Solid electrolyte sheet and all-solid-state battery
By adjusting the material particle size and binder amount of the inner and outer layers in the solid electrolyte sheet of the all-solid-state battery, the strength deviation and crack problems caused by the porous substrate are solved, and the strength and ion conductivity of the solid electrolyte layer are improved. properties, improving battery stability and charging and discharging efficiency.
Patent Information
- Application Number
- CN202410374330.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-01
AI Technical Summary
In all-solid-state batteries, there are challenges in improving long-term stability and charge and discharge efficiency, especially the strength deviation and crack problems caused by the use of porous substrates, which affect the strength and ion conductivity of the solid electrolyte layer.
By adjusting the material particle size and binder amount of the inner and outer layers in the solid electrolyte sheet, the inner layer is filled with a solid electrolyte composition with a high binder content and the outer layer is filled with a low binder content composition to improve the laminated structure. Strength and ionic conductivity of the solid electrolyte layer.
It achieves increased strength, crack suppression and improved ionic conductivity of the solid electrolyte layer, improving the stability and charge and discharge efficiency of all-solid-state batteries.
Smart Images

Figure CN118738530A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a solid electrolyte sheet and an all-solid battery. Background Art
[0002] In recent years, in order to ensure that more people have access to affordable, reliable, sustainable and advanced energy, research and development related to all-solid batteries that contribute to energy efficiency are being carried out. All-solid batteries generally have a structure in which a solid electrolyte layer is sandwiched between the positive electrode and the negative electrode. For example, the solid electrolyte layer of a lithium-ion all-solid battery has the function of conducting lithium ions and the function of a diaphragm that prevents short circuits between the positive electrode layer (positive electrode active material layer) in the positive electrode and the negative electrode layer (negative electrode active material layer) in the negative electrode. Here, it is generally believed that in order to improve energy density, the solid electrolyte layer as a diaphragm is preferably as thin as possible. However, simply making it thinner will cause cracks due to a decrease in strength, so a known all-solid battery containing a porous substrate that achieves thinning and strength assurance of the solid electrolyte layer is known (see patent document 1, etc.).
[0003] [Prior Technical Literature]
[0004] (Patent Document)
[0005] Patent Document 1: Japanese Patent Application Publication No. 2015-153460 Summary of the invention
[0006] [Problems to be solved by the invention]
[0007] However, in the technology related to all-solid-state batteries, the problem is to improve long-term stability and charge-discharge efficiency. By including a porous substrate, the strength of the solid electrolyte layer is improved, thereby improving the stability of the all-solid-state battery. However, the use of a porous substrate may lead to strength deviations, cracks may occur due to the inclusion of a porous substrate, and ion conductivity may decrease.
[0008] In order to solve the above problems, the main purpose of this case is to provide a solid electrolyte sheet with improved strength, suppressed cracking, and improved ion conductivity, and a solid-state battery having a solid electrolyte layer with improved strength, suppressed cracking, and improved ion conductivity. And further, it helps to improve energy efficiency.
[0009] [Technical means to solve the problem]
[0010] The present inventors have found that in order to solve the above-mentioned problems, it is effective to adjust the particle size of the solid electrolyte material used in the inner layer and the outer layer and the amount of the binder in a solid electrolyte sheet having an inner layer and an outer layer, wherein the inner layer is formed by filling a solid electrolyte composition containing a solid electrolyte material and a binder in a porous substrate, and the outer layer is laminated on the surface of the inner layer and contains the solid electrolyte composition, thereby completing the present invention. Therefore, the present invention provides the following contents.
[0011] (1) A solid electrolyte sheet comprising an inner layer, a first outer layer laminated on one surface of the inner layer, and a second outer layer laminated on the other surface of the inner layer, wherein the inner layer comprises a porous substrate and an inner layer solid electrolyte composition filled in the porous substrate, the inner layer solid electrolyte composition comprises a solid electrolyte material and a binder, the first outer layer comprises a first outer layer solid electrolyte composition comprising a solid electrolyte material and a binder, the second outer layer comprises a second outer layer solid electrolyte composition comprising a solid electrolyte material and a binder, the inner layer solid electrolyte composition has a higher binder content than the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition, and the average particle size of the solid electrolyte material contained in the inner layer solid electrolyte composition is smaller than the average particle size of the solid electrolyte material contained in the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition.
[0012] According to the solid electrolyte sheet of (1), since the binder content of the inner layer solid electrolyte composition is high and the adhesion with the inner layer porous substrate is high, cracks are not easy to occur. On the other hand, since the binder content of the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition is low, the ion conductivity is improved. In addition, since the average particle size of the solid electrolyte material of the inner layer solid electrolyte composition is small, it is easy to fill it into the inner layer porous substrate and fill it with high density, so the strength of the solid electrolyte sheet and the effect of suppressing the occurrence of cracks are improved. Furthermore, since the average particle size of the solid electrolyte material of the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition is large, the lithium ion conductivity of the solid electrolyte sheet is improved. Therefore, according to the solid electrolyte sheet of (1), the strength is improved, the occurrence of cracks is suppressed, and the ion conductivity is improved.
[0013] (2) The solid electrolyte sheet according to (1), wherein the binder content of the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition is within a range of 1 / 10 to 9 / 10 of the binder content of the inner layer solid electrolyte composition.
[0014] According to the solid electrolyte sheet of (2), since the binder contents of the inner layer solid electrolyte composition, the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition are in the above-mentioned relationship, the strength of the solid electrolyte sheet, the effect of suppressing crack occurrence and the lithium ion conductivity are improved more balanced.
[0015] (3) The solid electrolyte sheet according to (2), wherein the binder content of the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition is within a range of 3 / 10 to 6 / 10 of the binder content of the inner layer solid electrolyte composition.
[0016] According to the solid electrolyte sheet of (3), since the binder contents of the inner layer solid electrolyte composition, the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition are in the above-mentioned relationship, the strength of the solid electrolyte sheet, the effect of suppressing crack occurrence and the lithium ion conductivity are further improved in a balanced manner.
[0017] (4) The solid electrolyte sheet according to any one of (1) to (3), wherein the binder content of the inner layer solid electrolyte composition is in the range of 3 to 20% by mass.
[0018] According to the solid electrolyte sheet of (4), since the binder content of the inner layer solid electrolyte composition is within the above range, the strength of the solid electrolyte sheet, the effect of suppressing crack occurrence, and the lithium ion conductivity are further improved in a balanced manner.
[0019] (5) The solid electrolyte sheet according to (4), wherein the inner layer solid electrolyte composition has a binder content in the range of 3 to 9% by mass.
[0020] According to the solid electrolyte sheet of (5), since the binder content of the inner layer solid electrolyte composition is within the above range, the lithium ion conductivity is further improved.
[0021] (6) The solid electrolyte sheet according to (5), wherein the thickness of the inner layer is in the range of 10 to 25 μm.
[0022] According to the solid electrolyte sheet of (6), since the thickness of the inner layer is within the above range, the lithium ion conductivity is further improved.
[0023] (7) The solid electrolyte sheet according to (4), wherein the inner layer solid electrolyte composition has a binder content in the range of 10 to 20% by mass.
[0024] According to the solid electrolyte sheet of (7), since the binder content of the inner layer solid electrolyte composition is within the above range, the strength of the solid electrolyte sheet is further improved.
[0025] (8) A solid electrolyte sheet according to any one of (1) to (7), wherein the peak of the particle size distribution of the solid electrolyte material contained in the aforementioned inner layer solid electrolyte composition is in a region with a particle size of less than 1 μm, and the peak of the particle size distribution of the solid electrolyte material contained in the aforementioned first outer layer solid electrolyte composition and the aforementioned second outer layer solid electrolyte composition is in a region with a particle size of less than 1 μm and a region with a particle size of more than 3 μm.
[0026] According to the solid electrolyte sheet of (8), since the inner layer solid electrolyte composition contains a large number of microparticles of solid electrolyte material with a particle size of 1 μm or less, it is easy to fill in the porous substrate of the inner layer. As a result, the strength of the solid electrolyte sheet and the effect of suppressing the occurrence of cracks are improved. In addition, since the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition contain microparticles of solid electrolyte material with a particle size of 1 μm or less and coarse particles of solid electrolyte material with a particle size of 3 μm or more, the first outer layer and the second outer layer are easy to become dense by interposing microparticles between coarse particles. As a result, the lithium ion conductivity of the solid electrolyte sheet is improved.
[0027] (9) The solid electrolyte sheet according to any one of (1) to (8), wherein the thickness of the inner layer is in the range of 2 to 30 μm, and the thickness of the first outer layer and the second outer layer is in the range of 1 / 5 to 2 times the thickness of the inner layer.
[0028] According to the solid electrolyte sheet of (9), since the thicknesses of the inner layer, the first outer layer and the second outer layer are within the above ranges, the strength, the effect of suppressing crack occurrence and the lithium ion conductivity are further improved in a balanced manner.
[0029] (10) The solid electrolyte sheet according to (9), wherein the thickness of the first outer layer and the second outer layer is thinner than the thickness of the inner layer.
[0030] According to the solid electrolyte sheet of (10), since the thickness of the first outer layer and the second outer layer is thinner than the thickness of the inner layer, the lithium ion conductivity is further improved.
[0031] (11) The solid electrolyte sheet according to (10), wherein the thickness of the first outer layer and the second outer layer is in a range of 1 / 5 to 4 / 5 times the thickness of the inner layer.
[0032] According to the solid electrolyte sheet of (11), since the relationship between the thicknesses of the inner layer, the first outer layer, and the second outer layer is within the above range, the lithium ion conductivity is further improved.
[0033] (12) The solid electrolyte sheet according to any one of (9) to (11), wherein the thickness of the inner layer is in the range of 10 to 25 μm.
[0034] According to the solid electrolyte sheet of (12), since the thickness of the inner layer is within the above range, the lithium ion conductivity is further improved and the resistance is reduced.
[0035] (13) An all-solid-state battery comprising a positive electrode, a negative electrode, and a solid electrolyte layer arranged between the positive electrode and the negative electrode, wherein the solid electrolyte layer is composed of a solid electrolyte sheet described in any one of (1) to (12) and is arranged at a position where the first outer layer is in contact with the positive electrode and the second outer layer is in contact with the negative electrode.
[0036] According to the all-solid-state battery of (13), since the solid electrolyte layer is composed of the above-mentioned solid electrolyte sheet, the strength of the solid electrolyte layer is improved, the occurrence of cracks is suppressed, and the ion conductivity is improved.
[0037] (Effects of the Invention)
[0038] According to the present invention, a solid electrolyte sheet having improved strength, suppressed cracking, and improved ion conductivity, and an all-solid-state battery having a solid electrolyte layer having improved strength, suppressed cracking, and improved ion conductivity can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a cross-sectional view schematically showing the structure of an all-solid-state battery according to one embodiment of the present invention.
[0040] Figure 2 This is a scanning electron microscope (SEM) photograph of a cross section of the inner layer of the solid electrolyte sheet obtained in Example 1.
[0041] Figure 3 This is a cross-sectional SEM photograph of the first outer layer of the solid electrolyte sheet obtained in Example 1. DETAILED DESCRIPTION
[0042] Hereinafter, embodiments of the present invention will be described.
[0043] Figure 1 1 is a cross-sectional view of an all-solid-state battery 1 according to an embodiment of the present invention. Figure 1As shown, the all-solid battery 1 includes a positive electrode 10, a negative electrode 20 and a solid electrolyte layer 30. The all-solid battery 1 is a laminated body in which the positive electrode 10, the solid electrolyte layer 30 and the negative electrode 20 are laminated in sequence. The all-solid battery 1 of the embodiment is a lithium ion all-solid battery. In addition, the all-solid battery mentioned in this specification refers to a battery made of a fully solid battery.
[0044] The positive electrode 10 includes a positive electrode layer 11 and a positive electrode current collector 12. The positive electrode layer 11 is disposed on the solid electrolyte layer 30 side. The positive electrode current collector 12 constitutes the surface of the positive electrode 10 side in the all-solid battery 1.
[0045] The positive electrode layer 11 contains a positive electrode active material. The positive electrode active material used in the positive electrode layer 11 is not particularly limited, as long as it is a material that functions as the positive electrode of the all-solid-state battery 1. In addition, as specific positive electrode active materials, for example, if it is a sulfide system, titanium sulfide (TiS2), molybdenum sulfide (MoS2), iron sulfide (FeS, FeS2), copper sulfide (CuS) and nickel sulfide (Ni3S2) can be listed. In addition, if it is an oxide system, bismuth oxide (Bi2O3), bismuth lead oxide (Bi2Pb2O5), copper oxide (CuO), vanadium oxide (V6O 13 ), lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2), Li(NiCoMn)O2, Li(NiCoAl)O2, Li(NiCo)O2, etc. In addition, these may be mixed and used.
[0046] The positive electrode current collector 12 has the function of collecting electricity for the positive electrode layer 11. The positive electrode current collector 12 is a foil-shaped member made of an electrode material having conductivity. The electrode material used in the positive electrode current collector 12 is not particularly limited as long as it is a conductive material, and examples thereof include vanadium, aluminum, stainless steel, gold, platinum, manganese, iron, titanium, etc., among which aluminum is preferred. The shape and thickness of the positive electrode current collector 12 are not particularly limited as long as they are capable of collecting electricity for the positive electrode layer 11.
[0047] The negative electrode 20 includes a negative electrode layer 21 and a negative electrode current collector 22. The negative electrode layer 21 is disposed on the solid electrolyte layer 30 side. The negative electrode current collector 22 constitutes the surface of the negative electrode 20 side in the all-solid battery 1.
[0048] The negative electrode layer 21 may contain a negative electrode active material. The negative electrode active material used in the negative electrode layer 21 is not particularly limited, as long as it is a material that functions as the negative electrode of the all-solid-state battery 1, but it is preferably at least one of a Li-based material and a Si material. In addition, as a specific negative electrode active material, for example, carbon materials can be listed, specifically artificial graphite, graphite carbon fiber, resin calcined carbon, pyrolysis vapor deposited carbon, coke, secondary carbon microbeads (meso carbon microbeads, MCMB), furfuryl alcohol resin calcined carbon, polyacene, pitch-based carbon fiber, vapor deposited carbon fiber, natural graphite, difficult graphitization carbon, etc. Or, it can also be a mixture of them. In addition, as a negative electrode active material, a metal that forms an alloy with lithium or an alloy formed by combining these metals with other elements or compounds can be used. As a metal that forms an alloy with lithium, for example, metal indium, metal aluminum or metal silicon can be listed. Further, as the negative electrode layer 21, metallic lithium can be used.
[0049] The negative electrode current collector 22 has the function of collecting electricity from the negative electrode layer 21. The negative electrode current collector 22 is a foil-shaped member composed of an electrode material having conductivity. The electrode material used in the negative electrode current collector 22 is not particularly limited as long as it is a conductive material, and examples thereof include vanadium, stainless steel, manganese, iron, titanium, copper, nickel, cobalt, zinc, etc. Among them, copper and nickel are preferred due to their excellent conductivity and excellent current collection. The shape and thickness of the negative electrode current collector 22 are not particularly limited as long as they are capable of collecting electricity from the negative electrode layer 21.
[0050] The solid electrolyte layer 30 includes an inner layer 31, a first outer layer 32 laminated on one surface of the inner layer 31, and a second outer layer 33 laminated on the other surface of the inner layer 31. The first outer layer 32 is arranged at a position where the positive electrode 10 is in contact with the second outer layer 33 and the negative electrode 20 is in contact with the positive electrode 20. The thickness of the inner layer 31 may be, for example, in the range of 2 to 30 μm, or in the range of 10 to 25 μm. The thickness of the first outer layer 32 and the second outer layer 33 may be, for example, in the range of 1 / 5 to 2 times the thickness of the inner layer 31. From the viewpoint of improving the lithium ion conductivity of the solid electrolyte layer 30, the thickness of the first outer layer 32 and the second outer layer 33 may be thinner than the thickness of the inner layer 31, and the thickness of the first outer layer 32 and the second outer layer 33 may be in the range of 1 / 5 to 4 / 5 times the thickness of the inner layer 31.
[0051] The inner layer 31 includes a porous substrate (not shown) and an inner layer solid electrolyte composition (not shown) filled in the porous substrate. The inner layer 31 may also be composed only of a porous substrate filled with an inner layer solid electrolyte composition. The inner layer solid electrolyte composition contains a solid electrolyte material and a binder. The inner layer solid electrolyte composition may also be composed only of a solid electrolyte material and a binder.
[0052] The first outer layer 32 includes a first outer layer solid electrolyte composition, which contains a solid electrolyte material and a binder. The first outer layer 32 may also be composed only of the first outer layer solid electrolyte composition. The second outer layer 33 includes a second outer layer solid electrolyte composition, which contains a solid electrolyte material and a binder. The second outer layer 33 may also be composed only of the second outer layer solid electrolyte composition. The first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition may also be composed only of a solid electrolyte material and a binder. The first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition may also be the same.
[0053] The porous substrate contained in the inner layer 31 is preferably a woven fabric or a non-woven fabric. If it is a woven fabric or a non-woven fabric, it has an appropriate porosity and thickness, and it is easy to fill the inner layer solid electrolyte composition. There is no particular limitation on the material of the porous substrate, as long as it can be a material that can form an independent sheet. For example, polyethylene terephthalate (PET), polyamide (nylon), aromatic polyamide (aramid), Al2O3, glass, etc. can be listed. In addition, as a porous substrate, it is preferably composed of heat-resistant fibers. By forming the porous substrate with heat-resistant fibers, in the manufacturing process of the all-solid battery 1, for example, even if pressing is performed at a high temperature exceeding 200°C, short circuits can be suppressed. In addition, the solid electrolyte layer 30 can be sintered by high-temperature pressing, as a result, the interface resistance decreases, and the output of the battery can be increased. The porosity of the porous substrate can be in the range of 65 to 90%. When the porosity is within this range, the inner layer solid electrolyte composition can be easily filled into the porous substrate.
[0054] The same substance may be used as the solid electrolyte material and the binder contained in the inner layer solid electrolyte composition contained in the inner layer 31, the first outer layer solid electrolyte composition contained in the first outer layer 32, and the second outer layer solid electrolyte composition contained in the second outer layer 33. By using the same substance, the adhesion between the inner layer 31 and the first outer layer 32 and the second outer layer 33 becomes high.
[0055] The solid electrolyte material is not particularly limited as long as it can conduct lithium ions between the positive electrode 10 and the negative electrode 20. As the solid electrolyte material, for example, an oxide-based electrolyte or a sulfide-based electrolyte can be used. The solid electrolyte material preferably contains a lithium element. Among them, it is preferably a substance synthesized by the following compounds: as a first component, at least lithium sulfide is included, and as a second component, a substance synthesized by one or more compounds selected from the group consisting of silicon sulfide, phosphorus sulfide and boron sulfide; in terms of lithium ion conductivity, Li2S-P2S5 is particularly preferred.
[0056] When the solid electrolyte material is a sulfide-based electrolyte, it may further contain sulfides such as SiS2, GeS2, B2S3, etc. In addition, Li3PO4, halogen, halogen compound, etc. may be appropriately added to the solid electrolyte.
[0057] When the solid electrolyte material is a lithium ion conductor composed of an inorganic compound, examples thereof include Li3N, LISICON, LIPON (Li 3+y PO 4-x N x )、Thio-LISICON(Li 3.25 Ge 0.25 P 0.75 S4), Li2O-Al2O3-TiO2-P2O5 (LATP), etc.
[0058] The solid electrolyte material may also have an amorphous, glassy, crystalline (crystallized glass) or other structure. In the case where the solid electrolyte material is a sulfide-based solid electrolyte composed of Li2S-P2S5, the lithium ion conductivity of the amorphous body is 10 -4 Scm -1 On the other hand, the lithium ion conductivity in the case of a crystalline body is 10 -3 Scm -1 about.
[0059] The solid electrolyte material preferably contains at least one of phosphorus and sulfur. This can improve the lithium ion conductivity of the obtained all-solid battery 1.
[0060] The binder is attached to the porous substrate of the inner layer 31, the positive electrode 10 and the negative electrode 20, and a solid electrolyte material can be attached. As the binder, for example, it is preferred to include a binder resin showing adhesiveness. As the binder, for example, fluorine polymers, (meth) acrylic thermoplastic resins, silicone resins, urethane resins, nitrile resins, polyester resins, cellulose resins, styrene resins, styrene butadiene resins, vinyl acetate resins, fluoroethylene resins, polyvinyl ethers, rubbers, etc. can be cited. In addition, the so-called "(meth) acrylic acid" is a general term for acrylic acid and methacrylic acid.
[0061] Compared with the first outer layer solid electrolyte composition contained in the first outer layer 32 and the second outer layer solid electrolyte composition contained in the second outer layer 33, the binder content of the inner layer solid electrolyte composition contained in the inner layer 31 of the solid electrolyte layer 30 is higher. Since the binder content of the inner layer solid electrolyte composition is high, the adhesion with the porous substrate becomes higher. As a result, the strength of the solid electrolyte layer 30 is improved. On the other hand, since the binder content of the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition is low, the ion conductivity of the first outer layer 32 and the second outer layer 33 is improved. Therefore, according to the all-solid battery 1 of this embodiment, it is possible to take into account both the improvement in the strength of the solid electrolyte layer 30 brought about by the porous substrate and the improvement in lithium ion conductivity.
[0062] The binder content of the inner layer solid electrolyte composition is not particularly limited and can be in the range of 3 to 20% by mass. The binder content of the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition is not particularly limited and can be in the range of 1 / 10 to 9 / 10 of the binder content of the inner layer solid electrolyte composition, or in the range of 3 / 10 to 6 / 10. If the binder content of the inner layer solid electrolyte composition, the first outer layer solid electrolyte composition, and the second outer layer solid electrolyte composition is within the above range, the strength and lithium ion conductivity of the solid electrolyte layer 30 will be improved more balanced. From the viewpoint of improving the lithium ion conductivity of the solid electrolyte layer 30, the binder content of the inner layer solid electrolyte composition can also be in the range of 3 to 8% by mass. From the viewpoint of improving the strength of the solid electrolyte layer 30, the binder content of the inner layer solid electrolyte composition can also be in the range of 10 to 20% by mass.
[0063] In the present embodiment, the average particle size of the solid electrolyte material contained in the inner layer solid electrolyte composition is smaller than the average particle size of the solid electrolyte material contained in the aforementioned first outer layer solid electrolyte composition and the aforementioned second outer layer solid electrolyte composition. Solid electrolyte materials with small average particle size are easy to fill in porous substrates because the number of particles that can be filled per unit volume is large. Therefore, by reducing the average particle size of the solid electrolyte material contained in the inner layer solid electrolyte composition, the solid electrolyte material can be filled in the porous substrate of the inner layer 31 at a high density. On the other hand, since the number of contact points between particles per unit volume increases, the lithium ion conductivity tends to deteriorate. Therefore, by increasing the average particle size of the solid electrolyte material contained in the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition, the ion conductivity of the first outer layer 32 and the second outer layer 33 is improved. The average particle size of the solid electrolyte material contained in the inner layer solid electrolyte composition can be in the range of 0.5 to 1.5 μm, or in the range of 0.5 to 1.0 μm. In addition, the average particle size of the solid electrolyte material contained in the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition may be in the range of 2.0 to 10.0 μm, or in the range of 2.0 to 5.0 μm. The particle size of the solid electrolyte material is the longest diameter of the solid electrolyte material measured from a cross-sectional SEM photograph of the cross-section of the solid electrolyte layer 30 taken using a SEM (scanning electron microscope), and the average particle size is the number average value.
[0064] The particle size distribution of the solid electrolyte material contained in the inner layer solid electrolyte composition may have a peak in the region with a particle size of 1 μm or less. In addition, the particle size distribution may also be a particle size distribution based on the number of the longest diameter of the solid electrolyte material measured from the cross-sectional SEM photograph of the solid electrolyte layer 30. In this case, the inner layer solid electrolyte composition is easy to fill in the porous substrate of the inner layer 31 because it contains a large number of solid electrolyte material microparticles with a particle size of 1 μm or less. Thus, the strength of the solid electrolyte layer 30 is improved. In addition, the particle size distribution of the solid electrolyte material contained in the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition may have a peak in the region with a particle size of 1 μm or less and in the region with a particle size of 3 μm or more. In this case, the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition contain solid electrolyte material microparticles with a particle size of 1 μm or less and solid electrolyte material coarse particles with a particle size of 3 μm or more, so the microparticles intervene between the coarse particles, so that the first outer layer 32 and the second outer layer 33 are easy to become dense. Thus, the lithium ion conductivity of the solid electrolyte layer 30 is improved. Furthermore, the upper limit of the particle size of the solid electrolyte material contained in the first outer layer 32 and the second outer layer 33 is equal to or less than the thickness of the first outer layer 32 and the second outer layer 33 .
[0065] For example, the all-solid-state battery 1 can be manufactured by placing the first outer layer 32 of a solid electrolyte sheet (solid electrolyte layer 30) in which the first outer layer 32, the inner layer 31, and the second outer layer 33 are sequentially stacked on the positive electrode layer 11 of a positive electrode sheet (positive electrode 10) in which the positive electrode layer 11 and the positive electrode collector 12 are stacked, and then placing the negative electrode layer 21 of a negative electrode sheet (negative electrode 20) in which the negative electrode layer 21 and the negative electrode collector 22 are stacked on the solid electrolyte sheet, and then performing press bonding. As the press bonding, high-temperature press bonding at more than 200° C. can be performed.
[0066] For example, a solid electrolyte sheet can be manufactured by the following methods (1) to (3) using a porous substrate, an inner layer forming slurry for forming the inner layer 31, and an outer layer forming slurry for forming the first outer layer and the second outer layer. The inner layer forming slurry and the outer layer forming slurry respectively contain a solvent, a solid electrolyte, and a binder. The inner layer forming slurry contains a larger amount of binder than the outer layer forming slurry.
[0067] (1) Impregnation (dipping) method
[0068] The porous substrate is impregnated with the inner layer forming slurry, and then the porous substrate is pulled up from the inner layer forming slurry, and then dried to form an inner layer component having a porous substrate (inner layer 31) filled with an inner layer solid electrolyte composition. Next, the obtained inner layer component is impregnated with the outer layer forming slurry, and then the inner layer component is pulled up from the outer layer forming slurry, and then dried to form outer layers (first outer layer 32, second outer layer 33) on both sides of the inner layer 31 of the inner layer component.
[0069] (2) Coating method
[0070] The outer layer forming slurry is applied to the support sheet and dried to form the first outer layer 32. Next, the inner layer forming slurry is applied to the first outer layer 32, and then a porous substrate is arranged on the coating layer of the inner layer forming slurry, so that the porous substrate absorbs the coating layer, and then dried to form a porous substrate (inner layer 31) filled with an inner layer solid electrolyte composition. Next, the outer layer forming slurry is applied to the inner layer 31 and dried to form the second outer layer 33. As a support sheet, for example, aluminum foil or stainless steel foil can be used. As a coating method for the outer layer forming slurry and the inner layer forming slurry, for example, a die coating method can be used.
[0071] (3) Transfer method
[0072] An inner layer sheet having an inner layer 31 formed by filling an inner layer solid electrolyte composition in a porous substrate is prepared. In addition, an outer layer transfer sheet formed by forming a peelable outer layer (first outer layer 32, second outer layer 33) on a supporting sheet is prepared. For example, the inner layer sheet can be obtained by the following method: impregnating the porous substrate with an inner layer forming slurry, then pulling the porous substrate from the inner layer forming slurry, and then drying it, or applying the inner layer forming slurry to the porous substrate, followed by drying. For example, the outer layer transfer sheet can be obtained by the following method: applying an outer layer forming slurry on a supporting sheet, followed by drying. As a supporting sheet, for example, aluminum foil or stainless steel foil can be used.
[0073] The outer layer transfer sheet is disposed on both sides of the inner layer sheet, and the outer layers (first outer layer 32 and second outer layer 33) are transferred to both sides of the inner layer 31 by pressing to form an integrated whole, and then the supporting sheet is peeled off and removed.
[0074] Compared with (2) coating method and (3) transfer method, (1) impregnation method can easily reduce the amount of adhesive. On the other hand, compared with (1) impregnation method, (2) coating method and (3) transfer method can easily adjust the film thickness of the outer layer (first outer layer 32, second outer layer 33).
[0075] The solid electrolyte layer 30 used in the all-solid-state battery 1 of the present embodiment is not prone to cracking due to the high binder content of the inner layer solid electrolyte composition contained in the inner layer 31 and the high adhesion to the porous substrate of the inner layer 31. On the other hand, since the binder content of the first outer layer solid electrolyte composition contained in the first outer layer 32 and the second outer layer solid electrolyte composition contained in the second outer layer 33 is low, the ion conductivity is improved. In addition, since the average particle size of the solid electrolyte material of the inner layer solid electrolyte composition is small, it is easy to fill it into the porous substrate of the inner layer 31 and fill it at a high density, so the strength of the solid electrolyte layer 30 and the effect of suppressing the occurrence of cracks are improved. Furthermore, since the average particle size of the solid electrolyte material of the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition is large, the lithium ion conductivity of the solid electrolyte layer 30 is improved. As a result, the strength of the solid electrolyte layer 30 is improved, the occurrence of cracks is suppressed, and the ion conductivity is improved.
[0076] Furthermore, since the all-solid-state battery 1 of the present embodiment includes the above-described solid electrolyte layer 30 , stability and charge / discharge efficiency are improved over a long period of time.
[0077] The above describes the specific embodiments of the present invention, but the present invention is not limited to the above embodiments, and deformation, improvement, etc. within the scope of achieving the purpose of the present invention are also included in the scope of the present invention. For example, in the present embodiment, as a method for manufacturing an all-solid-state battery 1, a method of pressing and joining a stacked body in which each layer is sequentially arranged as a whole is exemplified, but the method for manufacturing an all-solid-state battery 1 is not limited to this. For example, the all-solid-state battery 1 can also be manufactured in the following manner. First, the positive electrode layer 11 of the positive electrode sheet stacked with the positive electrode layer 11 and the positive electrode collector 12 and the first outer layer sheet are pressed and joined to produce a positive electrode-first outer layer stacked sheet, and the negative electrode layer 21 of the negative electrode sheet stacked with the negative electrode layer 21 and the negative electrode collector 22 and the second outer layer sheet are pressed and joined to produce a negative electrode-second outer layer stacked sheet. Next, an inner layer sheet is prepared, and the first outer layer 32 of the positive electrode-first outer layer laminated sheet is press-bonded on one surface of the inner layer sheet, and the second outer layer 33 of the negative electrode-second outer layer laminated sheet is press-bonded on the other surface of the inner layer sheet. In this way, an electrode laminate sheet in which the positive electrode sheet, the solid electrolyte sheet, and the negative electrode sheet are stacked in sequence is obtained. The binder content of the inner layer solid electrolyte composition of the inner layer sheet can be in the range of 10 to 20% by mass. The average particle size of the solid electrolyte contained in the inner layer solid electrolyte composition can be in the range of 0.5 to 1.0 μm. The thickness of the inner layer sheet can be in the range of 5 to 15 μm. The binder content of the outer layer solid electrolyte composition of the first outer layer sheet and the second outer layer sheet can be in the range of 5 to 20% by mass. The average particle size of the solid electrolyte contained in the outer layer solid electrolyte composition can be in the range of 2.0 to 5.0 μm. The thickness of the first outer layer sheet and the second outer layer sheet can be in the range of 5 to 20 μm.
[0078] [Example]
[0079] [Example 1]
[0080] (Fabrication of Solid Electrolyte Sheet)
[0081] 51 parts by mass of fine powder of sulfide-based solid electrolyte (average particle size: 0.7 μm) and 3 parts by mass of styrene butadiene rubber (SBR)-based binder were added to 46 parts by mass of solvent and mixed to prepare slurry for inner layer formation. In addition, 10.5 parts by mass of fine powder of sulfide-based solid electrolyte (average particle size: 0.7 μm), 41.9 parts by mass of coarse powder of sulfide-based solid electrolyte (average particle size: 3.0 μm) and 1.6 parts by mass of SBR-based binder were added to 46 parts by mass of solvent and mixed to prepare slurry for outer layer formation.
[0082] The nonwoven fabric (material: PET, thickness: 10 μm, porosity: 75%, average fiber diameter: 3.0 μm) was immersed in the slurry for forming the inner layer, and after being pulled up from the slurry for forming the inner layer, it was dried. In this way, an inner layer component was prepared in which the inner layer solid electrolyte composition containing microparticles of a sulfide-based solid electrolyte and a binder were filled in the nonwoven fabric. The thickness of the obtained inner layer component was 30 μm. The obtained inner layer component was immersed in the slurry for forming the outer layer, and after being pulled up from the slurry for forming the outer layer, it was dried. In this way, a three-layer solid electrolyte sheet was prepared in which an outer layer (thickness: 20 μm) containing an outer layer composition was stacked on both sides of the inner layer, and the outer layer composition contained fine powder and coarse powder of a sulfide-based solid electrolyte and a binder.
[0083] The cross section of the obtained solid electrolyte sheet was observed using a SEM (scanning electron microscope). Figure 2 A cross-sectional SEM photograph of the inner layer of the solid electrolyte sheet is shown in FIG. Figure 3 A cross-sectional SEM photograph of the first outer layer of the solid electrolyte sheet layer is shown in FIG. Figure 2 The cross-sectional SEM photograph of 31 confirms that in the inner layer 31, the sulfide-based solid electrolyte particles 301 are closely attached to the periphery of the PET fibers 311 of the non-woven fabric, and the sulfide-based solid electrolyte particles 301 are densely filled inside the non-woven fabric. Figure 3 It is confirmed from the cross-sectional SEM photograph that the first outer layer 32 is formed with a sulfide-based solid electrolyte layer by interposing the sulfide-based solid electrolyte fine particles 301 between the sulfide-based solid electrolyte coarse particles 302 .
[0084] Example 2
[0085] A fine powder of a sulfide solid electrolyte (average particle size: 0.7 μm) and an SBR-based binder were mixed in a solvent at a ratio of 3% by mass of the SBR-based binder content in the solid component to prepare a slurry for forming an inner layer. A nonwoven fabric (material: PET, thickness: 10 μm, porosity: 75%, average fiber diameter: 3.0 μm) was immersed in the slurry for forming an inner layer, and pulled up from the slurry for forming an inner layer, and the slurry for forming an inner layer was attached to the nonwoven fabric, and then dried to obtain an inner layer component with a thickness of 30 μm.
[0086] A coarse powder of a sulfide-based solid electrolyte (average particle size: 3.0 μm) and an SBR-based binder were mixed in a solvent at a ratio of 1.6% by mass of the SBR-based binder in the solid component to prepare an outer layer forming slurry. An inner layer component was immersed in the outer layer forming slurry and pulled up from the inner layer forming slurry, and the outer layer forming slurry was attached to the inner layer component, followed by drying to produce a solid electrolyte sheet having an inner layer thickness of 30 μm and a first outer layer and a second outer layer thickness of 20 μm.
[0087] [Examples 3 and 4]
[0088] A solid electrolyte sheet was prepared in the same manner as in Example 2 except that the inner layer forming slurry and the outer layer forming slurry were attached so that the thickness of the inner layer would be as shown in Table 1 below.
[0089] [Comparative Example 1]
[0090] A solid electrolyte sheet was prepared in the same manner as in Example 2 except that a slurry containing a coarse powder of a sulfide solid electrolyte (average particle size: 3.0 μm) and an SBR-based binder in such a ratio that the content of the SBR-based binder in the solid content was 1.6 mass % (the slurry used as the slurry for forming the outer layer in Example 2) was used as the slurry for forming the inner layer, and a slurry containing a fine powder of a sulfide solid electrolyte (average particle size: 0.7 μm) and an SBR-based binder in such a ratio that the content of the SBR-based binder in the solid content was 3.0 mass % (the slurry used as the slurry for forming the inner layer in Example 2) was used as the slurry for forming the outer layer.
[0091] [evaluate]
[0092] (1) Section observation
[0093] The cross-sections of the solid electrolyte sheets obtained in Examples 1 to 3 were observed using SEM. The results confirmed that the sulfide-based solid electrolyte fine particles were densely filled inside the non-woven fabric of the inner layer. In addition, it was confirmed that the first outer layer was formed with a sulfide-based solid electrolyte layer by interposing the sulfide-based solid electrolyte fine particles 301 between the sulfide-based solid electrolyte coarse particles 302.
[0094] (2) Performance evaluation of all-solid-state battery cells
[0095] Using each of the above-mentioned solid electrolyte sheets, an all-solid-state battery cell was produced according to the following procedure.
[0096] [Production of positive electrode sheet]
[0097] Prepare an aluminum foil with a thickness of 12.0 μm as a positive electrode collector. Mix in the following proportions: 60.0 parts by mass of lithium nickel cobalt manganese composite oxide (NCM 622) as a positive electrode active material, 35.8 parts by mass of a sulfide solid electrolyte as a solid electrolyte, 2.9 parts by mass of acetylene black (DENKA BLACK Li-100, manufactured by DENKA Co., Ltd.) as a conductive aid, and 1.3 parts by mass of an SBR (styrene butadiene rubber)-based binder. Disperse the obtained mixture in a solvent to prepare a positive electrode active material slurry. Use a rod coater to make the unit area weight after drying to be 27.4 mg / cm 2 The obtained positive electrode active material slurry is applied to both sides of the positive electrode collector in a manner and dried to form a positive electrode layer to produce a positive electrode sheet.
[0098] [Production of negative electrode sheet]
[0099] A copper foil with a thickness of 10 μm was prepared as a negative electrode current collector, and a metal lithium foil with a thickness of 6.5 μm was laminated on the surface of the copper foil as a negative electrode layer to prepare a negative electrode sheet.
[0100] [Fabrication of all-solid-state battery cells]
[0101] The positive electrode sheet, solid electrolyte sheet, and negative electrode sheet obtained as above were cut into a size of 120 mm×30 mm, and the positive electrode sheet, solid electrolyte sheet, and negative electrode sheet obtained were stacked and pressed to form an electrode stack. The obtained electrode stack was used to make a solid-state battery cell.
[0102] [Single Cell Charge and Discharge Test]
[0103] Using the all-solid-state battery cells obtained as described above, charge and discharge tests were performed in the range of 2.65 to 4.3 V. The second charge and discharge capacity was 95% or more of the first charge and discharge capacity and was considered "passed". The capacity less than 95% was considered "failed". The results are shown in Table 1.
[0104] [Single resistor]
[0105] After the above-mentioned charge and discharge test, the all-solid-state battery cell was charged to a SOC (charge rate) of 50%, and then the cell resistance was measured.
[0106] [Table 1]
[0107]
[0108] From the results in Table 1, it can be seen that the binder content of the solid electrolyte sheets of Examples 2 to 4 and the average particle size of the solid electrolyte material are within the range of the present invention, and the all-solid battery monomer using the solid electrolyte sheets of Examples 2 to 4 has high second cycle charge and discharge efficiency and low monomer resistance. In particular, it can be seen that the thickness of the inner layer of the solid electrolyte sheets of Examples 3 to 4 is 25 μm or less, and the thickness of the first outer layer and the second outer layer is 7 μm or less, and the monomer resistance of the all-solid battery monomer using the solid electrolyte sheets of Examples 3 to 4 is further reduced. On the other hand, the binder content of the inner layer solid electrolyte composition of the solid electrolyte sheet of Comparative Example 1 is low, and the average particle size of the solid electrolyte material contained in the inner layer solid electrolyte composition is large, and the all-solid battery monomer using the solid electrolyte sheet of Comparative Example 1 is short-circuited at the time of the second cycle, and cannot be charged and discharged.
[0109] [Example 5]
[0110] The following sheets were prepared as the first outer layer sheet and the second sheet: a sheet containing a coarse powder of a sulfide-based solid electrolyte (average particle size: 3.0 μm) and a thickness of 7 μm of an SBR-based binder at a ratio of 5.0% by mass of the SBR-based binder. The following sheets were prepared as the inner layer sheet: a sheet containing a fine powder of a sulfide-based solid electrolyte (average particle size: 0.7 μm) and a thickness of 10 μm of an SBR-based binder at a ratio of 10% by mass of the SBR-based binder.
[0111] The positive electrode layer of the positive electrode sheet produced in the performance evaluation of the above-mentioned all-solid-state battery cell is pressed and bonded to the first outer layer sheet to produce a positive electrode-first outer layer laminated sheet. Similarly, the negative electrode layer 21 of the negative electrode sheet produced in the performance evaluation of the above-mentioned all-solid-state battery cell is pressed and bonded to the second outer layer sheet to produce a negative electrode-second outer layer laminated sheet. Next, the first outer layer of the positive electrode-first outer layer laminated sheet is press-bonded on one surface of the inner layer sheet, and the second outer layer of the negative electrode-second outer layer laminated sheet is press-bonded on the other surface of the inner layer sheet to obtain an electrode laminate sheet in which the positive electrode sheet, the solid electrolyte sheet, and the negative electrode sheet are stacked in sequence. The obtained electrode laminate sheet is cut into a size of 120 mm × 30 mm, and the obtained electrode laminate is used to produce an all-solid-state battery cell.
[0112] [Example 6, Comparative Examples 2-3]
[0113] The following sheets are used as the first outer layer sheet and the second outer layer sheet: a sheet containing a sulfide-based solid electrolyte and an SBR-based binder having an average particle size as recorded in Table 2 below, with the SBR-based binder content being in a ratio to the value recorded in Table 2 below; the following sheets are used as the inner layer sheet: a sheet containing a sulfide-based solid electrolyte and an SBR-based binder having an average particle size as recorded in Table 2 below, with the SBR-based binder content being in a ratio to the value recorded in Table 2 below; except for this, an all-solid-state battery monomer is prepared in the same manner as in Example 5.
[0114] [evaluate]
[0115] The all-solid-state battery cells obtained in Examples 5 and 6 and Comparative Examples 2 and 3 were evaluated in the same manner as the above-mentioned performance evaluation of the all-solid-state battery cells. The results are shown in Table 2 below.
[0116] [Table 2]
[0117]
[0118] As can be seen from the results in Table 2, the binder content of the solid electrolyte sheets of Examples 5 to 6 and the average particle size of the solid electrolyte material are within the range of the present invention, and the all-solid battery cells using the solid electrolyte sheets of Examples 5 to 6 have high charge and discharge efficiency in the second cycle and low cell resistance. On the other hand, the binder content of the inner layer solid electrolyte composition of the solid electrolyte sheets of Comparative Examples 2 to 3 is low, and the average particle size of the solid electrolyte material contained in the inner layer solid electrolyte composition is large. Although the all-solid battery cells using the solid electrolyte sheets of Comparative Examples 2 to 3 have high charge and discharge efficiency in the second cycle, the cell resistance becomes high.
[0119] Reference numerals
[0120] 1 All-solid-state battery
[0121] 10 Positive electrode
[0122] 11. Positive electrode layer
[0123] 12. Positive electrode collector
[0124] 20 Negative electrode
[0125] 21 Negative electrode layer
[0126] 22 Negative electrode collector
[0127] 30 Solid electrolyte layer
[0128] 31 Inner layer
[0129] 32 First outer layer
[0130] 33 Second outer layer
[0131] 301 Sulfide-based solid electrolyte microparticles
[0132] 302 Sulfide-based solid electrolyte coarse particles
[0133] 311 PET fiber for non-woven fabrics
Claims
1. A solid electrolyte sheet comprising an inner layer, a first outer layer laminated on one surface of the inner layer, and a second outer layer laminated on the other surface of the inner layer, The inner layer comprises a porous substrate and an inner layer solid electrolyte composition filled in the porous substrate, wherein the inner layer solid electrolyte composition contains a solid electrolyte material and a binder. The first outer layer comprises a first outer layer solid electrolyte composition comprising a solid electrolyte material and a binder. The second outer layer comprises a second outer layer solid electrolyte composition containing a solid electrolyte material and a binder, The inner layer solid electrolyte composition has a higher binder content than the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition. The average particle size of the solid electrolyte material contained in the inner layer solid electrolyte composition is smaller than the average particle size of the solid electrolyte material contained in the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition.
2. The solid electrolyte sheet according to claim 1, in, The binder content of the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition is within a range of 1 / 10 to 9 / 10 of the binder content of the inner layer solid electrolyte composition.
3. The solid electrolyte sheet according to claim 2, in, The binder content of the first outer layer solid electrolyte composition and the second outer layer solid electrolyte composition is within a range of 3 / 10 to 6 / 10 of the binder content of the inner layer solid electrolyte composition.
4. The solid electrolyte sheet according to claim 1, in, The binder content of the inner layer solid electrolyte composition is in the range of 3 to 20% by mass.
5. The solid electrolyte sheet according to claim 4, in, The binder content of the inner layer solid electrolyte composition is in the range of 3 to 9% by mass.
6. The solid electrolyte sheet according to claim 5, in, The thickness of the inner layer is in the range of 10 to 25 μm.
7. The solid electrolyte sheet according to claim 4, in, The binder content of the inner layer solid electrolyte composition is in the range of 10 to 20% by mass.
8. The solid electrolyte sheet according to claim 1, in, The peak of the particle size distribution of the solid electrolyte material contained in the aforementioned inner layer solid electrolyte composition is in the region with a particle size of less than 1 μm, and the peak of the particle size distribution of the solid electrolyte material contained in the aforementioned first outer layer solid electrolyte composition and the aforementioned second outer layer solid electrolyte composition is in the region with a particle size of less than 1 μm and in the region with a particle size of more than 3 μm.
9. The solid electrolyte sheet according to claim 1, in, The thickness of the inner layer is in the range of 2 to 30 μm, and the thickness of the first outer layer and the second outer layer is in the range of 1 / 5 to 2 times the thickness of the inner layer.
10. The solid electrolyte sheet according to claim 9, in, The thickness of the first outer layer and the second outer layer is thinner than the thickness of the inner layer.
11. The solid electrolyte sheet according to claim 10, in, The thickness of the first outer layer and the second outer layer is in the range of 1 / 5 to 4 / 5 times the thickness of the inner layer.
12. The solid electrolyte sheet according to claim 9, in, The thickness of the inner layer is in the range of 10 to 25 μm.
13. An all-solid-state battery comprising a positive electrode, a negative electrode, and a solid electrolyte layer disposed between the positive electrode and the negative electrode, The solid electrolyte layer is composed of the solid electrolyte sheet according to any one of claims 1 to 5, and is disposed at a position where the first outer layer is in contact with the positive electrode and the second outer layer is in contact with the negative electrode.