, the first solution is mixed with the reducing carbon source, the sodium source, and the sulfur source at a speed of 100 to 1600 rpm, preferably 500 to 1600 rpm, and more preferably 1000 to 1500 rpm; the mixing time is 20 to 600 min, preferably 100 to 500 min, and more preferably 200 to 400 min.
[0049] The mixing method includes any one or more of mechanical stirring, double-screw stirring, and sand milling. Sand milling can not only play a mixing role, but also control the particle size of the material.
[0050] In some embodiments, the solid content of the second solution is 30%-70%, for example, 30%, 40%, 50%, 60% or 70%.
[0051] In some embodiments, the drying comprises any one of vacuum drying, freeze drying, and spray drying.
[0052] The vacuum drying temperature is 100-120°C, for example, 100°C, 105°C, 110°C, 115°C or 120°C, and the drying time is 8-12h, for example, 8h, 9h, 10h, 11h or 12h.
[0053] The freeze-drying temperature is -40 to -60°C, for example -40°C, -45°C, -50°C, -55°C or -60°C, and the freeze-drying time is 5h to 10h, for example 5h, 6h, 7h, 8h, 9h or 10h.
[0054] Wherein, the inlet air temperature of the spray drying is 200-300°C, and the inlet air temperature of the spray drying can be, for example, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, 260°C, 270°C, 280°C, 290°C or 300°C; the outlet air temperature of the spray drying is 90-150°C, and the outlet air temperature of the spray drying can be, for example, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C or 150°C; the fan power of the spray drying is 30-50HZ, for example, 30HZ, 35HZ, 40HZ, 45HZ or 50HZ, and the peristaltic speed of the spray drying is 60-150rpm, for example, 60rpm, 70rpm, 80rpm, 90rpm, 100rpm, 110rpm, 120rpm, 130rpm, 140rpm or 150rpm.
[0055] In a preferred embodiment, the calcination includes a primary calcination and a secondary calcination.
[0056] In some embodiments, the temperature of the first calcination stage is 10-200°C, for example, it can be 10°C, 50°C, 80°C, 100°C, 120°C, 150°C, 170°C or 200°C; the time of one calcination stage is 1-24h, for example, it can be 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 12h, 15h, 16h, 18h, 20h, 22h, 23h or 24h; the heating rate is 1-10°C / min, for example, it can be 1°C / min, 3°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min.
[0057] In some embodiments, the temperature of the second-stage calcination is 200-500°C, for example, it can be 200°C, 250°C, 300°C, 350°C, 400°C, 450°C or 500°C; the time of the second-stage calcination is 4-24h, for example, it can be 4h, 5h, 6h, 8h, 9h, 10h, 12h, 15h, 18h, 20h, 22h or 24h; the heating rate is 1-8°C / min, for example, it can be 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min or 8°C / min.
[0058] In some embodiments, the calcination is carried out in a protective gas, and the protective gas includes any one or more of argon, nitrogen, hydrogen, ammonia, and methane. The flow rate of the protective gas is 0-30m / s. 3 / h.
[0059] Wherein, the oxygen content of the second-stage calcination process is 10-100 ppm, for example, it can be 10 ppm, 20 ppm, 30 ppm, 40 ppm, 50 ppm, 60 ppm, 70 ppm, 80 ppm, 90 ppm or 100 ppm.
[0060] The third aspect of the present application also provides a sodium iron sulfate positive electrode material, which is prepared by the preparation method of the sodium iron sulfate positive electrode material of the second aspect mentioned above.
[0061] The sodium ferric sulfate positive electrode material obtained by the preparation method directly utilizes elements such as Al, Mn, Ca, and Co present in the ore to achieve doping modification of the sodium ferric sulfate positive electrode material, forming a multi-entropy structure, thereby improving the ionic conductivity and electronic conductivity of the sodium ferric sulfate positive electrode material, and thus improving the cycle stability of the sodium ferric sulfate positive electrode material.
[0062] The fourth aspect of the present application also provides a positive electrode sheet, comprising the sodium iron sulfate positive electrode material of the first aspect or the third aspect.
[0063] The fifth aspect of the present application also provides a sodium ion battery, comprising the positive electrode sheet of the fourth aspect.
[0064] The sodium ferric sulfate positive electrode material prepared by the method for preparing the sodium ferric sulfate positive electrode material of the present application has good cycle performance and high capacity retention rate.
[0065] The sixth aspect of the present application also provides an electrical device, including the sodium ion battery of the fifth aspect mentioned above.
[0066] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0067] The hematite used in the following examples and comparative examples was purchased from 1688 Online Purchase, and the content of each element thereof is shown in Table 1.
[0068] Table 1 Hematite element content
[0069] Iron content (wt%) 58.76% Manganese content (wt%) 4.25% Calcium content (wt%) 2.04% Cobalt content (wt%) 4.17% Aluminum content (wt%) 1.55% Titanium content (wt%) 0.28%
[0070] Example 1
[0071] Example 1 provides a sodium iron sulfate positive electrode material and a preparation method thereof, please refer to Figure 1 , Figure 1 The process flow chart of the preparation method of the sodium iron sulfate positive electrode material of the present application includes the following steps:
[0072] Step 1: Take 152g of hematite, crush it in the air, and sieve to obtain mineral powder with a particle size of <5um. Place the mineral powder in a container, add 15L of 0.2mol / L dilute sulfuric acid solution, heat to 40°C, react for 8h, adjust the solution pH to 7, and obtain an iron / aluminum / cobalt / manganese / calcium / titanium solution.
[0073] Step 2: Add 0.25 mol of citric acid to the solution until the solution turns light green, then add 1 mol of sodium sulfate and deionized water at the same time, control the solid content to 50%, control the sand milling time to 400 min, the sand milling speed to 1500 r, and control the particle size of the material after sand milling to <200 nm.
[0074] Step 3: Control the spray creep speed to 80 rpm, the spray drying air inlet temperature to 210° C., and the air outlet temperature to 105° C. to obtain a spray-dried material, which is a calcined precursor.
[0075] Step 4: calcine the precursor in a H2 / Ar (volume ratio 5% / 95%) atmosphere, first heating to 100°C at a heating rate of 5°C / min for reaction for 3 hours, then heating to 350°C at a heating rate of 2°C / min for reaction for 8 hours, naturally cool to room temperature, and pass through a 300-mesh sieve after air flow crushing to obtain the sodium iron sulfate positive electrode material of Example 1.
[0076] The chemical formula of the sodium iron sulfate positive electrode material obtained in Example 1 is Na2Fe 1.6 Co 0.11 Al 0.09 Mn 0.12 Ca 0.08 (SO4)3@Ti2O3@C, the carbon layer thickness is 2nm, the mass of Ti element in the Ti2O3 coating layer is 900ppm relative to the sodium iron sulfate positive electrode material, and the electronic conductivity is 10.8*10 -5 S / cm, the ion migration coefficient is 6.7*10 -7 cm 2 / s, as shown in Table 2. The titanium element in hematite is insoluble in acid and cannot generate subsequent sulfate, so a Ti2O3 coating layer is formed on the surface of the sodium iron sulfate positive electrode material during the subsequent sintering process. The thickness of the carbon coating layer can be measured by TEM; the coating amount of Ti2O3 can be obtained by XRF testing.
[0077] The obtained positive electrode material is then prepared into positive electrode slurry, and then the slurry is prepared into positive electrode sheet, and the positive electrode sheet and sodium sheet are assembled into button batteries. The button battery is assembled according to the following steps: 1) According to the ratio of active material: conductive agent: binder = 8:1:1, NMP is used as solvent to stir the slurry for 6 hours; 2) The slurry is coated on 16u aluminum foil, the coating thickness is controlled to be 120um, and it is baked in a vacuum oven at 105℃ for 4 hours; 3) The electrode sheet is rolled and cut into small discs; 4) It is assembled according to the positive electrode shell-positive electrode sheet-diaphragm-sodium sheet-negative electrode shell, and 5 drops of sodium electrolyte are dripped into it; 5) It is left to stand for 12 hours and tested in the cabinet.
[0078] Figure 2 This is a charge and discharge curve of a sodium ion battery prepared from the sodium iron sulfate positive electrode material of Example 1. The platform voltage of the material can reach 3.75V; Figure 3 This is a cycle diagram of a sodium ion battery prepared using the sodium iron sulfate positive electrode material of Example 1. At a rate of 1C, the discharge capacity reaches 90 mAh / g after 400 cycles, and the capacity retention rate reaches more than 94%.
[0079] Example 2
[0080] Example 2 provides a sodium iron sulfate positive electrode material and a preparation method thereof, please refer to Figure 1 , including the following steps:
[0081] Step 1: Take 152g of hematite, crush it in the air, and sieve to obtain mineral powder with a particle size of less than 5um. Place the mineral powder in a container, add 30L of 0.2mol / L nitric acid solution, heat to 25°C, react for 6h, adjust the solution pH to 7, and obtain an iron / aluminum / cobalt / manganese / calcium / titanium solution.
[0082] Step 2: Add 0.3 mol of citric acid to the solution until the solution turns light green, then add 1 mol of sodium sulfate, 1 mol of ammonium sulfate, and deionized water at the same time, control the solid content to 60%, control the sand milling time to 600 min, the sand milling speed to 600 r, and control the particle size of the material after sand milling to <200 nm.
[0083] Step 3: Control the freeze-drying temperature to -50°C and the freeze-drying time to 8 hours to obtain a freeze-dried material, which is a calcination precursor.
[0084] Step 4: The precursor was calcined in a H2 / Ar (volume ratio 5% / 95%) atmosphere, first heated to 150°C at a heating rate of 5°C / min for 3h, then heated to 400°C at a heating rate of 2°C / min for 8h, naturally cooled to room temperature, and vibrated and crushed and passed through a 200-mesh sieve to obtain the sodium iron sulfate positive electrode material of Example 2. Figure 4 This is the SEM image of the sodium iron sulfate positive electrode material of Example 2.
[0085] The chemical formula of the sodium iron sulfate positive electrode material obtained in Example 2 is Na2Fe 1.6 Co 0.11 Al 0.09 Mn 0.12 Ca 0.08 The carbon layer thickness of (SO4)3@Ti2O3@C is 2.4nm, the mass of Ti element in the Ti2O3 coating layer is 925ppm relative to the sodium iron sulfate positive electrode material, and the electronic conductivity is 11.4*10 -5 S / cm, the ion migration coefficient is 7.3*10 -7 cm 2 / s, as shown in Table 2.
[0086] The obtained positive electrode material is then prepared into a positive electrode slurry, and then the slurry is prepared into a positive electrode sheet. The positive electrode sheet and the sodium sheet are assembled into a button battery. The assembly method refers to Example 1. The platform voltage of the material can reach 3.77V; at a rate of 1C, the discharge specific capacity after 400 cycles reaches 88mAh / g, and the capacity retention rate reaches more than 88%.
[0087] Example 3
[0088] Example 3 provides a sodium iron sulfate positive electrode material and a preparation method thereof, please refer to Figure 1, including the following steps:
[0089] Step 1: Take 152g of hematite, crush it in the air, and sieve to obtain mineral powder with a particle size of less than 5um. Place the mineral powder in a container, add 15L of 0.4mol / L acetic acid solution, heat to 30°C, react for 12h, adjust the solution pH to 7, filter out insoluble impurities, and obtain an iron / aluminum / cobalt / manganese / calcium / titanium solution.
[0090] Step 2: Add 0.45 mol of citric acid to the solution until the solution turns light green, then add 1 mol of sodium sulfate and 1 mol of ammonium sulfate, control the sand milling time to 200 min, the sand milling speed to 1100 r, and the particle size of the material after sand milling is controlled to be <200 nm.
[0091] Step 3: Control the vacuum drying temperature to 120° C. and the vacuum drying time to 10 h to obtain a vacuum dried material, which is a calcined precursor.
[0092] Step 4: The precursor was calcined in a H2 / Ar (volume ratio 5% / 95%) atmosphere, first heated to 200°C at a heating rate of 5°C / min for 3h, then heated to 500°C at a heating rate of 2°C / min for 8h, cooled naturally to room temperature, and passed through a 150-mesh sieve after air flow crushing to obtain the sodium iron sulfate positive electrode material of Example 3. The chemical formula of the obtained sodium iron sulfate positive electrode material is Na2Fe 1.6 Co 0.11 Al 0.09 Mn 0.12 Ca 0.08 (SO4)3@Ti2O3@C, the carbon layer thickness is 3nm, the mass of Ti element in the Ti2O3 coating layer is 938ppm relative to the sodium iron sulfate positive electrode material, and the electronic conductivity is 10.5*10 -5 S / cm, the ion migration coefficient is 5.8*10 -7 cm 2 / s, as shown in Table 2, XRD pattern Figure 6 shown.
[0093] The obtained positive electrode material is then prepared into a positive electrode slurry, and then the slurry is prepared into a positive electrode sheet. The positive electrode sheet and the sodium sheet are assembled into a button battery. The assembly method refers to Example 1. The platform voltage of the material can reach 3.74V; at a rate of 0.2C, the discharge specific capacity after 100 cycles reaches 95mAh / g, and the capacity retention rate reaches more than 88%.
[0094] Example 4
[0095] Example 4 provides a sodium iron sulfate positive electrode material and a preparation method thereof, please refer to Figure 1 , including the following steps:
[0096] Step 1: Take 152g of hematite, crush it in the air, and sieve to obtain mineral powder with a particle size of less than 5um. Place the mineral powder in a container, add 7.5L of 0.4mol / L dilute sulfuric acid solution, heat to 20°C, react for 10h, adjust the solution pH to 4, filter out insoluble impurities, and obtain an iron / aluminum / cobalt / manganese / calcium / titanium solution.
[0097] Step 2: Add 0.4 mol of citric acid to the solution until the solution turns light green, then add sodium carbonate and adjust the pH to 7. Control the sand milling time to 100 min and the sand milling speed to 900 r. The particle size of the material after sand milling is controlled to be <200 nm.
[0098] Step 3: Control the vacuum drying temperature to 120° C. and the vacuum drying time to 10 h to obtain a vacuum dried material, which is a calcined precursor.
[0099] Step 4: The precursor is calcined in a methane atmosphere, first heated to 100°C at a heating rate of 5°C / min for 3h, then heated to 350°C at a heating rate of 2°C / min for 8h, cooled naturally to room temperature, and sieved through a 300-mesh sieve after air flow crushing to obtain the sodium iron sulfate positive electrode material of Example 4. The chemical formula of the obtained sodium iron sulfate positive electrode material is Na2Fe 1.6 Co 0.11 Al 0.09 Mn 0.12 Ca 0.08 The carbon layer thickness of (SO4)3@Ti2O3@C is 2.9nm, the mass of Ti element in the Ti2O3 coating layer is 915ppm relative to the sodium iron sulfate positive electrode material, and the electronic conductivity is 11.1*10 -5 S / cm, ion migration coefficient is 6.0*10 - 7 cm 2 / s, as shown in Table 2.
[0100] The obtained positive electrode material is then prepared into a positive electrode slurry, and then the slurry is prepared into a positive electrode sheet. The positive electrode sheet and the sodium sheet are assembled into a button battery. The assembly method refers to Example 1. The platform voltage of the material can reach 3.74V; at a rate of 1C, the discharge specific capacity after 100 cycles reaches 84mAh / g, and the capacity retention rate reaches more than 85%.
[0101] Example 5
[0102] The sodium iron sulfate positive electrode material and the preparation method thereof of Example 5 are different from those of Example 1 in that the purchased raw materials such as sulfur source, sodium source, carbon source, dopant, etc. are used for synthesis. The preparation method of the sodium iron sulfate positive electrode material of Example 5 comprises the following steps:
[0103] Step 1: Take 1.6 mol of ferrous sulfate heptahydrate, 0.11 mol of cobalt sulfate, 0.045 mol of aluminum sulfate, 0.12 mol of manganese sulfate, 0.08 mol of calcium sulfate, 0.0045 mol of Ti2O3, 0.25 mol of oxalic acid, add 1 mol of sodium sulfate and deionized water at the same time, control the solid content to 60%, control the sand milling time to 150 min, control the sand milling speed to 1000 r, and control the particle size of the material after sand milling to be less than 200 nm.
[0104] Step 3: Control the freeze-drying temperature to -50°C and the freeze-drying time to 8 hours to obtain a freeze-dried material, which is a calcination precursor.
[0105] Step 4: calcine the precursor in a H2 / Ar (volume ratio 5% / 95%) atmosphere, first heat the temperature to 150°C at a heating rate of 5°C / min and react for 3 hours, then heat the temperature to 400°C at a heating rate of 2°C / min and react for 8 hours, naturally cool to room temperature, vibrate and crush, and pass through a 200-mesh sieve to obtain the sodium iron sulfate positive electrode material of Example 5.
[0106] The chemical formula of the obtained sodium iron sulfate positive electrode material is Na2Fe 1.6 Co 0.11 Al 0.09 Mn 0.12 Ca 0.08 (SO4)3@Ti2O3@C, the electrochemical performance of the material is equivalent to that of Example 1, but the cost is 30% higher.
[0107] Example 6
[0108] The difference between the sodium iron sulfate positive electrode material and the preparation method thereof of Example 6 and Example 5 is that the amount of Ti2O3 added is 0.0023 mol. The preparation method of the sodium iron sulfate positive electrode material of Example 6 comprises the following steps:
[0109] Step 1: Take 1.6 mol of ferrous sulfate heptahydrate, 0.11 mol of cobalt sulfate, 0.045 mol of aluminum sulfate, 0.12 mol of manganese sulfate, 0.08 mol of calcium sulfate, 0.0023 mol of Ti2O3, 0.25 mol of oxalic acid, add 1 mol of sodium sulfate and deionized water at the same time, control the solid content to 60%, control the sand milling time to 150 min, control the sand milling speed to 1000 r, and control the particle size of the material after sand milling to be less than 200 nm.
[0110] Step 3: Control the freeze-drying temperature to -50°C and the freeze-drying time to 8 hours to obtain a freeze-dried material, which is a calcination precursor.
[0111] Step 4: calcine the precursor in a H2 / Ar (volume ratio 5% / 95%) atmosphere, first react at 150°C for 3 hours with a heating rate of 5°C / min, then react at 400°C for 8 hours with a heating rate of 2°C / min, naturally cool to room temperature, vibrate and crush, and pass through a 200-mesh sieve to obtain the sodium iron sulfate positive electrode material of Example 6.
[0112] The chemical formula of the obtained sodium iron sulfate positive electrode material is Na2Fe 1.6 Co 0.11 Al 0.09 Mn 0.12 Ca 0.08 The carbon layer thickness of (SO4)3@Ti2O3@C is 2.1nm, the mass of Ti element in the Ti2O3 coating layer is 505ppm relative to the sodium iron sulfate positive electrode material, and the electronic conductivity is 10.1*10 -5 S / cm, the ion migration coefficient is 6.3*10 -7 cm 2 / s, at a rate of 1C, the discharge capacity after 150 cycles is 89mAh / g, and the capacity retention rate is over 95%.
[0113] Example 7
[0114] The difference between the sodium iron sulfate positive electrode material and the preparation method thereof of Example 7 and Example 5 is that the amount of Ti2O3 added is 0.0188 mol. The preparation method of the sodium iron sulfate positive electrode material of Example 7 comprises the following steps:
[0115] Step 1: Take 1.6 mol of ferrous sulfate heptahydrate, 0.11 mol of cobalt sulfate, 0.045 mol of aluminum sulfate, 0.12 mol of manganese sulfate, 0.08 mol of calcium sulfate, 0.0188 mol of Ti2O3, 0.25 mol of oxalic acid, add 1 mol of sodium sulfate and deionized water at the same time, control the solid content to 60%, control the sand milling time to 150 min, control the sand milling speed to 1000 r, and control the particle size of the material after sand milling to be less than 200 nm.
[0116] Step 3: Control the freeze-drying temperature to -50°C and the freeze-drying time to 8 hours to obtain a freeze-dried material, which is a calcination precursor.
[0117] Step 4: calcine the precursor in a H2 / Ar (volume ratio 5% / 95%) atmosphere, first react at 150°C for 3 hours with a heating rate of 5°C / min, then react at 400°C for 8 hours with a heating rate of 2°C / min, naturally cool to room temperature, vibrate and crush, and pass through a 200-mesh sieve to obtain the sodium iron sulfate positive electrode material of Example 7.
[0118] The chemical formula of the obtained sodium iron sulfate positive electrode material is Na2Fe 1.6 Co 0.11Al 0.09 Mn 0.12 Ca 0.08 (SO4)3@Ti2O3@C, the carbon layer thickness is 1.8nm, the mass of Ti element in the Ti2O3 coating layer is 4000ppm relative to the sodium iron sulfate positive electrode material, and the electronic conductivity is 10.4*10 -5 S / cm, the ion migration coefficient is 6.5*10 -7 cm 2 / s, at a rate of 1C, the discharge capacity after 120 cycles is 93mAh / g, and the capacity retention rate is over 90%.
[0119] Comparative Example 1
[0120] The sodium iron sulfate positive electrode material and preparation method thereof of Comparative Example 1 are different from those of Example 1 in that the first-stage calcination and the second-stage calcination temperatures exceed the set range. The preparation method of the sodium iron sulfate positive electrode material of Comparative Example 1 comprises the following steps:
[0121] Step 1: Take 152g of hematite, crush it in the air, and sieve to obtain mineral powder with a particle size of <5um. Place the mineral powder in a container, add 15L of 0.2mol / L dilute sulfuric acid solution, heat to 40°C, react for 8h, adjust the solution pH to 7, and obtain an iron / aluminum / cobalt / manganese / calcium / titanium solution.
[0122] Step 2: Add 0.25 mol of citric acid to the solution until the solution turns light green, then add 1 mol of sodium sulfate and deionized water at the same time, control the solid content to 50%, control the sand milling time to 400 min, the sand milling speed to 1500 r, and control the particle size of the material after sand milling to <200 nm.
[0123] Step 3: Control the spray creep speed to 80 rpm, the spray drying air inlet temperature to 210° C., and the air outlet temperature to 105° C. to obtain a spray-dried material, which is a calcined precursor.
[0124] Step 4: calcine the precursor in a H2 / Ar (volume ratio 5% / 95%) atmosphere, first heat the temperature to 300°C at a heating rate of 5°C / min and react for 3 hours, then heat the temperature to 600°C at a heating rate of 2°C / min and react for 8 hours, naturally cool to room temperature, and pass through a 300-mesh sieve after air flow crushing to obtain the sodium iron sulfate positive electrode material of Comparative Example 1.
[0125] The chemical formula of the obtained sodium iron sulfate positive electrode material is Na2Fe 1.6 Co 0.11 Al 0.09 Mn 0.12 Ca 0.08The carbon layer thickness of (SO4)3@Ti2O3@C is 1.7nm, the mass of Ti element in the Ti2O3 coating layer is 934ppm relative to the sodium iron sulfate positive electrode material, and the electronic conductivity is 8.3*10 -5 S / cm, the ion migration coefficient is 3.4*10 -7 cm 2 / s, as shown in Table 2.
[0126] The obtained positive electrode material is then prepared into positive electrode slurry, and then the slurry is prepared into positive electrode sheet, and the positive electrode sheet and sodium sheet are assembled into button batteries. The button battery is assembled according to the following steps: 1) According to the ratio of active material: conductive agent: binder = 8:1:1, NMP is used as solvent to stir the slurry for 6 hours; 2) The slurry is coated on 16u aluminum foil, the coating thickness is controlled to be 120um, and it is baked in a vacuum oven at 105℃ for 4 hours; 3) The electrode sheet is rolled and cut into small discs; 4) It is assembled according to the positive electrode shell-positive electrode sheet-diaphragm-sodium sheet-negative electrode shell, and 5 drops of sodium electrolyte are dripped into it; 5) It is left to stand for 12 hours and tested in the cabinet.
[0127] The platform voltage of the material can reach 3.25V; at a rate of 1C, the discharge capacity reaches 50mAh / g after 100 cycles, and the capacity retention rate is over 60%.
[0128] Comparative Example 2
[0129] The sodium iron sulfate positive electrode material and preparation method thereof of Comparative Example 2 differ from those of Example 1 in that only a two-stage calcination process is used without a one-stage calcination. The preparation method of the sodium iron sulfate positive electrode material of Comparative Example 2 comprises the following steps:
[0130] Step 1: Take 152g of hematite, crush it in the air, and sieve to obtain mineral powder with a particle size of <5um. Place the mineral powder in a container, add 15L of 0.2mol / L dilute sulfuric acid solution, heat to 40°C, react for 8h, adjust the solution pH to 7, and obtain an iron / aluminum / cobalt / manganese / calcium / titanium solution.
[0131] Step 2: Add 0.25 mol of citric acid to the solution until the solution turns light green, then add 1 mol of sodium sulfate and deionized water at the same time, control the solid content to 50%, control the sand milling time to 400 min, the sand milling speed to 1500 r, and control the particle size of the material after sand milling to <200 nm.
[0132] Step 3: Control the spray creep speed to 80 rpm, the spray drying air inlet temperature to 210° C., and the air outlet temperature to 105° C. to obtain a spray-dried material, which is a calcined precursor.
[0133] Step 4: calcine the precursor in a H2 / Ar (volume ratio 5% / 95%) atmosphere, heat to 350°C at a heating rate of 5°C / min for 8 hours, cool naturally to room temperature, and pass through a 300-mesh sieve after air flow crushing to obtain the sodium iron sulfate positive electrode material of Comparative Example 2.
[0134] The chemical formula of the obtained sodium iron sulfate positive electrode material is Na2Fe 1.6 Co 0.11 Al 0.09 Mn 0.12 Ca 0.08 The carbon layer thickness of (SO4)3@Ti2O3@C is 1.4nm, the mass of Ti element in the Ti2O3 coating layer is 929ppm relative to the sodium iron sulfate positive electrode material, and the electronic conductivity is 7.6*10 -5 S / cm, the ion migration coefficient is 4.5*10 -7 cm 2 / s, as shown in Table 2.
[0135] The obtained positive electrode material is then prepared into a positive electrode slurry, and then the slurry is prepared into a positive electrode sheet, and the positive electrode sheet and the sodium sheet are assembled into a button battery. The button battery is assembled according to the following steps: 1) According to the ratio of active material: conductive agent: binder = 8:1:1, NMP is used as a solvent to stir the slurry for 6 hours; 2) The slurry is coated on 16u aluminum foil, the coating thickness is controlled to be 120um, and it is baked in a vacuum oven at 105℃ for 4 hours; 3) The electrode sheet is rolled and cut into small discs; 4) It is assembled according to the positive electrode shell-positive electrode sheet-diaphragm-sodium sheet-negative electrode shell, and 5 drops of sodium-specific electrolyte are dripped into it; 5) It is left to stand for 12 hours and tested on the cabinet. The platform voltage of the material can reach 3.15V; at a rate of 1C, the discharge capacity after 100 cycles reaches 60mAh / g, and the capacity retention rate reaches more than 70%.
[0136] Comparative Example 3
[0137] The difference between the sodium iron sulfate positive electrode material and the preparation method thereof of Comparative Example 3 and Example 2 is that the reducing carbon source is adjusted to flake graphite. The preparation method of the sodium iron sulfate positive electrode material of Comparative Example 3 includes the following steps:
[0138] Step 1: Take 152g of hematite, crush it in the air, and sieve to obtain mineral powder with a particle size of less than 5um. Place the mineral powder in a container, add 30L of 0.2mol / L nitric acid solution, heat to 25°C, react for 6h, adjust the solution pH to 7, and obtain an iron / aluminum / cobalt / manganese / calcium / titanium solution.
[0139] Step 2: Add 0.3 mol of flake graphite, 1 mol of sodium sulfate, 1 mol of ammonium sulfate and deionized water to the solution, control the solid content to 60%, control the sand milling time to 600 min, the sand milling speed to 600 r, and control the particle size of the material after sand milling to <200 nm.
[0140] Step 3: Control the freeze-drying temperature to -50°C and the freeze-drying time to 8 hours to obtain a freeze-dried material, which is a calcination precursor.
[0141] Step 4: The precursor was calcined in a H2 / Ar (volume ratio 5% / 95%) atmosphere, first heated to 150°C at a heating rate of 5°C / min for 3h, then heated to 400°C at a heating rate of 2°C / min for 8h, naturally cooled to room temperature, and vibrated and crushed, and then sieved through a 200-mesh sieve to obtain the sodium iron sulfate positive electrode material of Comparative Example 3. The SEM image of the sodium iron sulfate positive electrode material of Comparative Example 3 is as follows: Figure 5 In Example 2, citric acid is used as the carbon source, which plays a reducing role while coating the material. It can be seen that the material particles are more rounded and have obvious traces of amorphous carbon coating. When using flake graphite to coat the material, obvious flake shapes can still be seen, with clear edges and corners.
[0142] The chemical formula of the obtained sodium iron sulfate positive electrode material is Na2Fe 1.6 Co 0.11 Al 0.09 Mn 0.12 Ca 0.08 The carbon layer thickness of (SO4)3@Ti2O3@C is 2.2nm, the mass of Ti element in the Ti2O3 coating layer is 917ppm relative to the sodium iron sulfate positive electrode material, and the electronic conductivity is 7.4*10 -5 S / cm, the ion migration coefficient is 3.2*10 -7 cm 2 / s, as shown in Table 2.
[0143] The obtained positive electrode material is then prepared into a positive electrode slurry, and then the slurry is prepared into a positive electrode sheet. The positive electrode sheet and the sodium sheet are assembled into a button battery. The assembly method is the same as that in Example 1. The platform voltage of the material can reach 3.73V; at a rate of 1C, the discharge specific capacity after 200 cycles reaches 84mAh / g, and the capacity retention rate reaches more than 66%.
[0144] Comparative Example 4
[0145] The sodium iron sulfate positive electrode material and the preparation method thereof of Comparative Example 4 are different from those of Example 2 in that no reducing carbon source is added. The preparation method of the sodium iron sulfate positive electrode material of Comparative Example 4 comprises the following steps:
[0146] Step 1: Take 152g of hematite, crush it in the air, and sieve to obtain mineral powder with a particle size of less than 5um. Place the mineral powder in a container, add 30L of 0.2mol / L nitric acid solution, heat to 25°C, react for 6h, adjust the solution pH to 7, and obtain an iron / aluminum / cobalt / manganese / calcium / titanium solution.
[0147] Step 2: Add 1 mol of sodium sulfate, 1 mol of ammonium sulfate, and deionized water at the same time, control the solid content to 60%, control the sand milling time to 600 min, the sand milling speed to 600 r, and control the particle size of the material after sand milling to <200 nm.
[0148] Step 3: Control the freeze-drying temperature to -50°C and the freeze-drying time to 8 hours to obtain a freeze-dried material, which is a calcination precursor.
[0149] Step 4: The precursor was calcined in a H2 / Ar (volume ratio 5% / 95%) atmosphere, first heated to 150°C at a heating rate of 5°C / min for 3h, then heated to 400°C at a heating rate of 2°C / min for 8h, naturally cooled to room temperature, and vibrated and crushed and passed through a 200-mesh sieve to obtain the sodium iron sulfate positive electrode material of Comparative Example 4.
[0150] The chemical formula of the obtained sodium iron sulfate positive electrode material is Na2Fe 1.6 Co 0.11 Al 0.09 Mn 0.12 Ca 0.08 The carbon layer thickness of (SO4)3@Ti2O3 is 0nm, the mass of Ti element in the Ti2O3 coating layer is 903ppm relative to the sodium iron sulfate positive electrode material, and the electronic conductivity is 1.2*10 -5 S / cm, the ion migration coefficient is 4.1*10 -7 cm 2 / s, as shown in Table 2.
[0151] The obtained positive electrode material is then prepared into a positive electrode slurry, and then the slurry is prepared into a positive electrode sheet. The positive electrode sheet and the sodium sheet are assembled into a button battery. The assembly method is the same as that in Example 1. The platform voltage of the material can reach 3.0V; at a rate of 1C, the discharge specific capacity after 50 cycles reaches 50mAh / g, and the capacity retention rate reaches more than 40%.
[0152] Comparative Example 5
[0153] The main difference between the positive electrode material preparation method of Comparative Example 5 and Example 1 is that an additional filtration step is performed when dissolving hematite to remove Ti2O3 that is insoluble in acid. The preparation method of the sodium iron sulfate positive electrode material of Comparative Example 5 includes the following steps:
[0154] Step 1: Take 152g of hematite, crush it in the air, and sieve to obtain mineral powder with a particle size of less than 5um. Place the mineral powder in a container, add 15L of 0.2mol / L dilute sulfuric acid solution, heat to 40°C, react for 8h, adjust the solution pH to 7, filter out insoluble impurities, and obtain an iron / aluminum / cobalt / manganese / calcium-containing solution.
[0155] Step 2: Add 0.25 mol of citric acid to the solution until the solution turns light green, then add 1 mol of sodium sulfate and deionized water at the same time, control the solid content to 50%, control the sand milling time to 400 min, the sand milling speed to 1500 r, and control the particle size of the material after sand milling to <200 nm.
[0156] Step 3: Control the spray creep speed to 80 rpm, the spray drying air inlet temperature to 210° C., and the air outlet temperature to 105° C. to obtain a spray-dried material, which is a calcined precursor.
[0157] Step 4: calcine the precursor in a H2 / Ar (volume ratio 5% / 95%) atmosphere, first heat the temperature to 100°C at a heating rate of 5°C / min and react for 3 hours, then heat the temperature to 350°C at a heating rate of 2°C / min and react for 8 hours, naturally cool to room temperature, and pass through a 300-mesh sieve after air flow crushing to obtain the sodium iron sulfate positive electrode material of Comparative Example 5.
[0158] The chemical formula of the obtained sodium iron sulfate positive electrode material is Na2Fe 1.6 Co 0.11 Al 0.09 Mn 0.12 Ca 0.08 (SO4)3@C, the carbon layer thickness is 2nm, the mass of Ti element in the Ti2O3 coating layer is 0 relative to the sodium iron sulfate positive electrode material, and the electronic conductivity is 8.8*10 -5 S / cm, the ion migration coefficient is 3.5*10 -7 cm 2 / s, as shown in Table 2.
[0159] The obtained positive electrode material is then prepared into a positive electrode slurry, and then the slurry is prepared into a positive electrode sheet, and the positive electrode sheet and the sodium sheet are assembled into a button battery. The button battery is assembled according to the following steps: 1) According to the ratio of active material: conductive agent: binder = 8:1:1, NMP is used as a solvent to stir the slurry for 6 hours; 2) The slurry is coated on 16u aluminum foil, the coating thickness is controlled to be 120um, and it is baked in a vacuum oven at 105℃ for 4 hours; 3) The electrode sheet is rolled and cut into small discs; 4) It is assembled according to the positive electrode shell-positive electrode sheet-diaphragm-sodium sheet-negative electrode shell, and 5 drops of sodium electrolyte are dripped into it; 5) It is left to stand for 12 hours and tested on the cabinet. The platform voltage of the material can reach 3.69V; at a rate of 1C, the discharge capacity after 100 cycles is 80mAh / g, and the capacity retention rate is more than 74%.
[0160] Comparative Example 6
[0161] The sodium iron sulfate positive electrode material and the preparation method thereof of Comparative Example 6 are different from those of Example 5 in that the doping elements Co and Al are lacking. The preparation method of the sodium iron sulfate positive electrode material of Comparative Example 6 comprises the following steps:
[0162] Step 1: Take 1.8 mol of ferrous sulfate heptahydrate, 0.12 mol of manganese sulfate, 0.08 mol of calcium sulfate, 0.0045 mol of Ti2O3, 0.25 mol of oxalic acid, add 1 mol of sodium sulfate and deionized water at the same time, control the solid content to 60%, control the sand milling time to 150 min, the sand milling speed to 1000 r, and control the particle size of the material after sand milling to be less than 200 nm.
[0163] Step 3: Control the freeze-drying temperature to -50°C and the freeze-drying time to 8 hours to obtain a freeze-dried material, which is a calcination precursor.
[0164] Step 4: calcine the precursor in a H2 / Ar (volume ratio 5% / 95%) atmosphere, first heat the temperature to 150°C at a heating rate of 5°C / min and react for 3 hours, then heat the temperature to 400°C at a heating rate of 2°C / min and react for 8 hours, naturally cool to room temperature, vibrate and crush, and pass through a 200-mesh sieve to obtain the sodium iron sulfate positive electrode material of Example 5.
[0165] The chemical formula of the obtained sodium iron sulfate positive electrode material is Na2Fe 1.8 Mn 0.12 Ca 0.08 The carbon layer thickness of (SO4)3@Ti2O3@C is 1.9nm, the mass of Ti element in the Ti2O3 coating layer is 950ppm relative to the sodium iron sulfate positive electrode material, and the electronic conductivity is 6.9*10 -5 S / cm, the ion migration coefficient is 2.9*10 -7 cm 2 / s, as shown in Table 2.
[0166] The obtained positive electrode material is then prepared into a positive electrode slurry, and then the slurry is prepared into a positive electrode sheet. The positive electrode sheet and the sodium sheet are assembled into a button battery. The assembly method is the same as that in Example 1. The platform voltage of the material can reach 3.4V; at a rate of 1C, the discharge specific capacity after 50 cycles reaches 60mAh / g, and the capacity retention rate reaches more than 60%.
[0167] Table 2 Related parameters of sodium iron sulfate positive electrode materials in various embodiments and comparative examples
[0168]
[0169] In summary, the sodium iron sulfate positive electrode material of the present application utilizes elements such as Al, Mn, Ca, and Co to achieve doping modification of the sodium iron sulfate positive electrode material, forming a multi-entropy structure, which improves the ionic conductivity and electronic conductivity of the sodium iron sulfate positive electrode material, thereby improving the cycle stability of the sodium iron sulfate positive electrode material. At the same time, Ti2O3 is used to coat the material, which is beneficial to reduce its water absorption and improve its air stability. The carbon coating layer of the sodium iron sulfate positive electrode material of the present application can achieve complete coating of the material, improve the electronic conductivity of the material, alleviate phase change, and improve the stability of the material.
[0170] The preparation method of the sodium iron sulfate positive electrode material provided in the present application uses hematite as a raw material to directly synthesize and prepare the sodium iron sulfate positive electrode material, realizes the doping and modification of the material by trace impurity elements in the ore after a one-step acid dissolution, effectively utilizes the associated Al, Mn, Ca, and Co elements in the ore to dope and modify it, and realizes the coating of the material by Ti2O3 at the same time, improves the environmental stability of the material, eliminates the ore impurity removal process, shortens the process flow, and effectively reduces the production cost. The preparation method introduces a reducing carbon source during the acid dissolution process, which can reduce the metal elements to the corresponding valence state on the one hand, and realizes the coating of the material during the subsequent drying and sintering process on the other hand, avoiding direct contact between the electrolyte and the material, and improving the electrochemical performance of the material.
[0171] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
[0172] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.
Claims
1. A sodium iron sulfate positive electrode material, characterized in that: The chemical formula of the sodium iron sulfate positive electrode material is Na2Fe 2-x-y-z-n Co x Al y Mn z Ca n (SO4)3@Ti2O3@C, where, 0<x+y+z+n<0.5, 0.0005<x<0.485, 0.0005<y<0.485, 0.0005<z<0.485, 0.0005<n<0.485, Na2Fe 2-x-y-z-n Co x Al y Mn z Ca n (SO4)3 is the core, Ti2O3 is the first coating layer covering the core, and C is the second coating layer covering the first coating layer.
2. The sodium iron sulfate positive electrode material according to claim 1, characterized in that The average thickness of the second coating layer is 0.5-5 nm, and the mass of the Ti element in the first coating layer is 500-4000 ppm relative to the sodium iron sulfate positive electrode material.
3. A method for preparing the sodium iron sulfate positive electrode material according to claim 1 or 2, characterized in that: include: Dissolving hematite with an acid solution to obtain a first solution; mixing the first solution with a reducing carbon source, a sodium source, and a sulfur source to obtain a second solution; Drying the second solution to obtain a precursor; The precursor is calcined to obtain the sodium iron sulfate positive electrode material.
4. The preparation method according to claim 3, characterized in that: At least one of the following conditions is met: A. The acid solution includes one or a mixture of phosphoric acid, perchloric acid, dichromic acid, iodic acid, hydroiodic acid, hydrosulfuric acid, boric acid, hydrochloric acid, sulfuric acid, sulfurous acid, nitric acid, hydrofluoric acid, and acetic acid; B. When condition A is met, the concentration of the sulfuric acid is 0.01 to 6 mol / L, and the concentration of the hydrofluoric acid is 0.01 to 0.4 mol / L; C. When condition A is met, the nitric acid and the sulfuric acid are not used at the same time; D. The reaction temperature of dissolving the hematite with an acid solution is 0°C to 40°C, and the reaction time is 6 to 12 hours; E. The pH of the first solution is 4-11.
5. The preparation method according to claim 3, characterized in that: At least one of the following conditions is met: a. The reducing carbon source comprises any one or more of citric acid, oxalic acid, oleic acid, pyromellitic acid, glucose, ethylene glycol, polyethylene glycol, formaldehyde, ascorbic acid, and pyrrole; b. The sodium source includes any one or more of sodium carbonate, sodium sulfate, sodium oxalate, sodium acetate, sodium alginate, and sodium citrate; c. The sulfur source includes any one or more of sulfuric acid, sulfur dioxide, sulfur trioxide, sodium sulfate, sodium sulfite, ammonium sulfate, and sodium thiosulfate; d. The mixing speed is 100 to 1600 rpm, and the mixing time is 20 to 600 min; e. The mixing method includes any one or more of mechanical stirring, double-screw stirring, and sand milling; f. The solid content of the second solution is 30%-70%.
6. The preparation method according to any one of claims 3 to 5, characterized in that: The calcination includes a first stage calcination and a second stage calcination; and / or, The drying includes any one of vacuum drying, freeze drying and spray drying; The preparation method satisfies at least one of the following conditions: (1) The temperature of the first stage calcination is 10-200°C, the time is 1-24h, and the heating rate is 1-10°C / min; (2) The temperature of the second stage calcination is 200-500°C, the time is 4-24h, and the heating rate is 1-8°C / min; (3) The calcination is carried out in a protective gas, wherein the protective gas includes any one or more of argon, nitrogen, hydrogen, ammonia, and methane; optionally, the flow rate of the protective gas is not higher than 30 m / s. 3 / h; (4) The oxygen content of the second-stage calcination process is 10-100 ppm; (5) The vacuum drying temperature is 100 to 120° C. and the time is 8 to 12 hours; (6) The freeze-drying temperature is -40 to -60°C and the time is 5 to 10 hours; (7) The inlet air temperature of the spray drying is 200-300°C, the outlet air temperature is 90-150°C, the fan power is 30-50HZ, and the peristaltic speed is 60-150rpm.
7. A positive electrode sheet, characterized in that: The invention comprises the sodium iron sulfate positive electrode material as described in claim 1 or 2.
8. A sodium ion battery, characterized in that: Including the positive electrode sheet as described in claim 7.
9. An electrical device, characterized in that: Including the sodium ion battery as described in claim 8.
Citation Information
Patent Citations
Sodium-ion battery positive electrode material as well as preparation method and application thereof
CN114477300A
Sodium-ion battery positive electrode material, preparation method thereof and sodium-ion battery
CN115312781A
Sodium-ion battery positive electrode material, preparation method thereof and sodium-ion battery
CN115312782A
Sodium-ion battery positive electrode material, preparation method thereof and sodium-ion battery
CN117239138A
Sodium ferric sulfate composite positive electrode material and preparation method and application thereof
CN117374285A
Cited By
Method for preparing moisture-resistant sodium ferric sulfate from pyrite
CN121107464A
Polyanionic sodium ion battery positive electrode material and preparation method thereof
CN121506942A