Secondary battery and electronic device
Patent Information
- Application Number
- CN202410707511.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-31
- Publication Date
- 2024-10-01
AI Technical Summary
During the cycling process of existing lithium-ion batteries, there are many side reactions between the positive electrode plate and the electrolyte, and between the negative electrode plate and the electrolyte. The initial impedance is large, which affects the dynamic performance and high-temperature float performance.
By designing the negative electrode plate structure and electrolyte components, regulating the thickness of the negative electrode material layer and the proportion of electrolyte components, we can improve the wettability of the electrolyte and the solubility of lithium salt, reduce side reactions, optimize conductivity, and thereby reduce impedance.
It effectively reduces the initial impedance of secondary batteries and the impedance growth during cycling, and improves the dynamic performance and high-temperature float performance.
Smart Images

Figure CN118738631A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of electrochemical technology, and in particular to a secondary battery and an electronic device. Background Art
[0002] Secondary batteries, such as lithium-ion batteries, are widely used in smart phones, wearable devices, consumer drones, electric vehicles and other fields due to their high energy density, long cycle life and no memory effect. With the widespread application of lithium-ion batteries in the above fields, the market has higher and higher requirements for the dynamic performance and high-temperature floating charge performance of lithium-ion batteries.
[0003] However, during the cycle of existing lithium-ion batteries, there are many side reactions between the positive electrode plate and the electrolyte, and between the negative electrode plate and the electrolyte, resulting in a large initial impedance. During the cycle of the lithium-ion battery, the impedance growth is also large, which affects the kinetic performance and high-temperature floating charge performance of the lithium-ion battery. Summary of the invention
[0004] The purpose of this application is to provide a secondary battery and an electronic device to improve the dynamic performance and high-temperature floating charge performance of the secondary battery. The specific technical solution is as follows:
[0005] The first aspect of the present application provides a secondary battery, which includes a negative electrode plate and an electrolyte, wherein the negative electrode plate includes a negative electrode current collector and a negative electrode material layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode material layer includes a first negative electrode material layer and a second negative electrode material layer stacked, wherein the second negative electrode material layer is located between the first negative electrode material layer and the negative electrode current collector, and the thickness of the first negative electrode material layer is H 1 μm, the thickness of the second negative electrode material layer is H 2 μm, 20≤H 1 ≤40,60≤H 2 ≤90; the first negative electrode material layer includes a first negative electrode active material, the second negative electrode material layer includes a second negative electrode active material, the Dv50 of the first negative electrode active material is greater than the Dv50 of the second negative electrode active material; the electrolyte includes lithium difluorophosphate and a propionate compound, the propionate compound includes propyl propionate; based on the mass of the electrolyte, the mass percentage of lithium difluorophosphate is W 1 %, the mass percentage of propyl propionate is W 2 %, 0.1≤W 1 ≤1,10≤W 2 ≤60,4≤W 1 ×H 1 ≤35. This application designs the negative electrode structure and electrolyte composition, and regulates H 1 , H 2 , W 1 , W 2 , W1 ×H 1 The value of is within the above range, and the Dv50 of the first negative electrode active material and the second negative electrode active material satisfies the above relationship, which can improve the wettability of the electrolyte to the negative electrode plate, reduce the side reactions between the positive electrode plate and the electrolyte, and between the negative electrode plate and the electrolyte during the cycle, increase the solubility of the lithium salt in the electrolyte and the conductivity of the electrolyte, and is beneficial to the transmission of lithium ions in the negative electrode plate and the electrolyte, thereby reducing the initial impedance of the secondary battery and the impedance growth during the cycle, thereby improving the kinetic performance and high-temperature floating charge performance of the secondary battery.
[0006] In some embodiments of the present application, 2≤H 2 / H 1 ≤4.5. By adjusting H 2 / H 1 When the value is within the above range, the wettability of the electrolyte to the negative electrode plate can be further improved, and the side reaction between the negative electrode plate and the electrolyte during the cycle can be reduced, which is beneficial to reduce the initial impedance of the secondary battery and the impedance growth during the cycle, and further beneficial to improve the kinetic performance and high-temperature floating charge performance of the secondary battery.
[0007] In some embodiments of the present application, 0.005≤W 1 / H 1 ≤0.05. By adjusting W 1 / H 1 The value of within the above range is conducive to the synergistic effect between the negative electrode plate and the electrolyte, further improving the kinetic performance of the first negative electrode material layer, thereby helping to further reduce the initial impedance of the secondary battery and the impedance growth during the cycle, and further helping to further improve the kinetic performance and high-temperature floating charge performance of the secondary battery.
[0008] In some embodiments of the present application, 250≤W 2 ×H 1 ≤2400. By adjusting W 2 ×H 1 The value of within the above range is conducive to the synergistic effect between the negative electrode plate and the electrolyte, improving the kinetic performance of the first negative electrode material layer, thereby helping to further reduce the initial impedance of the secondary battery and the impedance growth during the cycle, and further helping to further improve the kinetic performance and high-temperature floating charge performance of the secondary battery.
[0009] In some embodiments of the present application, the electrolyte includes a polynitrile compound, and the mass percentage of the polynitrile compound is W based on the mass of the electrolyte. 3 %, 0.1≤W 3≤5, the polynitrile compound includes at least one of succinonitrile, glutaronitrile, adiponitrile, pimelonitrile, suberonitrile, methyl glutaronitrile, 1,3,5-pentanetricarbonitrile, 1,2,3-propanetricarbonitrile, 1,3,6-hexanetricarbonitrile or 1,2,3-tris(2-cyanoethoxy)propane. On the basis that the electrolyte includes lithium difluorophosphate and propyl propionate, the above polynitrile compound is further introduced and its mass percentage content is regulated W 3 % Within the above range, the stability of the positive electrode sheet and the negative electrode sheet can be improved at the same time, and the electrochemical stability and thermal stability of the electrolyte can be improved, thereby reducing the initial impedance of the secondary battery and the impedance growth during the cycle, improving the kinetic performance of the secondary battery, and also improving the high-temperature floating charge performance of the secondary battery.
[0010] In some embodiments of the present application, 50≤W 3 ×H 1 ≤200. By adjusting W 3 ×H 1 When the value of is within the above range, the initial impedance of the secondary battery and the impedance growth during the cycle process can be reduced, the dynamic performance of the secondary battery can be improved, and the high-temperature floating charge performance of the secondary battery can be further improved.
[0011] In some embodiments of the present application, based on the mass of the electrolyte, the mass percentage of the propionate compound is W 4 %,10≤W 4 ≤65, 0.154≤W 2 / W 4 ≤1. On the basis of the electrolyte comprising lithium difluorophosphate and propyl propionate, the mass percentage content W of the propionate compound is regulated 4 % and W 2 / W 4 The value of within the above range is beneficial to further reduce the initial impedance of the secondary battery and the impedance growth during the cycle process, thereby improving the dynamic performance and high-temperature floating charge performance of the secondary battery.
[0012] In some embodiments of the present application, the propionate compound further comprises at least one of methyl propionate, ethyl propionate, butyl acrylate or butyl propionate. On the basis that the electrolyte comprises lithium difluorophosphate and propyl propionate, the electrolyte further comprises the propionate compound, which is beneficial to further reduce the initial impedance of the secondary battery and the impedance growth during the cycle process, thereby further improving the dynamic performance and high temperature floating charge performance of the secondary battery.
[0013] In some embodiments of the present application, the Dv50 of the first negative electrode active material is 12 μm to 14.9 μm, and the Dv90 of the first negative electrode active material is 20.5 μm to 25.9 μm. By regulating the Dv50 and Dv90 of the first negative electrode active material within the above range, the wettability of the electrolyte to the negative electrode plate can be improved, the side reaction between the negative electrode plate and the electrolyte during the cycle process can be reduced, and the stability of the negative electrode plate can be improved, which is conducive to further reducing the initial impedance of the secondary battery and the impedance growth during the cycle process, thereby helping to improve the kinetic performance of the secondary battery, and also helping to improve the high-temperature floating charge performance of the secondary battery.
[0014] In some embodiments of the present application, the Dv50 of the second negative electrode active material is 10 μm to 11.5 μm, and the Dv90 of the second negative electrode active material is 19.4 μm to 24.8 μm. By regulating the Dv50 and Dv90 of the second negative electrode active material within the above range, the wettability of the electrolyte to the negative electrode plate can be further improved, and the side reaction between the negative electrode plate and the electrolyte during the cycle process can be reduced, which is beneficial to reduce the initial impedance of the secondary battery and the impedance growth during the cycle process, thereby improving the kinetic performance of the secondary battery and improving the high-temperature floating charge performance of the secondary battery.
[0015] In some embodiments of the present application, the first negative electrode active material and the second negative electrode active material each independently include at least one of natural graphite, artificial graphite, soft carbon, hard carbon, mesophase carbon microspheres, silicon carbon compounds, silicon oxygen compounds or lithium titanate. The negative electrode sheet includes a first negative electrode material layer and a second negative electrode material layer, and regulates H 1 and H 2 The value of, the relationship between the Dv50 of the first negative electrode active material and the second negative electrode active material is within the scope of the present application, and the electrolyte includes lithium difluorophosphate and propyl propionate, and W is regulated 1 , W 2 , W 1 ×H 1 On the basis of the value within the scope of the present application, the selection of the first negative electrode active material and the second negative electrode active material can make the secondary battery have good dynamic performance and high-temperature floating charge performance.
[0016] The second aspect of the present application provides an electronic device, which includes the secondary battery provided by the first aspect of the present application. The secondary battery provided by the present application has good dynamic performance and high temperature floating charge performance, so that the electronic device provided by the present application has a long service life and good performance.
[0017] Beneficial effects of this application:
[0018] The present application provides a secondary battery and an electronic device. The secondary battery comprises a negative electrode plate and an electrolyte, wherein the negative electrode plate comprises a negative electrode current collector and a negative electrode material layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode material layer comprises a first negative electrode material layer and a second negative electrode material layer stacked, wherein the second negative electrode material layer is located between the first negative electrode material layer and the negative electrode current collector, and wherein the thickness of the first negative electrode material layer is H 1 μm, the thickness of the second negative electrode material layer is H 2 μm, 20≤H 1 ≤40,60≤H 2 ≤90; the first negative electrode material layer includes a first negative electrode active material, the second negative electrode material layer includes a second negative electrode active material, the Dv50 of the first negative electrode active material is greater than the Dv50 of the second negative electrode active material; the electrolyte includes lithium difluorophosphate and a propionate compound, the propionate compound includes propyl propionate; based on the mass of the electrolyte, the mass percentage of lithium difluorophosphate is W 1 %, the mass percentage of propyl propionate is W 2 %, 0.1≤W 1 ≤1,10≤W 2 ≤60,4≤W 1 ×H 1 ≤35. This application designs the negative electrode structure and electrolyte composition, and regulates H 1 , H 2 , W 1 , W 2 , W 1 ×H 1 The value of is within the above range, and the Dv50 of the first negative electrode active material and the second negative electrode active material satisfies the above relationship, which can improve the wettability of the electrolyte to the negative electrode plate, reduce the side reactions between the positive electrode plate and the electrolyte, and between the negative electrode plate and the electrolyte during the cycle, increase the solubility of the lithium salt in the electrolyte and the conductivity of the electrolyte, and is beneficial to the transmission of lithium ions in the negative electrode plate and the electrolyte, thereby reducing the initial impedance of the secondary battery and the impedance growth during the cycle, thereby improving the kinetic performance and high-temperature floating charge performance of the secondary battery.
[0019] Of course, implementing any product or method of the present application does not necessarily require achieving all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other embodiments can also be obtained based on these drawings.
[0021] Figure 1 A schematic diagram of the structure of a negative electrode sheet along its thickness direction according to an embodiment of the present application;
[0022] Figure 2 This is a graph showing the change in impedance of the lithium-ion batteries of Example 1-1 and Comparative Example 1 of the present application as a function of the number of cycles;
[0023] Figure 3 This is a graph showing the thickness change rate of the lithium-ion batteries of Example 1-1 of the present application and Comparative Example 1 as a function of charging time.
[0024] Reference numerals: negative electrode plate 10 , negative electrode current collector 11 , first negative electrode material layer 12 , second negative electrode material layer 13 . DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. All other embodiments obtained by those skilled in the art based on the present application belong to the scope of protection of the present application.
[0026] It should be noted that in the following content, lithium-ion batteries are used as an example of secondary batteries to explain the present application, but the secondary batteries of the present application are not limited to lithium-ion batteries. The specific technical solution is as follows:
[0027] The first aspect of the present application provides a secondary battery, which includes a negative electrode plate and an electrolyte, wherein the negative electrode plate includes a negative electrode current collector and a negative electrode material layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode material layer includes a first negative electrode material layer and a second negative electrode material layer stacked, wherein the second negative electrode material layer is located between the first negative electrode material layer and the negative electrode current collector, and the thickness of the first negative electrode material layer is H 1 μm, the thickness of the second negative electrode material layer is H 2 μm, 20≤H 1 ≤40,60≤H 2 ≤90. For example, H 1 The value of can be 20, 23, 25, 28, 30, 32, 36, 38, 40 or a range consisting of any two of these values. 2 The value of can be 60, 63, 65, 68, 70, 72, 76, 78, 80, 83, 85, 87, 90 or a range consisting of any two of the values. The first negative electrode material layer includes a first negative electrode active material, the second negative electrode material layer includes a second negative electrode active material, and the Dv50 of the first negative electrode active material is greater than the Dv50 of the second negative electrode active material. The electrolyte includes lithium difluorophosphate (LiPO 2 F 2) and a propionate compound, the propionate compound comprising propyl propionate; based on the mass of the electrolyte, the mass percentage of lithium difluorophosphate is W 1 %, the mass percentage of propyl propionate is W 2 %, 0.1≤W 1 ≤1,10≤W 2 ≤60,4≤W 1 ×H 1 ≤35. For example, W 1 The value of can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1 or a range consisting of any two values therein. 2 The value of can be 10, 15, 20, 24, 30, 35, 40, 46, 50, 54, 60 or a range consisting of any two values therein. 1 ×H 1 The value of can be 4, 8, 10, 12, 15, 17, 20, 23, 25, 28, 30, 35 or a range consisting of any two of the values.
[0028] The negative electrode plate includes a first negative electrode material layer and a second negative electrode material layer, and regulates H 1 , H 2 The value of is within the above range, which can reduce the consumption of electrolyte, make the electrolyte have good wettability to the first negative electrode material layer and the second negative electrode material layer, improve the wettability of the electrolyte to the negative electrode plate, facilitate the transmission of lithium ions in the negative electrode plate, and reduce the side reaction between the negative electrode plate and the electrolyte during the cycle, thereby reducing the initial impedance of the secondary battery and the impedance growth during the cycle, thereby improving the dynamic performance and high-temperature floating performance of the secondary battery. The first negative electrode material layer includes a first negative electrode active material, and the second negative electrode material layer includes a second negative electrode active material. The Dv50 of the first negative electrode active material is greater than the Dv50 of the second negative electrode active material. The specific surface area of the first negative electrode active material is small, which can reduce the side reaction between the negative electrode plate and the electrolyte and reduce the initial impedance of the secondary battery. The particle size of the second negative electrode active material is small, which can improve the wettability of the electrolyte to the negative electrode plate, increase the diffusion path of lithium ions, and reduce the impedance growth during the cycle of the secondary battery, thereby improving the dynamic performance and high-temperature floating performance of the secondary battery. The electrolyte includes lithium difluorophosphate and propyl propionate, and W is regulated 1 , W 2When the value of is within the above range, lithium difluorophosphate can participate in the film formation process of the positive electrode interface and the negative electrode interface at the same time, forming a more compact and stable positive electrode solid electrolyte interface (CEI) film and a negative electrode solid electrolyte interface (SEI) film, reducing the side reactions between the positive electrode sheet and the electrolyte, and between the negative electrode sheet and the electrolyte. Propyl propionate has a large dielectric constant and better solvent kinetics, which can increase the solubility of lithium salts in the electrolyte and the conductivity of the electrolyte, and is beneficial to the transmission of lithium ions in the electrolyte, thereby reducing the initial impedance of the secondary battery and the impedance growth during the cycle, thereby improving the kinetics and high-temperature floating performance of the secondary battery. By regulating W 1 ×H 1 The value of within the above range is conducive to the synergistic effect between the negative electrode sheet and the electrolyte, forming a denser and more stable SEI film at the negative electrode interface, further reducing the side reactions between the negative electrode sheet and the electrolyte, and improving the wettability of the electrolyte to the negative electrode sheet, which is beneficial to the transmission of lithium ions in the negative electrode sheet and improving the kinetic properties of the first negative electrode material layer, thereby further reducing the initial impedance of the secondary battery and the impedance growth during the cycle, and further improving the kinetic performance and high-temperature floating charge performance of the secondary battery.
[0029] When H 1 If the value of is too small, for example, less than 20, it is difficult to improve the impedance growth of the secondary battery during the cycle, thereby affecting the dynamic performance and high-temperature floating charge performance of the secondary battery. 1 When the value of is too large, for example, greater than 40, the kinetic performance of the first negative electrode material layer is too poor, and the wettability of the electrolyte to the second negative electrode material layer is too poor, and the transmission speed of lithium ions in the negative electrode sheet is too slow, resulting in excessive initial impedance of the secondary battery and impedance growth during the cycle, thereby affecting the kinetic performance and high-temperature floating charge performance of the secondary battery. 2 If the value of is too small, for example, less than 60, it is difficult to improve the initial impedance of the secondary battery, thereby affecting the dynamic performance and high-temperature floating charge performance of the secondary battery. 2 When the value is too large, for example greater than 90, the wettability of the electrolyte to the second negative electrode material layer is too poor, and the side reactions between the negative electrode plate and the electrolyte increase during the cycle, resulting in excessive growth in the initial impedance of the secondary battery and the impedance during the cycle, thereby affecting the kinetic performance and high-temperature floating charge performance of the secondary battery.
[0030] When the Dv50 of the first negative electrode active material is less than the Dv50 of the second negative electrode active material, the wettability of the electrolyte to the negative electrode plate is too poor, the transmission speed of lithium ions in the negative electrode plate is too slow, and at the same time, there are too many side reactions between the negative electrode plate and the electrolyte, resulting in excessive initial impedance of the secondary battery and impedance growth during the cycle, thereby affecting the kinetic performance and high-temperature floating charge performance of the secondary battery.
[0031] When W 1 When the value of is too small, for example, less than 0.1, the mass percentage of lithium difluorophosphate is too low, and it is difficult to form a dense and stable CEI film and SEI film at the positive electrode interface and the negative electrode interface. There are too many side reactions between the positive electrode plate and the electrolyte, and between the negative electrode plate and the electrolyte, resulting in excessive initial impedance of the secondary battery and impedance growth during the cycle, thereby affecting the kinetic performance and high-temperature floating charge performance of the secondary battery. 1 When the value of is too large, for example, greater than 1, the mass percentage of lithium difluorophosphate is too high, and its solubility in the electrolyte is too poor, and it is difficult to dissolve completely, and the electrolyte becomes turbid, which makes it difficult to be used in secondary batteries. 2 If the value of is too small, for example, less than 10, the mass percentage of propyl propionate is too low, and the solubility of lithium salt in the electrolyte is too low, which affects the conductivity of the electrolyte and is not conducive to the transmission of lithium ions in the electrolyte, resulting in excessive growth of the initial impedance of the secondary battery and the impedance during the cycle, thereby affecting the kinetic performance and high-temperature floating charge performance of the secondary battery. 2 When the value is too large, for example greater than 60, the mass percentage of propyl propionate is too high, which is not conducive to the dissolution of lithium ions and affects the transmission of lithium ions in the electrolyte, thereby affecting the kinetic performance and high-temperature floating charge performance of the secondary battery.
[0032] When W 1 ×H 1 If the value of is too small, for example, less than 4, it is not conducive to the synergistic effect between the negative electrode and the electrolyte, and it is difficult to form a dense and stable SEI film at the negative electrode interface. There are too many side reactions between the negative electrode and the electrolyte, resulting in excessive initial impedance of the secondary battery and impedance growth during the cycle, thereby affecting the kinetic performance and high-temperature floating charge performance of the secondary battery. 1 ×H 1 When the value is too large, for example greater than 35, it is not conducive to the synergistic effect of the negative electrode plate and the electrolyte, the kinetic performance of the first negative electrode material layer is too poor, the wettability of the electrolyte to the second negative electrode material layer is also too poor, the transmission speed of lithium ions in the negative electrode plate is too slow, and the solubility of lithium difluorophosphate in the electrolyte is too poor, resulting in excessive initial impedance of the secondary battery and impedance growth during the cycle, thereby affecting the kinetic performance and high-temperature floating charge performance of the secondary battery.
[0033] Therefore, the negative electrode plate includes a first negative electrode material layer and a second negative electrode material layer, and the H 1 and H 2 The value of is within the above range, the Dv50 of the first negative electrode active material and the second negative electrode active material satisfies the above relationship, and the electrolyte includes lithium difluorophosphate and propyl propionate, and W is regulated 1 , W 2 , W 1 ×H1 When the value of is within the above range, the initial impedance of the secondary battery and the impedance growth during the cycle can be reduced, and the dynamic performance and high-temperature floating charge performance of the secondary battery can be improved.
[0034] For ease of understanding, in this application, the length direction of the negative electrode sheet itself is defined as Y, and the thickness direction is defined as Z. The negative electrode sheet usually has a long side and a short side, and the length direction is the extension direction of the long side of the negative electrode sheet. It should be understood that the above definition of direction is for the purpose of convenient description of this application. Figure 1 As shown, the negative electrode sheet 10 includes a negative electrode current collector 11 and a second negative electrode material layer 13 and a first negative electrode material layer 12 sequentially disposed on one surface of the negative electrode current collector 11. 1 is the thickness of the first negative electrode material layer, H 2 is the thickness of the second negative electrode material layer. In the present application, the negative electrode material layer can be arranged on one surface of the negative electrode current collector along its thickness direction, or on two surfaces of the negative electrode current collector along its thickness direction. It should be noted that the "surface" here can be the entire area of the surface of the negative electrode current collector, or it can be a partial area of the surface of the negative electrode current collector. This application has no special restrictions, as long as the purpose of this application can be achieved.
[0035] In some embodiments of the present application, 2≤H 2 / H 1 ≤4.5. For example, H 2 / H 1 The value of can be 2, 2.3, 2.5, 2.8, 3, 3.2, 3.6, 3.8, 4, 4.2, 4.5 or a range consisting of any two of them. 2 / H 1 When the value is within the above range, the electrolyte can have good wettability to the first negative electrode material layer and the second negative electrode material layer, improve the wettability of the electrolyte to the negative electrode plate, and is beneficial to the transmission of lithium ions in the negative electrode plate. At the same time, it can also reduce the side reaction between the negative electrode plate and the electrolyte during the cycle process, thereby helping to reduce the initial impedance of the secondary battery and the impedance growth during the cycle, and further helping to improve the kinetic performance and high-temperature floating charge performance of the secondary battery.
[0036] In some embodiments of the present application, 0.005≤W 1 / H 1 ≤0.05. For example, W 1 / H 1 The value of can be 0.005, 0.01, 0.015, 0.02, 0.024, 0.03, 0.036, 0.04, 0.045, 0.05 or a range consisting of any two of them. 1 / H1 The value of within the above range is conducive to the synergistic effect between the negative electrode plate and the electrolyte, forming a denser and more stable SEI film at the negative electrode interface, further reducing the side reaction between the negative electrode interface and the electrolyte, and further improving the wettability of the electrolyte to the negative electrode plate, which is beneficial to the transmission of lithium ions in the negative electrode plate, and further improving the kinetic performance of the first negative electrode material layer, thereby helping to further reduce the initial impedance of the secondary battery and the impedance growth during the cycle, and further helping to further improve the kinetic performance and high-temperature floating charge performance of the secondary battery.
[0037] In some embodiments of the present application, 250≤W 2 ×H 1 ≤2400. For example, W 2 ×H 1 The value of can be 250, 500, 800, 1000, 1200, 1500, 1800, 2000, 2400 or a range consisting of any two of the values. 2 ×H 1 The value of within the above range is conducive to the synergistic effect between the negative electrode plate and the electrolyte, improving the solubility of the lithium salt in the electrolyte and the conductivity of the electrolyte, and can also improve the wettability of the electrolyte to the negative electrode plate, which is beneficial to the transmission of lithium ions in the electrolyte and the negative electrode plate, and improves the kinetic properties of the first negative electrode material layer, thereby helping to further reduce the initial impedance of the secondary battery and the impedance growth during the cycle, and further helping to further improve the kinetic performance and high-temperature floating charge performance of the secondary battery.
[0038] In some embodiments of the present application, the electrolyte includes a polynitrile compound, and the mass percentage of the polynitrile compound is W based on the mass of the electrolyte. 3 %, 0.1≤W 3 ≤5. The polynitrile compound includes at least one of succinonitrile, glutaronitrile, adiponitrile, pimelonitrile, suberonitrile, methylglutaronitrile, 1,3,5-pentanetricarbonitrile, 1,2,3-propanetricarbonitrile, 1,3,6-hexanetricarbonitrile or 1,2,3-tris(2-cyanoethoxy)propane. For example, W 3 The value of can be 0.1, 0.6, 1, 1.5, 2, 2.4, 3, 3.6, 4, 4.5, 5 or a range consisting of any two of the values. On the basis that the electrolyte includes lithium difluorophosphate and propyl propionate, the above-mentioned polynitrile compound is further introduced and its mass percentage content W is regulated 3% Within the above range, the strong coordination ability of the polynitrile compound can be complexed with the high-valent metal ions (such as cobalt ions) at the positive electrode interface, reducing the phase change reaction of the positive electrode active material caused by the dissolution of metal ions, forming a more stable CEI film, and a reduction reaction can occur at the negative electrode interface to form a stable SEI film, while improving the stability of the positive and negative electrode sheets, and the carbon-nitrogen triple bond energy in the polynitrile compound is high and not easily oxidized, which can reduce the oxidation and decomposition of the electrolyte and produce gas, improve the electrochemical stability and thermal stability of the electrolyte, thereby reducing the initial impedance of the secondary battery and the impedance growth during the cycle, improving the kinetic performance of the secondary battery, and also improving the high-temperature floating charge performance of the secondary battery. In this application, high temperature refers to a temperature greater than or equal to 40°C.
[0039] In some embodiments of the present application, 50≤W 3 ×H 1 ≤200. For example, W 3 ×H 1 The value of can be 50, 80, 100, 120, 150, 180, 200 or a range consisting of any two of these values. 3 ×H 1 When the value of is within the above range, it is beneficial to exert the synergistic effect between the negative electrode sheet and the electrolyte, and a reduction reaction occurs at the negative electrode interface to form a stable SEI film, thereby improving the stability of the negative electrode sheet. It can also improve the wettability of the electrolyte to the negative electrode sheet, which is beneficial to the transmission of lithium ions in the negative electrode sheet, improve the kinetic properties of the first negative electrode material layer, reduce the oxidative decomposition and gas production of the electrolyte, and improve the electrochemical stability and thermal stability of the electrolyte, thereby reducing the initial impedance of the secondary battery and the impedance growth during the cycle, improving the kinetic properties of the secondary battery, and further improving the high-temperature floating charge performance of the secondary battery.
[0040] In some embodiments of the present application, based on the mass of the electrolyte, the mass percentage of the propionate compound is W 4 %,10≤W 4 ≤65, 0.154≤W 2 / W 4 ≤1. For example, W 4 The value of can be 10, 15, 20, 24, 30, 35, 40, 46, 50, 54, 60, 65 or a range consisting of any two values therein. 2 / W 4 The value of can be 0.154, 0.3, 0.35, 0.4, 0.5, 0.62, 0.7, 0.85, 0.9, 1 or a range consisting of any two of the values. On the basis that the electrolyte includes lithium difluorophosphate and propyl propionate, the mass percentage content W of the propionate compound is regulated4 % and W 2 / W 4 When the value is within the above range, the solubility of lithium salt in the electrolyte and the conductivity of the electrolyte can be improved, which is beneficial to the transmission of lithium ions in the electrolyte, thereby helping to reduce the initial impedance of the secondary battery and the impedance growth during the cycle, and further helping to improve the kinetic performance and high-temperature floating charge performance of the secondary battery.
[0041] In some embodiments of the present application, the propionate compound further comprises at least one of methyl propionate, ethyl propionate, butyl acrylate or butyl propionate. On the basis that the electrolyte comprises lithium difluorophosphate and propyl propionate, the electrolyte further comprises the propionate compound, which can improve the solubility of lithium salt in the electrolyte and the conductivity of the electrolyte, facilitate the transmission of lithium ions in the electrolyte, and facilitate further reducing the initial impedance of the secondary battery and the impedance growth during the cycle process, thereby facilitating further improving the dynamic performance and high temperature floating charge performance of the secondary battery.
[0042] In the present application, the electrolyte also includes other organic solvents. The present application has no particular restrictions on the types of other organic solvents, as long as the purpose of the present application can be achieved. For example, other organic solvents may include but are not limited to at least one of carbonate compounds, carboxylate compounds, ether compounds or other organic solvents. The above-mentioned carbonate compounds may include but are not limited to at least one of chain carbonate compounds, cyclic carbonate compounds or fluorocarbonate compounds. The above-mentioned chain carbonate compounds may include but are not limited to at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC) or ethyl methyl carbonate (MEC). The above-mentioned cyclic carbonate may include but are not limited to at least one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC) or vinyl ethylene carbonate (VEC). The fluorinated carbonate compound may include, but is not limited to, at least one of fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, or trifluoromethylethylene carbonate. The carboxylate compound may include, but is not limited to, at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, γ-butyrolactone, decalactone, valerolactone, or caprolactone. The above-mentioned ether compound may include but is not limited to at least one of dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran or tetrahydrofuran. The above-mentioned other organic solvents may include but are not limited to at least one of dimethyl sulfoxide, 1,2-dioxolane, cyclopentane, methyl cyclopentane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, dimethylformamide, trimethyl phosphate, triethyl phosphate or trioctyl phosphate. Based on the mass of the electrolyte, the mass percentage of other organic solvents is 14% to 81%. For example, the mass percentage of other organic solvents can be 14%, 19%, 24%, 30%, 40%, 50%, 62%, 70%, 78%, 81% or a range composed of any two of the values.
[0043] In the present application, the electrolyte also includes a lithium salt. The present application has no particular restrictions on the lithium salt, as long as the purpose of the present application can be achieved. For example, the lithium salt may include but is not limited to LiPF 6 , LiBF 4 、LiAsF 6 、LiClO 4 、LiB(C 6H 5 ) 4 、LiCH 3 SO 3 、LiCF 3 SO 3 、LiN(SO 2 CF 3 ) 2 、LiC(SO 2 CF 3 ) 3 , Li 2 SiF 6 At least one of lithium bis(oxalato)borate (LiBOB) and lithium difluoroborate. Based on the mass of the electrolyte, the mass percentage of the lithium salt is 8% to 15%.
[0044] In some embodiments, the electrolyte may include lithium salt, lithium difluorophosphate, propyl propionate and other organic solvents. The mass percentages of lithium salt, lithium difluorophosphate and propyl propionate are as described above, and the mass percentage of other organic solvents is 24% to 81%. The secondary battery including the above electrolyte has good kinetic performance and high temperature floating charge performance.
[0045] In some embodiments, the electrolyte may include lithium salt, lithium difluorophosphate, propyl propionate, polynitrile compounds and other organic solvents. The mass percentage of lithium salt, lithium difluorophosphate, propyl propionate and polynitrile compounds is as described above, and the mass percentage of other organic solvents is 19% to 81%. The secondary battery including the above electrolyte has good dynamic performance and high temperature floating charge performance.
[0046] In some embodiments, the electrolyte may include lithium salt, lithium difluorophosphate, propionate compound and other organic solvents. The propionate compound includes propyl propionate and at least one of methyl propionate, ethyl propionate, butyl acrylate or butyl propionate. The mass percentage of lithium salt, lithium difluorophosphate and propionate compound is as described above, and the mass percentage of other organic solvents is 19% to 81%. The secondary battery including the above electrolyte has good dynamic performance and high temperature floating charge performance.
[0047] In some embodiments, the electrolyte may include lithium salt, lithium difluorophosphate, propionate compound, polynitrile compound and other organic solvents. The propionate compound includes at least one of propyl propionate and methyl propionate, ethyl propionate, butyl acrylate or butyl propionate. The mass percentage of lithium salt, lithium difluorophosphate, propionate compound and polynitrile compound is as described above, and the mass percentage of other organic solvents is 14% to 81%. The secondary battery including the above electrolyte has better dynamic performance and high temperature floating charge performance.
[0048] In some embodiments of the present application, the Dv50 of the first negative electrode active material is 12 μm to 14.9 μm, and the Dv90 of the first negative electrode active material is 20.5 μm to 25.9 μm. For example, the Dv50 of the first negative electrode active material can be 12 μm, 12.3 μm, 12.7 μm, 13 μm, 13.4 μm, 13.7 μm, 14 μm, 14.5 μm, 14.9 μm, or a range consisting of any two of the values, and the Dv90 of the first negative electrode active material can be 20.5 μm, 21 μm, 21.6 μm, 22 μm, 22.4 μm, 23 μm, 23.5 μm, 24 μm, 24.6 μm, 25 μm, 25.9 μm, or a range consisting of any two of the values. By regulating the Dv50 and Dv90 of the first negative electrode active material within the above range, the consumption of electrolyte by the negative electrode plate can be reduced, the wettability of the electrolyte to the negative electrode plate can be improved, which is beneficial to the transmission of lithium ions in the negative electrode plate. It can also reduce the side reaction between the negative electrode plate and the electrolyte during the cycle process, and improve the stability of the negative electrode plate, which is beneficial to reduce the initial impedance of the secondary battery and the impedance growth during the cycle process, and then help to improve the kinetic performance of the secondary battery, and also help to improve the high-temperature floating charge performance of the secondary battery.
[0049] In some embodiments of the present application, the Dv50 of the second negative electrode active material is 10 μm to 11.5 μm, and the Dv90 of the second negative electrode active material is 19.4 μm to 24.8 μm. For example, the Dv50 of the second negative electrode active material can be 10 μm, 10.3 μm, 10.5 μm, 10.7 μm, 11 μm, 11.2 μm, 11.5 μm, or a range consisting of any two of the values, and the Dv90 of the second negative electrode active material can be 19.4 μm, 20 μm, 20.5 μm, 21 μm, 21.6 μm, 22 μm, 22.4 μm, 23 μm, 23.5 μm, 24 μm, 24.8 μm, or a range consisting of any two of the values. By regulating the Dv50 and Dv90 of the second negative electrode active material within the above range, the wettability of the electrolyte to the negative electrode plate can be improved, and the side reactions between the negative electrode plate and the electrolyte during the cycle can be reduced, which is beneficial to reducing the initial impedance of the secondary battery and the impedance growth during the cycle, and further beneficial to improving the kinetic performance of the secondary battery, and also beneficial to improving the high-temperature floating charge performance of the secondary battery.
[0050] In the present application, Dv50 refers to the particle size at which 50% of the volume is accumulated from the small particle size in the volume-based particle size distribution of the material. Dv90 refers to the particle size at which 90% of the volume is accumulated from the small particle size in the volume-based particle size distribution of the material. In some embodiments, the Dv90 of the first negative electrode active material is less than the thickness H of the first negative electrode material layer. 1 .
[0051] Generally, the first negative electrode active material and the second negative electrode active material with different Dv50 and Dv90 can be obtained by mechanical crushing (such as ball milling). For example, the Dv50 and Dv90 of the first negative electrode active material and the Dv50 and Dv90 of the second negative electrode active material can be regulated by regulating the ball milling time. When other conditions remain unchanged, the ball milling time is extended, and the Dv50 of the first negative electrode active material decreases; the ball milling time is shortened, and the Dv50 of the first negative electrode active material increases. When other conditions remain unchanged, the ball milling time is extended, and the Dv90 of the first negative electrode active material decreases; the ball milling time is shortened, and the Dv90 of the first negative electrode active material increases. When other conditions remain unchanged, the ball milling time is extended, and the Dv50 of the second negative electrode active material decreases; the ball milling time is shortened, and the Dv50 of the second negative electrode active material increases. When other conditions remain unchanged, the ball milling time is extended, and the Dv90 of the second negative electrode active material decreases; the ball milling time is shortened, and the Dv90 of the second negative electrode active material increases.
[0052] In some embodiments of the present application, the first negative electrode active material and the second negative electrode active material each independently include natural graphite, artificial graphite, soft carbon, hard carbon, mesophase carbon microspheres, silicon carbon compound SiC, silicon oxygen compound SiO x (0<x≤2) or at least one of lithium titanate. The negative electrode sheet includes a first negative electrode material layer and a second negative electrode material layer, and regulates H 1 and H 2 The value of, the relationship between the Dv50 of the first negative electrode active material and the second negative electrode active material is within the scope of the present application, and the electrolyte includes lithium difluorophosphate and propyl propionate, and W is regulated 1 , W 2 , W 1 ×H 1 Based on the value of within the scope of this application, the selection of the first negative electrode active material and the second negative electrode active material can make the secondary battery have good dynamic performance and high temperature floating charge performance. In this application, the types of the first negative electrode active material and the second negative electrode active material can be the same or different.
[0053] In the present application, the first negative electrode material layer includes a first negative electrode active material, and may also include a first negative electrode binder and a first negative electrode conductor, or the first negative electrode material layer may also include a first negative electrode binder, a first negative electrode conductor or a first thickener. Based on the mass of the first negative electrode material layer, the mass percentage of the first negative electrode active material may be 86% to 99%, the mass percentage of the first negative electrode binder may be 0.5% to 5%, the mass percentage of the first negative electrode conductor may be 0.5% to 5%, and the mass percentage of the first thickener may be 0% to 4%.
[0054] In the present application, the second negative electrode material layer includes a second negative electrode active material, and may also include a second negative electrode binder and a second negative electrode conductor, or the second negative electrode material layer may also include a second negative electrode binder, a second negative electrode conductor or a second thickener. Based on the mass of the second negative electrode material layer, the mass percentage of the second negative electrode active material may be 86% to 99%, the mass percentage of the second negative electrode binder may be 0.5% to 5%, the mass percentage of the second negative electrode conductor may be 0.5% to 5%, and the mass percentage of the second thickener may be 0% to 4%.
[0055] The present application has no particular restrictions on the types of the first negative electrode binder, the second negative electrode binder, the first negative electrode conductor and the second negative electrode conductor, as long as the purpose of the present application can be achieved. For example, the first negative electrode binder and the second negative electrode binder can each independently include but are not limited to at least one of polyacrylic acid, sodium polyacrylate, potassium polyacrylate, lithium polyacrylate, polyimide, polyvinyl alcohol, polyamide-imide, styrene-butadiene rubber or polyvinylidene fluoride. For example, the first negative electrode conductor and the second negative electrode conductor can each independently include but are not limited to at least one of conductive carbon black (Super P), carbon nanotubes (CNTs), carbon fibers, flake graphite, graphene, metal materials or conductive polymers, and the conductive carbon black can include but are not limited to at least one of acetylene black or Ketjen black. The above-mentioned carbon nanotubes can include but are not limited to single-walled carbon nanotubes and / or multi-walled carbon nanotubes. The above-mentioned carbon fibers can include but are not limited to vapor-grown carbon fibers (VGCF) and / or nanocarbon fibers. The above-mentioned metal materials can include but are not limited to metal powders and / or metal fibers, and specifically, the metal can include but are not limited to at least one of copper, nickel, aluminum or silver. The conductive polymer may include but is not limited to at least one of polyphenylene derivatives, polyaniline, polythiophene, polyacetylene or polypyrrole. The present application has no particular restrictions on the types of the first thickener and the second thickener, as long as the purpose of the present application can be achieved. For example, the first thickener and the second thickener may each independently include but is not limited to at least one of sodium carboxymethyl cellulose or lithium carboxymethyl cellulose.
[0056] The present application has no particular restrictions on the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the negative electrode current collector may include copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam or composite current collector. For example, the composite current collector may be a lithium copper composite current collector, a carbon copper composite current collector, a nickel copper composite current collector, a titanium copper composite current collector, etc. The present application has no particular restrictions on the thickness of the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the thickness of the negative electrode current collector may be 4 μm to 15 μm.
[0057] Optionally, the negative electrode material layer may further include a conductive layer, and the conductive layer is located between the negative electrode current collector and the second negative electrode material layer. The present application has no particular restrictions on the composition of the conductive layer, and it may be a conductive layer commonly used in the art. For example, the conductive layer includes a conductive agent and a binder. The present application has no particular restrictions on the conductive agent and the binder in the conductive layer, and for example, it may be at least one of the above-mentioned first negative electrode conductive agent and the above-mentioned first negative electrode binder.
[0058] The present application has no particular restrictions on the preparation method of the negative electrode sheet, as long as the purpose of the present application can be achieved. For example, the preparation method of the negative electrode sheet may include but is not limited to the following steps: (1) preparing a first negative electrode slurry and a second negative electrode slurry; (2) coating the second negative electrode slurry on one surface of the negative electrode current collector, and after drying, forming a second negative electrode material layer on one surface of the negative electrode current collector; then coating the first negative electrode slurry on the surface of the second negative electrode material layer, and after drying, forming a second negative electrode material layer and a first negative electrode material layer on one surface of the negative electrode current collector in sequence; (3) repeating the above steps on the other surface of the negative electrode current collector, forming a first negative electrode material layer and a second negative electrode material layer on both surfaces of the negative electrode current collector; (4) cold pressing, cutting, and welding the negative electrode tabs to obtain the negative electrode sheet.
[0059] Generally, the thickness H of the first negative electrode material layer can be adjusted by adjusting the coating surface density of the first negative electrode material layer. 1 For example, when other conditions remain unchanged, the coating surface density of the first negative electrode material layer increases, H 1 Increase; the coating surface density of the first negative electrode material layer decreases, H 1 Reduce.
[0060] Generally, the thickness H of the second negative electrode material layer can be adjusted by adjusting the coating surface density of the second negative electrode material layer. 2 For example, when other conditions remain unchanged, the coating surface density of the second negative electrode material layer increases, H 2 Increase; the coating surface density of the second negative electrode material layer decreases, H 2 Reduce.
[0061] In the present application, the secondary battery also includes a positive electrode plate, and the positive electrode plate includes a positive electrode collector and a positive electrode material layer disposed on at least one surface of the positive electrode collector. The above-mentioned "positive electrode material layer disposed on at least one surface of the positive electrode collector" means that the positive electrode material layer can be disposed on one surface of the positive electrode collector along its own thickness direction, or it can be disposed on two surfaces of the positive electrode collector along its own thickness direction. It should be noted that the "surface" here can be the entire area of the surface of the positive electrode collector, or it can be a partial area of the surface of the positive electrode collector. This application has no special restrictions, as long as the purpose of this application can be achieved.
[0062] The present application has no particular restrictions on the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the positive electrode current collector may include aluminum foil, aluminum alloy foil or a composite current collector (such as an aluminum-carbon composite current collector). The present application has no particular restrictions on the thickness of the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the thickness of the positive electrode current collector may be 5 μm to 20 μm.
[0063] The positive electrode material layer includes a positive electrode active material. The present application has no particular limitation on the positive electrode active material as long as the purpose of the present application can be achieved. For example, the positive electrode active material may include but is not limited to lithium nickel cobalt manganese oxide (such as NCM811, NCM622, NCM523, NCM111), lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium-rich manganese-based materials, lithium cobalt oxide (LiCoO 2 ), at least one of lithium manganese oxide, lithium iron manganese phosphate or lithium titanate.
[0064] The positive electrode material layer may also include a positive electrode conductor and a positive electrode binder. The present application has no particular restrictions on the types of the positive electrode conductor and the positive electrode binder, as long as the purpose of the present application can be achieved. For example, it may be at least one of the above-mentioned first negative electrode conductor and the above-mentioned first negative electrode binder. The present application has no particular restrictions on the mass ratio of the positive electrode active material, the positive electrode conductor, and the positive electrode binder in the positive electrode material layer. Those skilled in the art can select according to actual needs, as long as the purpose of the present application can be achieved.
[0065] The present application has no particular restrictions on the thickness of the positive electrode material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the positive electrode material layer can be 30 μm to 120 μm. The present application has no particular restrictions on the compaction density of the positive electrode material layer, as long as the purpose of the present application can be achieved. For example, the compaction density of the positive electrode material layer can be 3 g / cm 3 Up to 5g / cm 3 .
[0066] Optionally, the positive electrode sheet may further include a conductive layer, which is located between the positive electrode current collector and the positive electrode material layer. The composition of the conductive layer is not particularly limited, and it can be a conductive layer commonly used in the art. The conductive layer includes a conductive agent and a binder. The present application does not particularly limit the conductive agent and binder in the conductive layer, for example, it can be at least one of the above-mentioned first negative electrode conductive agent and the above-mentioned first negative electrode binder.
[0067] In the present application, the secondary battery also includes a separator. The present application has no particular restrictions on the separator, as long as the purpose of the present application can be achieved. For example, the material of the separator may include but is not limited to polyethylene (PE), polypropylene (PP)-based polyolefins (PO), polyesters (e.g., polyethylene terephthalate (PET) film), cellulose, polyimide (PI), polyamide (PA), spandex or aramid. The type of separator may include at least one of a woven membrane, a non-woven membrane, a microporous membrane, a composite membrane, a rolled membrane or a spun membrane.
[0068] In some embodiments, the isolation film may include a substrate layer and a surface treatment layer. The substrate layer may be a nonwoven fabric, a film or a composite film having a porous structure, and the material of the substrate layer may include at least one of polyethylene, polypropylene, polyethylene terephthalate or polyimide. Optionally, a polypropylene porous film, a polyethylene porous film, a polypropylene nonwoven fabric, a polyethylene nonwoven fabric or a polypropylene-polyethylene-polypropylene porous composite film may be used.
[0069] Optionally, a surface treatment layer is disposed on at least one surface of the substrate layer. The surface treatment layer may be a polymer layer or an inorganic layer, or a layer formed by mixing a polymer and an inorganic layer.
[0070] In some embodiments, the inorganic layer includes inorganic particles and a binder. The present application has no particular restrictions on inorganic particles, such as inorganic particles can include aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide or barium sulfate. The present application has no particular restrictions on the binder in the inorganic layer, such as the binder in the inorganic layer can be at least one of the above-mentioned first negative electrode binders. In some embodiments, the polymer layer includes a polymer, and the material of the polymer includes at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylate, polyvinyl pyrrolidone, polyvinyl ether or polyvinylidene fluoride or poly (vinylidene fluoride-hexafluoropropylene).
[0071] In the present application, there is no particular limitation on the thickness of the isolation film, as long as the purpose of the present application can be achieved. For example, the thickness of the isolation film may be 3 μm to 30 μm.
[0072] In the present application, the secondary battery also includes a shell for accommodating a positive electrode plate, a separator, a negative electrode plate and an electrolyte, as well as other components known in the field of secondary batteries, and the present application does not limit the above-mentioned other components. The present application has no special restrictions on the shell, and it can be a shell known in the art, as long as the purpose of the present application can be achieved. For example, the shell can be a hard shell or a flexible shell. The material of the hard shell can be metal, and the present application does not limit the type of metal. A metal hard shell known in the art can be used, as long as the purpose of the present application can be achieved. The flexible shell can be a metal plastic film, such as an aluminum plastic film, a steel plastic film, etc.
[0073] The preparation process of the secondary battery of the present application is well known to those skilled in the art, and there is no particular limitation in the present application. For example, the preparation process of the secondary battery may include but is not limited to the following steps: stacking the positive electrode sheet, the separator and the negative electrode sheet in order, and winding, folding and other operations as needed to obtain an electrode assembly of a winding structure, placing the electrode assembly in a shell, injecting the electrolyte into the shell and sealing it to obtain a secondary battery. Alternatively, stack the positive electrode sheet, the separator and the negative electrode sheet in order, and then fix the four corners of the entire laminate structure with tape to obtain an electrode assembly of a laminate structure, place the electrode assembly in a shell, inject the electrolyte into the shell and seal it to obtain a secondary battery. In addition, overcurrent protection elements, guide plates, etc. may also be placed in the shell as needed to prevent the pressure inside the secondary battery from rising and overcharging and discharging.
[0074] The second aspect of the present application provides an electronic device, which includes the secondary battery provided by the first aspect of the present application. The secondary battery provided by the present application has good dynamic performance and high temperature floating charge performance, so that the electronic device provided by the present application has a long service life and good performance.
[0075] The present application does not particularly limit the type of electronic device, and it can be any electronic device known in the prior art. For example, the electronic device can include but is not limited to a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD television, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery and a lithium-ion capacitor, etc.
[0076] Example
[0077] The following examples and comparative examples are given to more specifically describe the embodiments of the present application. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.
[0078] Test methods and equipment:
[0079] Thickness test
[0080] After the lithium-ion batteries of the embodiments and comparative examples were discharged to 3V at 0.2C, the negative electrode plates were disassembled, cleaned with dimethyl carbonate (DMC), dried at 60°C, and the cross-section of the negative electrode plates along the thickness direction was polished with argon ions. Then, the cross-section of the negative electrode plates was observed using a scanning electron microscope (SEM) and the thickness H of the first negative electrode material layer was tested. 1 , the thickness H of the second negative electrode material layer 2 and H 2 / H 1 .
[0081] Tests of Dv50 and Dv90 of the first negative electrode active material and the second negative electrode active material
[0082] According to the national standard “Particle Size Distribution Laser Diffraction Method” (GB / T19077-2016), a laser particle size analyzer (model: MS3000) was used to test the Dv50 and Dv90 of the first negative electrode active material and the second negative electrode active material.
[0083] Testing of electrolyte components:
[0084] The lithium-ion battery is discharged at a constant current of 0.2C to 3V and then disassembled. The electrolyte is collected by centrifugation, extrusion or other methods, and then tested by gas chromatography-mass spectrometry (GC-MS, instrument model is Agilent 8890) and ion chromatography (IC, instrument model is AQUION ion chromatography) to obtain each component in the electrolyte and test its content.
[0085] Initial impedance test
[0086] The lithium-ion battery was placed in a 25°C constant temperature box, and after standing for 4 hours, it was charged at a constant current of 0.7C to the rated voltage (4.48V in the present embodiment), and then charged at a constant voltage of 4.48V to a current of 0.05C, and then stood for 2 hours, and then discharged at a constant current of 0.2C to a voltage of 3.0V. The capacity of the lithium-ion battery measured at this time was recorded as the reference capacity C 1, that is, the capacity at 100% SOC (State of Charge). The lithium-ion battery is charged at a constant current of 0.7C to a voltage of 4.48V, then charged at a constant voltage of 4.48V to a current of 0.05C, left to stand for 10 minutes, and then discharged at a constant current of 0.1C to 0.3C. 1 (70% SOC), 0.8C 1 (20% SOC), 0.9C 1 (10% SOC), and test the voltage and current of the lithium-ion battery under the above three different SOCs respectively, calculate the ratio of voltage to current, and obtain the impedance of 70% SOC, which is recorded as R 1 The impedance of 20% SOC is recorded as R 2 , 10% SOC impedance is recorded as R 3 . Through the lithium-ion battery R 1 , R 2 , R 3 The value of R of lithium-ion battery is used to evaluate its initial impedance. 1 , R 2 , R 3 The smaller the value, the smaller the initial impedance, R 1 , R 2 , R 3 The larger the value of , the larger the initial impedance.
[0087] Impedance growth test
[0088] The lithium-ion battery was placed in a 25°C constant temperature box and left to stand for 4 hours. Then, it was discharged at a constant current of 0.02C to 0.3C. 1 (70% SOC), 0.8C 1 (20% SOC), 0.9C 1 (10% SOC). The voltage of the lithium-ion battery at 70% SOC is recorded as U' 70% , the current is recorded as I' 70% ; The voltage of the lithium-ion battery at 20% SOC is recorded as U' 20% , the current is recorded as I' 20% ; The voltage of the lithium-ion battery at 10% SOC is recorded as U' 10% , the current is recorded as I' 10%. Charge the lithium-ion battery at a constant current of 0.7C to a voltage of 4.48V, charge at a constant voltage of 4.48V to a current of 0.05C, let it stand for 2h, and then discharge at a constant current of 0.5C to a voltage of 3.0V. This is one charge and discharge cycle. Perform a charge and discharge cycle on the lithium-ion battery according to the above method, and perform a discharge capacity recovery test every 50 charge and discharge cycles. Charge the lithium-ion battery at a constant current of 0.7C to a voltage of 4.48V, charge at a constant voltage of 4.48V to a current of 0.05C, let it stand for 2h, and then discharge at a constant current of 0.2C to 0.3C in sequence. 1 (70% SOC), 0.8C 1 (20% SOC), 0.9C 1 (10% SOC). The voltage of the lithium-ion battery at 70% SOC is recorded as U 70% , current is recorded as I 70% ; The voltage of the lithium-ion battery at 20% SOC is recorded as U 20% , current is recorded as I 20% ; The voltage of the lithium-ion battery at 10% SOC is recorded as U 10% , current is recorded as I 10% R is calculated by the following formula 70% , R 20% , R 10% : R 70% =(U 70% -U' 70% ) / (I 70% -I' 70% );R 20% =(U 20% -U' 20% ) / (I 20% -I' 20% );R 10% =(U 10% -U' 10% ) / (I 10% -I' 10% ). Calculate R 70% , R 20% , R 10% The average value is taken as the impedance value of the lithium-ion battery at the corresponding number of cycles. The above charge and discharge method is followed until 1000 cycles. Three lithium-ion batteries are tested in each embodiment and comparative example, and the average value of the impedance of the three lithium-ion batteries is calculated as the impedance of the lithium-ion battery. The impedance of the lithium-ion battery at the 300th cycle is recorded as R 300 The impedance at the 1000th cycle is recorded as R 1000 The impedance growth of lithium-ion batteries is evaluated by K calculated by the following formula: K = (R 1000 -R 300) / (1000-300). The smaller the value of K, the smaller the impedance increase, and the larger the value of K, the larger the impedance increase.
[0089] High temperature float charge performance test
[0090] The lithium-ion battery was placed in a 25°C constant temperature box. After standing for 4 hours, it was charged to 4.48V at a constant current of 0.7C, charged to a current of 0.05C at a constant voltage of 4.48V, and then stood for 2 hours. Then, it was discharged to a voltage of 3.0V at a constant current of 0.2C. The lithium-ion battery was then charged to 4.48V at a constant current of 0.7C, and charged to a current of 0.05C at a constant voltage of 4.48V. The thickness of the lithium-ion battery at this time was measured and recorded as the initial thickness T. 0 Place the lithium-ion battery in a 55°C constant temperature box and leave it for 1.5 hours. Charge the lithium-ion battery to 4.48V at a constant current of 0.4C, and charge it to 60mA at a constant voltage of 4.48V. Continue charging at a constant current (100mA) and a constant voltage (4.48V), and measure the thickness of the lithium-ion battery every 96 hours, and record it as T i , the thickness change rate of the lithium-ion battery is T i / T 0 , when T i / T 0 When the value reaches 108.5%, record the charging time of the lithium-ion battery at constant current (100mA) and constant voltage (4.48V). Take 3 lithium-ion batteries for each embodiment and comparative example for testing, calculate the average value of the above charging time of the 3 lithium-ion batteries, and record it as D. The high-temperature floating charge performance is evaluated by the value of D. The larger the value of D of the lithium-ion battery, the better the high-temperature floating charge performance, and the smaller the value of D, the worse the high-temperature floating charge performance.
[0091] Example 1-1
[0092] <Preparation of negative electrode sheet>
[0093] The first negative electrode active material artificial graphite and the first negative electrode binder styrene butadiene rubber (SBR, weight average molecular weight Mw = 5×10 6 ), the first thickener sodium carboxymethyl cellulose (CMC-Na, Mw = 7 × 10 5 ), the first negative electrode conductive agent conductive carbon black (Super P) is mixed in a mass ratio of 96:1.5:1.5:1, and then deionized water is added as a solvent to prepare a slurry with a solid content of 50wt%, and the first negative electrode slurry is obtained after vacuum stirring.
[0094] The second negative electrode active material artificial graphite and the second negative electrode binder styrene butadiene rubber (SBR, Mw = 5 × 10 6 ), the second thickener sodium carboxymethyl cellulose (CMC-Na, Mw = 7 × 10 5), the second negative electrode conductive agent conductive carbon black (Super P) is mixed in a mass ratio of 96:1.5:1.5:1, and then deionized water is added as a solvent to prepare a slurry with a solid content of 50wt%, and the second negative electrode slurry is obtained after vacuum stirring.
[0095] The second negative electrode slurry was uniformly coated on one surface of the negative electrode current collector copper foil with a thickness of 10 μm, and the coating surface density was 5.81 mg / cm 2 , dried at 85°C to obtain a negative electrode sheet coated with the second negative electrode material layer on one side. Then, the first negative electrode slurry was evenly coated on the surface of the second negative electrode material layer away from the negative electrode current collector, with a coating surface density of 2.33 mg / cm 2 , and dried at 85°C to obtain a negative electrode sheet coated with the second negative electrode material layer and the first negative electrode material layer on one side. Then, repeat the above steps on the other surface of the copper foil to obtain a negative electrode sheet coated with the second negative electrode material layer and the first negative electrode material layer on both sides. Then, cold press, cut, and weld the negative electrode tab nickel tab to obtain a negative electrode sheet with a specification of 76mm×867mm for standby use. Among them, the thickness of the first negative electrode material layer H 1 , the thickness H of the second negative electrode material layer 2 As shown in Table 1, Dv50 and Dv90 of the first negative electrode active material and the second negative electrode active material are shown in Table 3.
[0096] <Preparation of Electrolyte>
[0097] In an argon atmosphere glove box with a water content of less than 10 ppm, other organic solvents ethylene carbonate (EC), propylene carbonate (PC), and diethyl carbonate (DEC) were mixed in a mass ratio of 1:1:1 as a base solvent, and then lithium salt lithium hexafluorophosphate (LiPF 6 ), lithium difluorophosphate and propyl propionate, and mixed evenly to obtain an electrolyte. Among them, based on the mass of the electrolyte, the lithium salt LiPF 6 The mass percentage of lithium difluorophosphate is 12.5%, and the mass percentage of lithium difluorophosphate is W 1 % and the mass percentage of propyl propionate W 2 % are shown in Table 1, and the rest is the base solvent.
[0098] <Preparation of positive electrode sheet>
[0099] The positive electrode active material is lithium cobalt oxide, the positive electrode conductive agent is conductive carbon black (Super P), the positive electrode conductive agent is carbon nanotube (CNT), and the positive electrode binder is polyvinylidene fluoride (PVDF, Mw = 7×10 6) are mixed in a mass ratio of 97:0.8:0.7:1.5, N-methylpyrrolidone (NMP) is added as a solvent, and a slurry with a solid content of 70wt% is prepared. After vacuum stirring, the positive electrode slurry is obtained. The positive electrode slurry is evenly coated on one surface of a positive electrode current collector aluminum foil with a thickness of 10μm, and dried at 120°C to obtain a positive electrode sheet coated with a single-sided positive electrode material layer. Then repeat the above steps on the other surface of the aluminum foil to obtain a positive electrode sheet coated with a positive electrode material layer on both sides. After drying at 120°C, cold pressing is performed, and then cutting and welding of the positive electrode aluminum ears are performed to obtain a positive electrode sheet with a specification of 74mm×851mm for standby use. Among them, the thickness of the positive electrode material layer is 92μm, and the compaction density of the positive electrode material layer is 4.15g / cm 3 .
[0100] <Preparation of Separator Film>
[0101] A porous polyethylene film with a thickness of 7 μm (provided by Celgard) was used as the substrate layer. Inorganic particles of aluminum oxide and inorganic layer binder polyvinylidene fluoride (Mw = 7×10 6 ) were mixed at a mass ratio of 4:1, N-methylpyrrolidone (NMP) was added, and the mixture was stirred evenly under the action of a vacuum mixer to obtain an inorganic slurry with a solid content of 30wt%, and the inorganic slurry was evenly coated on one surface of the substrate layer to form an inorganic layer with a thickness of 2μm. Then, the polymer polyvinylidene fluoride (Mw = 7×10 6 ) was dissolved in deionized water to obtain a polymer layer slurry with a solid content of 25 wt%, and then the polymer layer slurry was evenly coated on the surface of the inorganic layer on one side and the substrate layer on the other side, with a coating surface density of 2.5 mg / cm 2 , forming a polymer layer, and obtaining an isolation membrane containing an inorganic layer and a polymer layer on one side and only a polymer layer on the other side.
[0102] <Preparation of lithium-ion batteries>
[0103] The positive electrode sheet, separator and negative electrode sheet prepared above are stacked and wound in sequence to obtain an electrode assembly with a wound structure, wherein the side of the separator containing the inorganic layer and the polymer layer faces the positive electrode sheet, and the side containing only the polymer layer faces the negative electrode sheet. The electrode assembly is placed in an aluminum-plastic film packaging bag, and after drying, the electrolyte is injected, and a lithium-ion battery is obtained through vacuum packaging, standing, formation (0.3C constant current charging to 3.5V, and then 1C constant current charging to 3.9V), capacity, degassing, trimming and other processes.
[0104] Example 1-2 to Example 1-16
[0105] Except for adjusting the relevant preparation parameters in <Preparation of Negative Electrode Sheet> and <Preparation of Electrolyte> according to Table 1, the rest is the same as Example 1-1. Among them, the coating surface density of the first negative electrode material layer is adjusted to adjust the H 1 By adjusting the coating surface density of the second negative electrode material layer, H 2 When the mass percentage of lithium difluorophosphate is W 1 % or the mass percentage of propyl propionate W 2 When % changes, the mass percentage of the basic solvent changes accordingly, and the mass ratio of each component in the basic solvent and the mass percentage of the lithium salt remain unchanged.
[0106] Example 2-1 to Example 2-7
[0107] In addition to adjusting the coating surface density of the first negative electrode material layer in <Preparation of negative electrode sheet>, H 1 The values are shown in Table 2. In the preparation of the electrolyte, the polynitrile compound 1,2,3-tris(2-cyanoethoxy)propane is added as shown in Table 2, and the rest is the same as in Example 1-1. 3 % changes, the mass percentage of the basic solvent changes accordingly, and the mass ratio of each component in the basic solvent, the mass percentage of lithium salt, lithium difluorophosphate and propyl propionate remain unchanged.
[0108] Example 2-8 to Example 2-10
[0109] Except that the propionate compound methyl propionate is added in the preparation of the electrolyte as shown in Table 2, the rest is the same as Example 1-1. 2 % and the mass percentage of propionate compounds W 4 When % changes, the mass percentage of the basic solvent changes accordingly, and the mass ratio of each component in the basic solvent, the mass percentage of the lithium salt and the lithium difluorophosphate remain unchanged.
[0110] Example 2-11
[0111] In addition to adding the polynitrile compound 1,2,3-tri(2-cyanoethoxy)propane and the propionate compound methyl propionate as shown in Table 2 in <Preparation of Electrolyte>, the mass percentage of the base solvent changes accordingly, and the mass ratio of each component in the base solvent, the mass percentage of lithium salt and lithium difluorophosphate remain unchanged, the rest is the same as Example 1-1.
[0112] Example 3-1 to Example 3-8
[0113] Except for adjusting the relevant preparation parameters in <Preparation of Negative Electrode Sheet> according to Table 1, the rest is the same as Example 1-1. Among them, the Dv50, Dv90 of the first negative electrode active material and the Dv50, Dv90 of the second negative electrode active material are adjusted by adjusting the ball milling time.
[0114] Comparative Example 1
[0115] Except that the following preparation method is used for <Preparation of Negative Electrode Sheet>, the rest is the same as Example 1-1.
[0116] <Preparation of negative electrode sheet>
[0117] The negative electrode active material artificial graphite and the negative electrode binder styrene butadiene rubber (SBR, Mw = 5 × 10 6 ), thickener sodium carboxymethyl cellulose (CMC-Na, Mw = 7 × 10 5 ), the negative electrode conductive agent conductive carbon black (Super P) was mixed in a mass ratio of 96:1.5:1.5:1, and then deionized water was added as a solvent to prepare a slurry with a solid content of 50wt%, and the negative electrode slurry was obtained after vacuum stirring. The negative electrode slurry was evenly coated on one surface of the negative electrode current collector copper foil with a thickness of 10μm, and the coating surface density was 8.14mg / cm 2 , dried at 85°C to obtain a negative electrode sheet coated with a negative electrode material layer on one side. After that, repeat the above steps on the other surface of the copper foil to obtain a negative electrode sheet coated with a negative electrode material layer on both sides. After cold pressing, cutting, and welding of the negative electrode tab nickel tab, a negative electrode sheet with a specification of 76mm×867mm is obtained for standby use. Among them, the thickness of the negative electrode material layer is 105μm, and the Dv50 of the negative active material is 11μm and the Dv90 is 22μm.
[0118] Comparative Examples 2 to 5
[0119] Except for adjusting the relevant preparation parameters in Table 1 in <Preparation of Negative Electrode Sheet>, the rest is the same as Example 1-1. Among them, the coating surface density of the first negative electrode material layer is adjusted to adjust H 1 By adjusting the coating surface density of the second negative electrode material layer, H 2 .
[0120] Comparative Example 6
[0121] Except that lithium difluorophosphate is not added in <Preparation of Electrolyte>, the mass percentage of the base solvent changes accordingly, and the mass ratio of each component in the base solvent, the mass percentage of lithium salt and propyl propionate remain unchanged, the rest is the same as Example 1-1.
[0122] Comparative Example 7 to Comparative Example 8
[0123] Except for adjusting the relevant preparation parameters in Table 1 in <Preparation of Electrolyte>, the rest is the same as Example 1-1. 1 % changes, the mass percentage of the basic solvent changes accordingly, and the mass ratio of each component in the basic solvent, the mass percentage of the lithium salt and propyl propionate remain unchanged.
[0124] Comparative Example 9
[0125] Except that propyl propionate is not added in <Preparation of Electrolyte>, the mass percentage of the base solvent changes accordingly, and the mass ratio of each component in the base solvent, the mass percentage of lithium salt and lithium difluorophosphate remain unchanged, the rest is the same as Example 1-1.
[0126] Comparative Example 10 to Comparative Example 11
[0127] Except for adjusting the relevant preparation parameters in Table 1 in <Preparation of Electrolyte>, the rest is the same as Example 1-1. 2 When % changes, the mass percentage of the basic solvent changes accordingly, and the mass ratio of each component in the basic solvent, the mass percentage of the lithium salt and the lithium difluorophosphate remain unchanged.
[0128] Comparative Example 12
[0129] Except that lithium difluorophosphate and propyl propionate are not added in <Preparation of Electrolyte>, the mass percentage of the base solvent changes accordingly, and the mass ratio of each component in the base solvent and the mass percentage of the lithium salt remain unchanged, the rest is the same as Example 1-1.
[0130] Comparative Example 13
[0131] Except that the relevant preparation parameters in <Preparation of Negative Electrode Sheet> are adjusted according to Table 1, the Dv50 of the first negative electrode active material is 11μm, Dv90 is 22μm, and the Dv50 of the second negative electrode active material is 13μm, Dv90 is 23μm, the rest is the same as Example 1-1.
[0132] The preparation parameters and performance parameters of each embodiment and comparative example are shown in Tables 1 to 3.
[0133] Table 1
[0134]
[0135] Note: “ / ” in Table 1 means there is no corresponding parameter.
[0136] It can be seen from Examples 1-1 to 1-16 and Comparative Examples 1 to 13 that the present invention designs the negative electrode structure and electrolyte composition, and regulates H 1 , H2 , W 1 , W 2 , W 1 ×H 1 The value of is within the scope of this application, and the Dv50 of the first negative electrode active material is regulated to be greater than the Dv50 of the second negative electrode active material, the R 1 , R 2 , R 3 , K is smaller, that is, the initial impedance and the impedance growth during the cycle are smaller, and D is larger, indicating that the lithium-ion battery has good dynamic performance and high-temperature floating charge performance. The negative electrode sheet of the lithium-ion battery in Comparative Example 1 does not include the first negative electrode material layer and the second negative electrode material layer; the lithium-ion batteries in Comparative Examples 2 and 3 have H 1 The value of is not within the scope of this application; the lithium ion batteries of Comparative Examples 4 to 5, whose H 2 The value is not within the scope of this application; the lithium ion battery of Comparative Example 6, the electrolyte does not include lithium difluorophosphate and W 1 ×H 1 The value of is not within the scope of this application; the lithium ion batteries of Comparative Examples 7 to 8, whose W 1 and W 1 ×H 1 The value is not within the scope of the present application; the lithium ion battery of Comparative Example 9, the electrolyte does not include propyl propionate; the lithium ion batteries of Comparative Examples 10 to 11, their W 2 The value of is not within the scope of the present application; the lithium ion battery of Comparative Example 12, whose electrolyte does not include lithium difluorophosphate and propyl propionate, the lithium ion battery of Comparative Example 13, whose Dv50 of the first negative electrode active material is less than the Dv50 of the second negative electrode active material, the lithium ion batteries of Comparative Examples 1 to Comparative Examples 13, R 1 , R 2 , R 3 , K is larger, that is, the initial impedance and the impedance growth during the cycle are larger, and D is smaller, indicating that the kinetic performance and high-temperature floating charge performance of the lithium-ion battery are poor.
[0137] H 1 The value of usually affects the dynamic performance and high temperature floating charge performance of lithium ion batteries. From Example 1-1 to Example 1-3 and Comparative Example 2 to Comparative Example 3, it can be seen that when H 1 The value of is too small, for example, in Comparative Example 2, the R 1 , R 2 , R 3 , K is larger, that is, the initial impedance and the impedance growth during the cycle are larger, and D is smaller; when H 1 When the value of is too large, for example, in Comparative Example 3, the R 1 , R 2 , R3 , K is larger, that is, the initial impedance and the impedance growth during the cycle are larger, and D is smaller, indicating that the kinetic performance and high-temperature floating charge performance of the lithium-ion battery are poor. 1 When the value is within the range of this application, the R 1 , R 2 , R 3 , K is smaller, that is, the initial impedance and the impedance growth during the cycle are smaller, and D is larger, indicating that the lithium-ion battery has good kinetic performance and high-temperature floating charge performance.
[0138] H 2 The value of usually affects the dynamic performance and high temperature floating charge performance of lithium ion batteries. It can be seen from Example 1-1, Example 1-4 to Example 1-5, Comparative Example 4 to Comparative Example 5 that when H 2 The value of is too small, for example, in Comparative Example 4, the R 1 , R 2 , R 3 , K is larger, that is, the initial impedance and the impedance growth during the cycle are larger, and D is smaller; when H 2 When the value of is too large, for example, in Comparative Example 5, the R 1 , R 2 , R 3 , K is larger, that is, the initial impedance and the impedance growth during the cycle are larger, and D is smaller, indicating that the kinetic performance and high-temperature floating charge performance of the lithium-ion battery are poor. 2 When the value is within the range of this application, the R 1 , R 2 , R 3 , K is smaller, that is, the initial impedance and the impedance growth during the cycle are smaller, and D is larger, indicating that the lithium-ion battery has good kinetic performance and high-temperature floating charge performance.
[0139] The relationship between the Dv50 of the first negative electrode active material and the second negative electrode active material usually affects the kinetic performance and high temperature floating charge performance of the lithium ion battery. It can be seen from Example 1-1 and Comparative Example 13 that when the Dv50 of the first negative electrode active material is less than the Dv50 of the second negative electrode active material, such as in Comparative Example 13, the R 1 , R 2 , R 3 , K is larger, that is, the initial impedance and the impedance growth during the cycle are larger, and D is smaller, indicating that the kinetic performance and high-temperature floating charge performance of the lithium-ion battery are poor. When the Dv50 of the first negative electrode active material is greater than the Dv50 of the second negative electrode active material, the R 1 , R 2 , R 3, K is smaller, that is, the initial impedance and the impedance growth during the cycle are smaller, and D is larger, indicating that the lithium-ion battery has good kinetic performance and high-temperature floating charge performance.
[0140] W 1 The value of W usually affects the dynamic performance and high temperature floating charge performance of lithium ion batteries. It can be seen from Example 1-1, Example 1-7 to Example 1-10, and Comparative Example 6 to Comparative Example 8 that when W 1 If the value of is too small, such as in Comparative Examples 6 and 7, the R 1 , R 2 , R 3 , K is larger, that is, the initial impedance and the impedance growth during the cycle are larger, and D is smaller; when W 1 When the value of is too large, for example, in Comparative Example 8, the R 1 , R 2 , R 3 , K is larger, that is, the initial impedance and the impedance growth during the cycle are larger, and D is smaller, indicating that the kinetic performance and high-temperature floating charge performance of the lithium-ion battery are poor. 1 When the value is within the range of this application, the R 1 , R 2 , R 3 , K is smaller, that is, the initial impedance and the impedance growth during the cycle are smaller, and D is larger, indicating that the lithium-ion battery has good kinetic performance and high-temperature floating charge performance.
[0141] W 2 The value of W usually affects the dynamic performance and high temperature floating charge performance of lithium ion batteries. It can be seen from Example 1-1, Example 1-13 to Example 1-14, Comparative Example 9 to Comparative Example 11 that when W 2 The value of is too small, such as in Comparative Examples 9 and 10, the R 1 , R 2 , R 3 , K is larger, that is, the initial impedance and the impedance growth during the cycle are larger, and D is smaller; when W 2 When the value of is too large, for example, in Comparative Example 11, the R 1 , R 2 , R 3 , K is larger, that is, the initial impedance and the impedance growth during the cycle are larger, and D is smaller, indicating that the kinetic performance and high-temperature floating charge performance of the lithium-ion battery are poor. 2 When the value is within the range of this application, the R 1 , R 2 , R 3, K is smaller, that is, the initial impedance and the impedance growth during the cycle are smaller, and D is larger, indicating that the lithium-ion battery has good kinetic performance and high-temperature floating charge performance.
[0142] W 1 ×H 1 The value of W usually affects the dynamic performance and high temperature floating charge performance of lithium ion batteries. It can be seen from Example 1-1, Example 1-7 to Example 1-10, and Comparative Example 6 to Comparative Example 8 that when W 1 ×H 1 If the value of is too small, such as in Comparative Examples 6 and 7, the R 1 , R 2 , R 3 , K is larger, that is, the initial impedance and the impedance growth during the cycle are larger, and D is smaller; when W 1 ×H 1 When the value of is too large, for example, in Comparative Example 8, the R 1 , R 2 , R 3 , K is larger, that is, the initial impedance and the impedance growth during the cycle are larger, and D is smaller, indicating that the kinetic performance and high-temperature floating charge performance of the lithium-ion battery are poor. 1 ×H 1 When the value is within the range of this application, the R 1 , R 2 , R 3 , K is smaller, that is, the initial impedance and the impedance growth during the cycle are smaller, and D is larger, indicating that the lithium-ion battery has good kinetic performance and high-temperature floating charge performance.
[0143] H 2 / H 1 The value of usually affects the dynamic performance and high temperature floating charge performance of lithium-ion batteries. From Examples 1-1 to 1-6, it can be seen that when H 2 / H 1 When the value is within the range of this application, the R 1 , R 2 , R 3 , K is small, that is, the initial impedance and the impedance growth during the cycle are small, and D is large, indicating that the lithium-ion battery has good kinetic performance and high-temperature floating charge performance.
[0144] W 1 / H 1 The value of W usually affects the dynamic performance and high temperature floating charge performance of lithium-ion batteries. 1 / H 1 When the value is within the range of this application, the R1 , R 2 , R 3 , K is small, that is, the initial impedance and the impedance growth during the cycle are small, and D is large, indicating that the lithium-ion battery has good kinetic performance and high-temperature floating charge performance.
[0145] W 2 ×H 1 The value of W usually affects the dynamic performance and high temperature floating charge performance of lithium-ion batteries. 2 ×H 1 When the value is within the range of this application, the R 1 , R 2 , R 3 , K is small, that is, the initial impedance and the impedance growth during the cycle are small, and D is large, indicating that the lithium-ion battery has good kinetic performance and high-temperature floating charge performance.
[0146] from Figure 2 It can be seen that the impedance of the lithium ion battery of Example 1-1 is 46.1 mΩ at the 300th cycle, and the impedance is 50.4 mΩ at the 1000th cycle, and the K value is 6.14×10 -3 mΩ / cycle. The impedance of the lithium-ion battery in Comparative Example 1 is 59.0 mΩ at the 300th cycle and 66.2 mΩ at the 1000th cycle, and the K value is 10.29×10 -3 The K value of Example 1-1 is smaller than that of Comparative Example 1, indicating that the impedance growth of the lithium ion battery of Example 1-1 during the cycle is smaller and the kinetic performance is better.
[0147] from Figure 3 It can be seen that under the same charging time, the thickness change rate of the lithium ion battery of Example 1-1 is smaller. When the thickness change rate of the lithium ion battery reaches 108.5%, D of Example 1-1 is 1248h, while D of Comparative Example 1 is 932h. The D value of Example 1-1 is larger than that of Comparative Example 1, indicating that the high-temperature floating charge performance of the lithium ion battery of Example 1-1 is better.
[0148] Table 2
[0149]
[0150] Note: “ / ” in Table 2 means there is no corresponding parameter.
[0151] The electrolyte includes a polynitrile compound and a mass percentage content W of the polynitrile compound. 3% usually affects the dynamic performance and high temperature floating performance of lithium ion batteries. It can be seen from Examples 1-1, 2-1 to 2-7, and 2-11 that when the electrolyte includes a polynitrile compound and the mass percentage content of the polynitrile compound is adjusted W 3 % Within the scope of this application, the R 1 , R 2 , R 3 , K is small, that is, the initial impedance and the impedance growth during the cycle are small, and D is large, indicating that the lithium-ion battery has good kinetic performance and high-temperature floating charge performance.
[0152] W 3 ×H 1 The value of usually affects the dynamic performance and high temperature floating charge performance of lithium-ion batteries. It can be seen from Examples 1-1, 2-1 to 2-7, and 2-11 that when W 3 ×H 1 When the value is within the range of this application, the R 1 , R 2 , R 3 , K is small, that is, the initial impedance and the impedance growth during the cycle are small, and D is large, indicating that the lithium-ion battery has good kinetic performance and high-temperature floating charge performance.
[0153] The electrolyte includes a propionate compound and a mass percentage content W of the propionate compound. 4 % usually affects the dynamic performance and high temperature floating performance of lithium ion batteries. It can be seen from Examples 1-1, 2-8 to 2-10 that when the electrolyte includes a propionate compound and the mass percentage content of the propionate compound is adjusted W 4 % Within the scope of this application, the R 1 , R 2 , R 3 , K is small, that is, the initial impedance and the impedance growth during the cycle are small, and D is large, indicating that the lithium-ion battery has good kinetic performance and high-temperature floating charge performance.
[0154] W 2 / W 4 The value of W usually affects the dynamic performance and high temperature floating charge performance of lithium-ion batteries. 2 / W 4 When the value is within the range of this application, the R 1 , R 2 , R 3, K is small, that is, the initial impedance and the impedance growth during the cycle are small, and D is large, indicating that the lithium-ion battery has good kinetic performance and high-temperature floating charge performance.
[0155] Table 3
[0156]
[0157] The Dv50 and Dv90 of the first negative electrode active material usually affect the kinetic performance and high temperature floating charge performance of the lithium ion battery. It can be seen from Examples 1-1, 3-1 and 3-4 that when the Dv50 and Dv90 of the first negative electrode active material are within the range of this application, the R 1 , R 2 , R 3 , K is small, that is, the initial impedance and the impedance growth during the cycle are small, and D is large, indicating that the lithium-ion battery has good kinetic performance and high-temperature floating charge performance.
[0158] The Dv50 and Dv90 of the second negative electrode active material usually affect the kinetic performance and high temperature floating charge performance of the lithium ion battery. It can be seen from Examples 1-1, 3-5 to 3-7 that when the Dv50 and Dv90 of the second negative electrode active material are within the range of this application, the R 1 , R 2 , R 3 , K is small, that is, the initial impedance and the impedance growth during the cycle are small, and D is large, indicating that the lithium-ion battery has good kinetic performance and high-temperature floating charge performance.
[0159] The type of the first negative electrode active material usually affects the kinetic performance and high temperature floating charge performance of the lithium ion battery. It can be seen from Examples 1-1 and 3-8 that the first negative electrode active material within the scope of this application is selected, and the R 1 , R 2 , R 3 , K is small, that is, the initial impedance and the impedance growth during the cycle are small, and D is large, indicating that the lithium-ion battery has good kinetic performance and high-temperature floating charge performance.
[0160] The type of the second negative electrode active material usually affects the kinetic performance and high temperature floating charge performance of the lithium ion battery. It can be seen from Examples 1-1 and 3-8 that the selection of the second negative electrode active material within the scope of the present application can improve the R 1 , R 2 , R 3 , K is small, that is, the initial impedance and the impedance growth during the cycle are small, and D is large, indicating that the lithium-ion battery has good kinetic performance and high-temperature floating charge performance.
[0161] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0162] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.
[0163] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.
Claims
1. A secondary battery, comprising a negative electrode plate and an electrolyte, wherein the negative electrode plate comprises a negative electrode current collector and a negative electrode material layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode material layer comprises a first negative electrode material layer and a second negative electrode material layer stacked, wherein the second negative electrode material layer is located between the first negative electrode material layer and the negative electrode current collector, wherein the thickness of the first negative electrode material layer is H1 μm, the thickness of the second negative electrode material layer is H2 μm, 20≤H1≤40, 60≤H2≤90; The first negative electrode material layer includes a first negative electrode active material, the second negative electrode material layer includes a second negative electrode active material, and the Dv50 of the first negative electrode active material is greater than the Dv50 of the second negative electrode active material; The electrolyte includes lithium difluorophosphate and a propionate compound, and the propionate compound includes propyl propionate; based on the mass of the electrolyte, the mass percentage of the lithium difluorophosphate is W1%, the mass percentage of the propyl propionate is W2%, 0.1≤W1≤1, 10≤W2≤60, 4≤W1×H1≤35.
2. The secondary battery according to claim 1, wherein 2≤H2 / H1≤4.
5.
3. The secondary battery according to claim 1, wherein 0.005≤W1 / H1≤0.
05.
4. The secondary battery according to claim 1, wherein 250≤W2×H1≤2400.
5. The secondary battery according to any one of claims 1 to 4, wherein The electrolyte comprises a polynitrile compound, and based on the mass of the electrolyte, the mass percentage of the polynitrile compound is W3%, 0.1≤W3≤5; The polynitrile compound includes at least one of succinonitrile, glutaronitrile, adiponitrile, pimelonitrile, suberonitrile, methylglutaronitrile, 1,3,5-pentanetricarbonitrile, 1,2,3-propanetricarbonitrile, 1,3,6-hexanetricarbonitrile or 1,2,3-tris(2-cyanoethoxy)propane.
6. The secondary battery according to claim 5, wherein 50≤W3×H1≤200.
7. The secondary battery according to any one of claims 1 to 4, wherein Based on the mass of the electrolyte, the mass percentage of the propionate compound is W4%, 10≤W4≤65, 0.154≤W2 / W4≤1.
8. The secondary battery according to claim 7, wherein The propionate compound further includes at least one of methyl propionate, ethyl propionate, butyl acrylate or butyl propionate.
9. The secondary battery according to any one of claims 1 to 4, wherein The Dv50 of the first negative electrode active material is 12 μm to 14.9 μm, and the Dv90 of the first negative electrode active material is 20.5 μm to 25.9 μm.
10. The secondary battery according to any one of claims 1 to 4, wherein The Dv50 of the second negative electrode active material is 10 μm to 11.5 μm, and the Dv90 of the second negative electrode active material is 19.4 μm to 24.8 μm.
11. The secondary battery according to any one of claims 1 to 4, wherein The first negative electrode active material and the second negative electrode active material each independently include at least one of natural graphite, artificial graphite, soft carbon, hard carbon, mesophase carbon microbeads, silicon-carbon compounds, silicon-oxygen compounds or lithium titanate. 12 . An electronic device comprising the secondary battery according to claim 1 .
Citation Information
Cited By
Secondary battery and electronic device
EP4773341A1
Secondary battery and electronic device