Aluminum-plastic composite film, preparation method thereof and lithium ion battery

By using an aluminum-plastic composite film structure with an aluminum alloy layer and a graphene-nano-silicon composite layer in the lithium-ion battery film, the problem of insufficient mechanical and corrosion resistance of the existing film is solved, and the sealing and deep forming performance are improved. And the safety performance is enhanced through the PET antifouling layer, enabling a more efficient battery film design.

CN118738692APending Publication Date: 2024-10-01浙江华正能源材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410761194.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing aluminum-plastic composite films for lithium-ion batteries have deficiencies in mechanical properties, electrolyte corrosion resistance and deep forming performance, and the accumulation of static charges may lead to safety hazards.

Method used

An aluminum-plastic composite film using a CPP heat sealing layer, an aluminum alloy layer, a graphene-nano-silicon composite layer and a PET antifouling layer laminated in sequence is prepared through evaporation and physical vapor deposition processes. The graphene-nano-silicon composite layer is used Improve mechanical properties and anti-static properties, and the PET antifouling layer is used to prevent electrolyte corrosion.

Benefits of technology

It significantly improves the density, strength, sealing performance, deep forming performance, corrosion resistance and safety performance of the aluminum-plastic composite film, simplifies the preparation process, is suitable for industrial production, and improves the performance and safety performance of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004891115570000061
    Figure BDA0004891115570000061
Patent Text Reader

Abstract

The invention belongs to the technical field of aluminum-plastic films, and particularly relates to an aluminum-plastic composite film, a preparation method thereof and a lithium ion battery. The aluminum-plastic composite film comprises a CPP heat sealing layer, an aluminum alloy layer, a graphene-nano silicon composite layer, a bonding layer and a PET antifouling layer which are sequentially stacked, wherein the aluminum alloy layer is evaporated on the CPP heat sealing layer, and the graphene-nano silicon composite layer is deposited on the aluminum alloy layer through physical vapor deposition. Compared with an aluminum-plastic film with a conventional structure, the aluminum-plastic composite film is lower in density, higher in strength, better in sealing performance, deep punching forming performance, corrosion resistance and warping resistance, more environmentally friendly and better in safety performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aluminum-plastic films, and in particular relates to an aluminum-plastic composite film and a preparation method thereof, and a lithium ion battery. Background Art

[0002] The black aluminum-plastic composite film structure commonly used in lithium-ion batteries is generally a composite material composed of nylon (outer protective layer), a black masterbatch bonding layer, an aluminum foil layer (middle barrier layer), an inner bonding layer, and polypropylene (inner heat sealing layer). Its main function is to serve as a lithium battery packaging film to protect the internal structure of the lithium battery.

[0003] Among them, aluminum and aluminum alloys have excellent properties such as low density, high strength and good ductility, and are widely used in the aerospace and automotive industries, but the poor mechanical properties of aluminum limit its wide application in other fields. Existing nylon has excellent mechanical properties, but it is not resistant to electrolyte corrosion, and is prone to breakage or pinhole cracks during the deep-drawing process, which not only affects the deep-drawing performance of aluminum-plastic film, but also poses a safety hazard. Graphene has extremely low surface resistance, and static charges can be quickly conducted or dissipated on the surface of the film, avoiding the accumulation of static charges and improving safety performance, especially in the field of power batteries, where overheating of the battery poses a risk of explosion. Summary of the invention

[0004] Based on the above-mentioned shortcomings and deficiencies in the prior art, the object of the present invention is to provide an aluminum-plastic composite film and a preparation method thereof and a lithium ion battery.

[0005] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:

[0006] An aluminum-plastic composite film comprises a CPP heat-sealing layer, an aluminum alloy layer, a graphene-nano silicon composite layer, an adhesive layer and a PET antifouling layer which are stacked in sequence; wherein the aluminum alloy layer is evaporated on the CPP heat-sealing layer, and the graphene-nano silicon composite layer is physically vapor deposited on the aluminum alloy layer.

[0007] As a preferred embodiment, the mass ratio of graphene to nano-silicon in the graphene-nano-silicon composite layer is 1:(2-8).

[0008] As a preferred solution, the thickness of the CPP heat-sealing layer is 15-80 μm, the thickness of the aluminum alloy layer is 20-45 μm, the thickness of the graphene-nanosilicon composite layer is 15-25 μm, the thickness of the adhesive layer is 2-5 μm, and the thickness of the PET antifouling layer is 6-12 μm.

[0009] As a preferred solution, the glue of the adhesive layer is a multifunctional polyurethane resin adhesive.

[0010] As a preferred solution, the thickness of the aluminum-plastic composite film is 58-167 μm.

[0011] The present invention also provides a method for preparing the aluminum-plastic composite film as described in any of the above schemes, comprising the following steps:

[0012] (1) A CPP heat-sealing layer cast film is selected as a vapor deposition substrate, firstly plasma-cleaned, then sent into a vapor deposition chamber through a guide roller, evacuated to a vacuum degree of ≤100 MPa, heated to 1300-1800° C. by high-frequency current, and cooled and deposited an aluminum alloy layer on the surface of the heat-sealing layer cast film through a cooling roller;

[0013] (2) blowing graphene and nano-silicon from bottom to top in the evaporation chamber through airflow to physically vapor deposit a graphene-nano-silicon composite layer on the surface of the aluminum alloy layer;

[0014] (3) Dry-bonding the PET antifouling layer on the surface of the graphene-nano silicon composite layer and curing it.

[0015] As a preferred embodiment, in step (1), the plasma cleaning process is as follows: the vacuum degree of the cleaning chamber is ≤100 MPa, and the cleaning time is 1-5 s.

[0016] As a preferred embodiment, in step (1), the evaporation material in the evaporation chamber includes the following components in weight percentage: 0.01-0.2% titanium, 0.2-1% manganese, 0.05-0.2% chromium, 0.1-0.5% zinc, 1-3% magnesium, 2-6% copper, and the rest is aluminum;

[0017] The temperature of the cooling roller is -80 to -5°C.

[0018] As a preferred embodiment, in step (3), the aging process is: placing at 50-70°C for 48-144 hours.

[0019] The present invention also provides a lithium ion battery packaged with the aluminum-plastic composite film as described in any of the above solutions.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) The aluminum-plastic composite film of the present invention has lower density, higher strength, better sealing performance, deep forming performance, corrosion resistance and anti-warping performance, and is more environmentally friendly and has better safety performance than conventional aluminum-plastic films.

[0022] (2) The preparation process of the present invention is simple and suitable for industrial production;

[0023] (3) The lithium-ion battery of the present invention adopts the aluminum-plastic composite film of the present invention, and has better performance and safety performance. DETAILED DESCRIPTION

[0024] The technical solution of the present invention is further explained below through specific embodiments.

[0025] Embodiment 1:

[0026] The method for preparing the aluminum-plastic composite film of the present embodiment comprises the following steps:

[0027] The CPP heat-sealing layer cast film is selected as the evaporation substrate, and the CPP is plasma cleaned. The vacuum degree of the cleaning chamber is 100MPa, and the cleaning time is 3s. After cleaning, it is sent to the vacuum chamber through a guide roller and evacuated to a vacuum degree of 100MPa. The evaporation chamber is heated to 1400°C by a current high-frequency heating method. Among them, the evaporation material in the aluminum evaporation chamber is 0.2% titanium, 0.5% manganese, 0.1% chromium, 0.5% zinc, 3% magnesium, 5% copper, and the rest is aluminum; then a layer of aluminum alloy layer is cooled and deposited on the surface of the CPP by a cooling roller, and the temperature of the cooling roller is -20°C;

[0028] Then, graphene and nano-silicon are blown into the evaporation chamber from bottom to top by airflow, and the mass ratio of graphene to nano-silicon is 3:7, so that a graphene-nano-silicon (Gr-NSi) composite layer is physically vapor deposited on the surface of the aluminum alloy layer;

[0029] Finally, a layer of antifouling PET transparent film was dry-laminated on the Gr-NSi composite layer and aged at 60°C for 48 hours to obtain an aluminum-plastic composite film. The glue used for dry lamination is a multifunctional polyurethane resin adhesive, which is made of VN930 (main agent) + CA-N6 (curing agent) from Shanghai Weikai Optoelectronic New Materials Co., Ltd., with a volume ratio of 100:14.

[0030] The aluminum-plastic composite film of this embodiment includes a CPP heat-sealing layer, an aluminum alloy layer, a graphene-nanosilicon composite layer, an adhesive layer and a PET antifouling layer stacked in sequence, wherein the thickness of the CPP heat-sealing layer is 60 μm, the thickness of the aluminum alloy layer is 30 μm, the thickness of the Gr-NSi composite layer is 15 μm, the thickness of the adhesive layer is 5 μm, the thickness of the PET antifouling layer is 10 μm, and the total thickness of the aluminum-plastic composite film is 120 μm.

[0031] The aluminum-plastic composite film of this embodiment uses a vapor-deposited aluminum alloy layer instead of commercially available aluminum foil, and a Gr-NSi composite layer instead of a PA film layer. The CPP heat-sealing layer and the aluminum alloy layer, and the aluminum alloy layer and the Gr-NSi composite layer are all directly composited by a vapor deposition process. The adhesive layer in the middle is omitted, the process is more environmentally friendly, and the sealing performance and electrolyte resistance of the aluminum-plastic composite film are also better.

[0032] Embodiment 2:

[0033] The aluminum-plastic composite film of this embodiment is different from that of Embodiment 1 in that:

[0034] In the evaporation chamber, only graphene is blown in from bottom to top by air flow, and a layer of graphene (Gr) is physically vapor deposited on the surface of the aluminum alloy layer;

[0035] The rest is the same as in Example 1.

[0036] Embodiment 3:

[0037] The aluminum-plastic composite film of this embodiment is different from that of Embodiment 1 in that:

[0038] In the evaporation chamber, only nano-silicon powder is blown in from bottom to top by air flow, and a layer of nano-silicon (NSi) is physically vapor-deposited on the surface of the aluminum alloy layer;

[0039] The rest is the same as in Example 1.

[0040] Embodiment 4:

[0041] The aluminum-plastic composite film of this embodiment is different from that of Embodiment 1 in that:

[0042] A layer of nylon PA film is directly dry-laminated on the surface of the aluminum alloy layer to replace the Gr-NSi composite layer, and a layer of anti-fouling PET transparent film is dry-laminated on the surface of the nylon PA film;

[0043] The thickness of nylon (PA) film is 15 μm;

[0044] The rest is the same as in Example 1.

[0045] Embodiment 5:

[0046] The aluminum-plastic composite film of this embodiment is different from that of Embodiment 1 in that:

[0047] The evaporated aluminum layer is an aluminum evaporated layer of pure aluminum vapor;

[0048] The rest is the same as in Example 1.

[0049] Embodiment 6:

[0050] The aluminum-plastic composite film of this embodiment is different from that of embodiment 2 in that the evaporated aluminum foil layer is an aluminum evaporated layer of pure aluminum vapor;

[0051] The rest is the same as Example 2.

[0052] Embodiment 7:

[0053] The aluminum-plastic composite film of this embodiment is different from that of embodiment 3 in that the evaporated aluminum foil layer is an aluminum evaporated layer of pure aluminum vapor;

[0054] The rest is the same as in Example 3.

[0055] Embodiment 8:

[0056] The preparation process of the aluminum-plastic composite film of this embodiment is as follows:

[0057] The patent document with application number 201911126888.2 discloses a method for preparing a high-barrier aluminum-plastic film for lithium battery soft packaging, which comprises vapor-depositing an aluminum / graphene co-deposited layer on a PA cast film and then thermally compounding the CPP cast film.

[0058] Comparative Example 1:

[0059] The aluminum-plastic film of this comparative example differs from that of Example 4 in that the aluminum vapor-deposited layer is replaced by commercially available aluminum foil;

[0060] The rest is the same as in Example 1.

[0061] The following performance tests were performed on the aluminum-plastic films of Examples 1-8 and Comparative Example 1:

[0062] 1. Deep drawing performance test:

[0063] Specimen size: 120mm×10mm, punching die model: 104050, die side R1.5, corner R1.5, punching depth: 7.0mm.

[0064] 2. Anti-warping performance test

[0065] Measure the aluminum-plastic film specimens in the deep-drawing test and compare the difference in warpage.

[0066] 3. Inner layer electrolyte resistance test

[0067] Sample size: 150mm×15mm. The sample was immersed in a PP bottle of electrolyte at 85℃ for 4 weeks and then tested.

[0068] 4. Moisture barrier performance test

[0069] Sample size: 200mm×10mm. Fold the sample in half and heat seal both sides to form a bag with one side open. Dehydrate the electrolyte to 20-50ppm in advance, inject 5mL of electrolyte in the glove box (nitrogen atmosphere), slightly squeeze the gas in the bag and heat seal. Place the sample in a 60℃ / 90%RH constant temperature and humidity chamber for 4 weeks, and then test the water permeability in the sample bag.

[0070] The above test results are shown in Table 1:

[0071] Table 1 Performance test results comparison table

[0072]

[0073] From the performance comparison between the aluminum-plastic films of the above embodiments and comparative examples, it can be seen that the deep-drawing forming performance, anti-warping performance, electrolyte resistance performance and moisture barrier performance of the composite aluminum-plastic film of the present invention are significantly improved. The thermal bonding adopted in Example 8 can improve the adhesion between the aluminum foil layer and the CPP layer, improve the ability of the inner layer to prevent the swelling and shedding of the electrolyte, thereby improving the electrolyte resistance performance of the inner layer, and greatly improve the moisture barrier performance, but the CPP used in this process needs high temperature and high pressure conditions to play a bonding role. Due to long-term high-temperature baking, the aluminum-plastic film becomes brittle, thereby greatly reducing its deep-drawing performance; and after cooling, because the shrinkage coefficients of each layer also have large differences, the aluminum-plastic film is prone to curling, and the appearance of the finished product is also poor.

[0074] The present invention directly vacuum evaporates a layer of aluminum foil on a plasma-cleaned heat-sealing layer CPP by a vapor deposition method (PVD) to replace the commonly used dry-type aluminum foil laminating method. Since the density of the evaporated coating is poor, trace metal elements such as Zn, Mg, and Gr are doped in the aluminum vapor to improve the ductility of the aluminum foil, and a graphene-nano silicon (Gr-NSi) composite layer is vapor-deposited on the outside of the aluminum foil layer. Finally, a layer of polyethylene terephthalate (PET) is dry-laminated as an anti-fouling layer.

[0075] The vapor deposition process equipment is simple and the cost is relatively low. The coating process has low requirements for the substrate and reduces the use of adhesive layer glue and black masterbatch, making it more environmentally friendly. The use of trace metal elements, graphene and nano-silicon has an anti-static effect on the surface of the film, which allows the static charge on the surface of the film to be quickly conducted to avoid static charge accumulation, thereby improving the safety performance and service life of the product. At the same time, it also improves the mechanical properties of the aluminum-plastic film. The deep forming performance, corrosion resistance, sealing performance and anti-warping performance of the aluminum-plastic film are also significantly improved.

[0076] In view of the numerous embodiments of the scheme of the present invention, the raw materials and dosage involved can be selected according to actual needs within the limited range, and the experimental data of each embodiment is huge and numerous, which is not suitable for listing and explaining one by one here, but the content required to be verified and the final conclusion obtained in each embodiment are similar. Therefore, the verification content of each embodiment will not be explained one by one here.

[0077] The above description is only a detailed description of the preferred embodiments and principles of the present invention. For ordinary technicians in this field, according to the ideas provided by the present invention, there will be changes in the specific implementation methods, and these changes should also be regarded as the protection scope of the present invention.

Claims

1. An aluminum-plastic composite film, characterized in that: It includes a CPP heat-sealing layer, an aluminum alloy layer, a graphene-nano silicon composite layer, an adhesive layer and a PET antifouling layer stacked in sequence; wherein the aluminum alloy layer is evaporated on the CPP heat-sealing layer, and the graphene-nano silicon composite layer is physically vapor deposited on the aluminum alloy layer.

2. The aluminum-plastic composite film according to claim 1, characterized in that: The mass ratio of graphene to nano-silicon in the graphene-nano-silicon composite layer is 1:(2-8).

3. The aluminum-plastic composite film according to claim 1, characterized in that: The thickness of the CPP heat-sealing layer is 15-80 μm, the thickness of the aluminum alloy layer is 20-45 μm, the thickness of the graphene-nano silicon composite layer is 15-25 μm, the thickness of the adhesive layer is 2-5 μm, and the thickness of the PET antifouling layer is 6-12 μm.

4. The aluminum-plastic composite film according to claim 1, characterized in that: The glue of the bonding layer is a multifunctional polyurethane resin adhesive.

5. The aluminum-plastic composite film according to claim 1, characterized in that: The thickness of the aluminum-plastic composite film is 58-167μm.

6. The method for preparing the aluminum-plastic composite film according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) A CPP heat-sealing layer cast film is selected as a vapor deposition substrate, firstly plasma-cleaned, then sent into a vapor deposition chamber through a guide roller, evacuated to a vacuum degree of ≤100 MPa, heated to 1300-1800° C. by high-frequency current, and cooled and deposited an aluminum alloy layer on the surface of the heat-sealing layer cast film through a cooling roller; (2) blowing graphene and nano-silicon from bottom to top in the evaporation chamber through airflow to physically vapor deposit a graphene-nano-silicon composite layer on the surface of the aluminum alloy layer; (3) Dry-bonding the PET antifouling layer on the surface of the graphene-nano silicon composite layer and curing it.

7. The preparation method according to claim 6, characterized in that: In the step (1), the plasma cleaning process is as follows: the vacuum degree of the cleaning chamber is ≤100 MPa, and the cleaning time is 1-5 s.

8. The preparation method according to claim 6, characterized in that: In the step (1), the evaporation material in the evaporation chamber includes the following components in weight percentage: 0.01-0.2% titanium, 0.2-1% manganese, 0.05-0.2% chromium, 0.1-0.5% zinc, 1-3% magnesium, 2-6% copper, the rest is aluminum; The temperature of the cooling roller is -80 to -5°C.

9. The preparation method according to claim 6, characterized in that: In the step (3), the aging process is: placing at 50-70°C for 48-144 hours.

10. A lithium ion battery, characterized in that: The method is packaged using the aluminum-plastic composite film as described in any one of claims 1 to 5.