Copper-clad plate, printed circuit board, electronic equipment and manufacturing method of copper-clad plate
By using a multi-layer wetted substrate and fluororesin film structure in the copper-clad laminate, combined with the optimization of the adhesive film, the problems of poor dielectric properties and insufficient mechanical strength of the copper-clad laminate in the existing technology are solved, and high mechanical strength and good dielectric strength are achieved. Copper-clad laminate with electrical properties, suitable for high-performance electronic equipment.
Patent Information
- Application Number
- CN202310365340.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-01
AI Technical Summary
The existing copper-clad laminates have poor dielectric properties and insufficient mechanical strength, making it difficult to meet the needs of electronic equipment with high information processing and transmission capabilities.
Adopting a copper-clad laminate structure including at least two wetted substrates and fluororesin films, improving the mechanical strength and dielectric properties by adjusting the composition and layout of the wetted substrates and fluororesin films, and optimizing surface flatness and adhesion through the use of adhesive films Together.
The high mechanical strength, dimensional stability and good dielectric properties of the copper-clad laminate are achieved, and deformation and cost during processing are reduced.
Smart Images

Figure CN118741850A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of circuit board manufacturing, and in particular to a copper clad laminate, a printed circuit board, an electronic device, and a method for manufacturing the copper clad laminate. Background Art
[0002] With the development of global information technology, the information carrying, processing and transmission capabilities of electronic devices are becoming increasingly demanding. This requires the printed circuit board (PCB) that carries signal transmission to have better dielectric properties. As the main component of PCB, copper clad laminate also needs to have better dielectric properties.
[0003] In the related art, the copper clad laminate generally includes a fluororesin film, such as polytetrafluoroethylene (PTFE), but PTFE is a thermoplastic material with insufficient mechanical strength and a large expansion and contraction problem during processing. Summary of the invention
[0004] In order to solve the above technical problems, the present application provides a copper clad laminate, a printed circuit board, an electronic device and a method for manufacturing a copper clad laminate, which can improve the mechanical strength of the copper clad laminate while maintaining good dielectric properties.
[0005] The present application provides a copper clad laminate, comprising a first copper foil, a second copper foil and a body. The body comprises: at least two impregnated substrates and a fluororesin film. The number of the impregnated substrates may be two, three, four or more. At least two impregnated substrates are stacked between the first copper foil and the second copper foil, each impregnated substrate comprises a substrate and a first fluororesin emulsion film, a portion of the first fluororesin emulsion film is located inside the substrate, and a portion of the first fluororesin emulsion film is disposed on the surface of the substrate facing the first copper foil and the surface facing the second copper foil. The fluororesin film is stacked between the first copper foil and the second copper foil. That is, at least two impregnated substrates and the fluororesin film are disposed between the first copper foil and the second copper foil.
[0006] In the present application, the impregnated substrate includes a substrate and a first fluororesin emulsion film immersed in the interior of the substrate and attached to the upper and lower surfaces of the substrate, and the substrate has good dimensional stability and good processability. Therefore, the impregnated substrate has good dimensional stability and good processability. The body includes at least two impregnated substrates, thereby improving the mechanical strength of the body. When the copper-clad laminate is processed, the copper-clad laminate is not prone to large deformation. Therefore, the overall processability of the copper-clad laminate is good, that is, the expansion and contraction during the processing is small. In addition, the fluororesin film has the characteristic of adjustable dielectric properties. Therefore, the dielectric properties of the fluororesin film can be adjusted by adjusting the proportion of each component in the fluororesin film, thereby achieving better dielectric properties. In other words, the copper-clad laminate has high mechanical strength, good dimensional stability, good processability and can achieve better dielectric properties.
[0007] In a possible implementation, a wetting substrate is disposed between the fluororesin film and the first copper foil, and between the fluororesin film and the second copper foil, respectively. When the number of the wetting substrates is two, one of the wetting substrates is disposed between the fluororesin film and the first copper foil, and the other of the wetting substrates is disposed between the fluororesin film and the second copper foil, that is, the fluororesin film is located between the two wetting substrates. In this way, in the copper clad laminate, the fluororesin film is located in the middle of the copper clad laminate, a wetting substrate and a first copper foil are disposed on its upper surface, and a wetting substrate and a second copper foil are disposed on its lower surface. In other words, the copper clad laminate is symmetrically structured about the center of the fluororesin film, so that when the copper clad laminate is subjected to external force, the symmetrical structure can be arranged to avoid uneven force on the upper and lower parts of the copper clad laminate.
[0008] In another possible implementation, at least two wetted substrates are in contact with each other and are located between the fluororesin film and the first copper foil, or at least two wetted substrates are in contact with each other and are located between the fluororesin film and the second copper foil.
[0009] In a possible embodiment, the body further includes at least two first adhesive films, one of which is located between the wet substrate and the first copper foil, and one of which is located between the wet substrate and the second copper foil. That is, when the number of wet substrates is two, one first adhesive film is arranged between one of the wet substrates and the first copper foil; and one first adhesive film is arranged between the other wet substrate and the second copper foil. Since the first fluororesin emulsion film arranged on the surface of the substrate is usually thin, part of the substrate will be exposed on the surface of the first fluororesin emulsion film facing the first copper foil, that is, the surface flatness of the wet substrate facing the first copper foil is poor. When the first adhesive film is arranged between the wet substrate and the first copper foil, in the process of making the fluororesin film, the second copper foil, the first adhesive film, the wet substrate, the fluororesin film, the wet substrate, the first adhesive film and the first copper foil can be stacked in sequence and then pressed under high pressure and high temperature. In this process, the first adhesive film flows at high temperature, thereby covering the substrate exposed to the first fluororesin emulsion film. The first adhesive film is in contact with the first copper foil on the side away from the wetted substrate, thereby improving the surface flatness of the surface in contact with the first copper foil. When a circuit structure is formed on the first copper foil, the dimensional deformation of the circuit structure can be reduced. Moreover, when the surface flatness in contact with the first copper foil is good, the bonding force between the wetted substrate and the first copper foil can also be increased. Similarly, the first adhesive film located between the wetted substrate and the second copper foil can also reduce the dimensional deformation of the circuit structure formed on the second copper foil, and can also increase the bonding force between the wetted substrate and the second copper foil.
[0010] Moreover, the thickness of the first adhesive film is less than 10 μm. If the thickness of the first adhesive film is greater than 10 μm, the thickness of the first adhesive film is too thick. On the one hand, it is easy to produce large deformation under high-temperature pressing, thereby affecting the circuit structure set on the first copper foil. On the other hand, when the first adhesive film is too thick, the mass proportion of the wetted substrate will be reduced, thereby affecting the dimensional stability of the copper clad laminate. Therefore, when the thickness of the first adhesive film is less than 10 μm, the impact on the circuit structure set on the first copper foil can be reduced, and the impact on the dimensional stability of the copper clad laminate can also be reduced.
[0011] Furthermore, the thickness of the wetted substrate is less than the thickness of the fluororesin film. Since the dielectric loss of the wetted substrate is higher than the dielectric loss of the fluororesin film, when the thickness of the wetted substrate is less than the thickness of the fluororesin film, the mass proportion of the wetted substrate with higher dielectric loss in the copper clad laminate can be smaller, while the mass proportion of the fluororesin film with lower dielectric loss in the copper clad laminate can be larger, thereby achieving lower dielectric loss of the copper clad laminate.
[0012] The fluororesin film includes fluororesin and filler; the mass proportion of fluororesin is 20%-50%, and the mass proportion of filler is 50%-80%. If the mass proportion of fluororesin is less than 20%, and the mass proportion of filler is greater than 80%, the mass proportion of fluororesin is too small and the mass proportion of filler is too large, which will cause larger pores to be generated inside the fluororesin film. If the mass proportion of fluororesin is greater than 50%, and the mass proportion of filler is less than 50%, the mass proportion of fluororesin is too large and the mass proportion of filler is too small, which will cause the dimensional stability of the fluororesin film to be poor. Therefore, when the mass proportion of fluororesin is 20%-50% and the mass proportion of filler is 50%-80%, the mass proportion of fluororesin and the mass proportion of filler are both moderate, which can reduce the situation of larger pores in the fluororesin film, and at the same time improve the dimensional stability of the fluororesin film.
[0013] In some possible embodiments of the present application, the body further includes a second fluororesin emulsion film, a portion of the second fluororesin emulsion film is located inside the fluororesin film, a portion of the second fluororesin emulsion film is disposed on the surface of the fluororesin film facing the first copper foil and in contact with one of the wetted substrates; a portion of the second fluororesin emulsion film is disposed on the surface facing the second copper foil and in contact with the other wetted substrate. Since fillers can usually be added to the fluororesin film, when there are more fillers, part of the fillers will be exposed, that is, part of the fillers will be exposed on the surface of the fluororesin film. When part of the second fluororesin emulsion film is disposed on the surface of the fluororesin film, during the process of making the copper clad laminate, during high-temperature pressing, the second fluororesin emulsion film can flow at high temperature, thereby covering the fluororesin film exposed to the second fluororesin emulsion film, thereby increasing the surface flatness of the fluororesin film with the second fluororesin emulsion film attached to the surface, and further increasing the adhesion between the fluororesin film and the wetted substrate.
[0014] In some possible embodiments of the present application, the first fluororesin emulsion film may include a fluororesin emulsion, a first additive and a filler, and the second fluororesin emulsion film may include a fluororesin emulsion and a second additive, and the mass proportion of the second additive is lower than the mass proportion of the first additive. Since part of the first fluororesin emulsion film needs to be immersed in the interior of the substrate and attached to the surface of the substrate, and the material of the substrate is different from the material of the first fluororesin emulsion film, more first additives are required to enable the first fluororesin emulsion film to be better immersed in the interior of the substrate. The second fluororesin emulsion film needs to be immersed in the interior of the fluororesin film and attached to the surface of the fluororesin film, and the material of the fluororesin emulsion film and the material of the fluororesin film both include fluororesin, so less second additives are required to enable the second fluororesin emulsion film to be immersed in the interior of the fluororesin film. When the mass proportion of the second additive in the second fluororesin emulsion film is lower than the mass proportion of the first additive in the first fluororesin emulsion film, it is possible to reduce the amount of the second additive while satisfying the requirement that the second fluororesin emulsion film is immersed in the interior of the fluororesin film, thereby reducing costs.
[0015] In addition, the substrate may include glass fiber cloth or quartz fiber cloth. Glass fiber cloth and quartz fiber cloth have good toughness and are not easily deformed, so the processability of the two is good. When the substrate includes glass fiber cloth or quartz fiber cloth, the processability of the substrate is also good.
[0016] The present application also provides a printed circuit board, comprising a first core board, the first core board comprising a circuit structure and any one of the above copper-clad boards, the circuit structure being arranged on the copper-clad board. The printed circuit board can achieve all the effects of the copper-clad board.
[0017] When the printed circuit board is a multilayer board structure, the printed circuit board also includes a second core board and an adhesive layer, and the adhesive layer is stacked between the first core board and the second core board. The number of the second core boards can be one or more, and the number of the adhesive layers can also be one or more. Two adjacent second core boards are connected by the adhesive layer, and the second core board and the first core board are also connected by the adhesive layer. Since the mechanical strength of the first core board is relatively high, when the printed circuit board is processed, the first core board is not easy to produce a large deformation, so the copper clad plate has better processability as a whole.
[0018] The adhesive layer includes a main body and a second adhesive film stacked on two opposite surfaces of the main body. Since the main body includes at least two wetted substrates and a fluororesin film, the main body has high mechanical strength, good dimensional stability, good processability and can achieve good dielectric properties. When the adhesive layer includes the main body, the adhesive layer has high mechanical strength, good dimensional stability, good processability and can achieve good dielectric properties. Moreover, when the adhesive layer also includes a second adhesive film, the bonding force between the adhesive layer and the first core plate can be improved, and the bonding force between the adhesive layer and the second core plate can be improved.
[0019] In a possible implementation, the structure of the second core board is the same as that of the first core board. Thus, when manufacturing the copper clad laminate, the first core board and the second core board can be manufactured using the same process, thereby simplifying the manufacturing process of the copper clad laminate.
[0020] In another possible implementation manner, the structure of the second core plate is different from that of the first core plate.
[0021] The present application also provides an electronic device, comprising a housing and the above-mentioned printed circuit board, wherein the printed circuit board is arranged in the housing. The electronic device can achieve all the effects of the printed circuit board.
[0022] The present application also provides a method for manufacturing a copper-clad laminate, the method comprising: manufacturing at least two impregnated substrates, each impregnated substrate comprising a substrate and a first fluororesin emulsion film, a portion of the first fluororesin emulsion film being immersed in the interior of the substrate, and a portion of the first fluororesin emulsion film being attached to two opposite surfaces of the substrate. Manufacturing a fluororesin film. Providing a first copper foil and a second copper foil. Pressing at least two impregnated substrates, the fluororesin film, the first copper foil and the second copper foil to form a copper-clad laminate, wherein at least two impregnated substrates are stacked between the first copper foil and the second copper foil, and the fluororesin film is stacked between the first copper foil and the second copper foil.
[0023] In the present application, the impregnated substrate includes a substrate and a first fluororesin emulsion film immersed in the interior of the substrate and attached to the upper and lower surfaces of the substrate, and the substrate has good dimensional stability and good processability, therefore, the impregnated substrate has good dimensional stability and good processability. The copper-clad laminate includes at least two impregnated substrates, thereby improving the mechanical strength of the copper-clad laminate, and when the copper-clad laminate is processed, the copper-clad laminate is not prone to large deformation, therefore, the overall processability of the copper-clad laminate is good. In addition, the fluororesin film has the characteristic of adjustable dielectric properties, therefore, the dielectric properties of the fluororesin film can be adjusted by adjusting the proportion of each component in the fluororesin film, thereby achieving better dielectric properties. In other words, the copper-clad laminate has high mechanical strength, good dimensional stability, good processability and can achieve better dielectric properties.
[0024] The present application also provides a method for manufacturing a printed circuit board, wherein a first circuit structure is formed on a copper-clad laminate to obtain a first core board, the copper-clad laminate is manufactured according to the above copper-clad laminate manufacturing method; a second circuit structure is formed on the copper-clad laminate to obtain a second core board; an adhesive layer is manufactured; and the first core board, the adhesive layer, and the second core board are pressed together to form a printed circuit board. Since the first core board has a high mechanical strength, the first core board is not prone to significant deformation when the copper-clad laminate is processed, and therefore, the printed circuit board has good overall processability.
[0025] In some possible embodiments, the step of making an adhesive layer includes: making at least two wetted substrates and fluororesin films respectively; pressing at least two wetted substrates and fluororesin films to form a pressed part; providing at least two second adhesive films; and arranging two of the second adhesive films on two opposite surfaces of the pressed part to form an adhesive layer. Since the main body includes at least two wetted substrates and fluororesin films, the main body has high mechanical strength, good dimensional stability, good processability, and can achieve good dielectric properties. When the adhesive layer includes at least two wetted substrates, fluororesin films, and at least two second adhesive films, the adhesive layer has high mechanical strength, good dimensional stability, good processability, and can achieve good dielectric properties. Moreover, when the adhesive layer also includes a second adhesive film, the bonding force between the adhesive layer and the first core board can be improved, as well as the bonding force between the adhesive layer and the second core board can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the description of the embodiments of the present application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0027] Figure 1 It is a schematic diagram of the structure of the copper clad plate in the first related technology;
[0028] Figure 2 It is a schematic diagram of the structure of the copper clad plate in the second related art;
[0029] Figure 3 This is a schematic diagram of the structure of the copper clad laminate in the first embodiment of the present application;
[0030] Figure 4 This is a schematic diagram of the structure of the copper clad laminate in the second embodiment of the present application;
[0031] Figure 5 This is a schematic diagram of the structure of the copper clad laminate in the third embodiment of the present application;
[0032] Figure 6This is a schematic diagram of the structure of a copper clad laminate in the fourth embodiment of the present application;
[0033] Figure 7a This is a schematic diagram of the structure of a copper clad laminate in the fifth embodiment of the present application;
[0034] Figure 7b This is a schematic diagram of the structure of a copper clad laminate in the sixth embodiment of the present application;
[0035] Figure 8 This is a schematic diagram of the structure of a printed circuit board in the seventh embodiment of the present application;
[0036] Fig. 9 This is a schematic diagram of the structure of a printed circuit board in an eighth embodiment of the present application;
[0037] Fig.10 for Fig. 9 A schematic diagram of the structure of the bonding layer in the printed circuit board shown;
[0038] Fig.11 This is a schematic diagram of the structure of a printed circuit board in a ninth embodiment of the present application;
[0039] Fig.12 This is a schematic diagram of the structure of a printed circuit board in a tenth embodiment of the present application;
[0040] Fig.13 This is a schematic diagram of the structure of a printed circuit board in the eleventh embodiment of the present application;
[0041] Fig.14 This is a schematic structural diagram of a printed circuit board in the twelfth embodiment of the present application;
[0042] Fig.15 for Figure 3 The production flow chart of the copper clad laminate shown;
[0043] Fig.16 for Figure 4 The production flow chart of the copper clad laminate shown;
[0044] Fig.17 for Figure 5 The production flow chart of the copper clad laminate shown;
[0045] Fig.18 for Fig. 9 The printed circuit board production flow chart is shown.
[0046] Icon: 1-printed circuit board; 100-copper clad laminate; 11-core layer; 12-copper foil; 13-fluororesin emulsion film; 10-first core board; 11-first copper foil; 12-second copper foil; 13-body; 131-impregnated substrate; 1311-substrate; 1312-first fluororesin emulsion film; 132-fluororesin film; 133-second fluororesin emulsion film; 134-first adhesive film; 20-second core board; 30-adhesive layer; 31-second adhesive film; 32-thermosetting resin impregnated substrate. DETAILED DESCRIPTION
[0047] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0048] The term "and / or" herein is merely a description of the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B may represent: A exists alone, A and B exist at the same time, and B exists alone, wherein A and B may be singular or plural. The character " / " generally indicates that the associated objects before and after are in an "or" relationship. "At least one (item)" refers to one or more, and "plurality" refers to two or more. "At least one of the following (items)" or similar expressions refers to any combination of these items, including any combination of single (items) or plural (items). For example, at least one (item) of a, b or c may represent: a, b, c, "a and b", "a and c", "b and c", or "a and b and c", wherein a, b, c may be single or multiple.
[0049] The terms "first" and "second" in the description and claims of the embodiments of the present application are used to distinguish different objects rather than to describe a specific order of objects. For example, a first target object and a second target object are used to distinguish different target objects rather than to describe a specific order of target objects.
[0050] "Connected", "connected" and similar words are used to express the intercommunication or interaction between different components, which may include direct connection or indirect connection through other components. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, inclusion of a series of steps or units. Methods, systems, products or devices are not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices. "Up", "down", "left", "right" and the like are only used relative to the orientation of the components in the drawings. These directional terms are relative concepts. They are used for description and clarification relative to the description, which may change accordingly according to the change of the orientation of the components in the drawings.
[0051] In the embodiments of the present application, words such as "exemplary" or "for example" are used to indicate examples, illustrations or descriptions. Any embodiment or design described as "exemplary" or "for example" in the embodiments of the present application should not be interpreted as being more preferred or more advantageous than other embodiments or designs. Specifically, the use of words such as "exemplary" or "for example" is intended to present related concepts in a specific way.
[0052] In the description of the embodiments of the present application, unless otherwise specified, the meaning of "multiple" refers to two or more than two. For example, multiple processing units refer to two or more processing units; multiple systems refer to two or more systems.
[0053] With the development of global information technology, the information carrying, processing and transmission capabilities of electronic devices are increasingly required. At the same time, electronic devices are gradually becoming lighter and thinner, and circuit wiring is gradually becoming more dense, which requires that the printed circuit board that carries the signal transmission has good dielectric properties to ensure the integrity of the signal transmission, achieve high-speed transmission, and reduce the heat dissipation of the process. Here, the electronic device can be a mobile phone, a tablet computer, a laptop computer, an ultra-mobile personal computer (UMPC), a handheld computer, a touch TV, a walkie-talkie, a netbook, a POS machine, a personal digital assistant (PDA), a wearable device, etc.
[0054] Dielectric properties can be expressed by dielectric constant Dk and dielectric loss Df. Dielectric constant Dk refers to the ability of a substance to hold charge, and is a physical quantity that measures the degree of polarization of a dielectric. The larger the dielectric constant Dk, the stronger the ability of the surface to bind charges, the less likely the charges are to be polarized, the weaker the polarization electric field, and the better the insulation properties of the material. Dielectric loss Df refers to the energy consumed per unit time by a dielectric under the action of an electric field, and can usually be expressed by the dielectric loss tangent.
[0055] Better dielectric properties may refer to a higher dielectric constant Dk and a lower dielectric loss Df, specifically, a dielectric constant Dk ≥ 3.0 and a dielectric loss Df ≤ 0.0008.
[0056] Figure 1 The copper clad laminate 100 shown can be a basic plate material of a printed circuit board. A circuit structure is arranged on the copper clad laminate 100 to form a printed circuit board. When the printed circuit board is required to have good dielectric properties, it means that the copper clad laminate 100 is also required to have good dielectric properties.
[0057] In a related technique, Figure 1 As shown, the copper clad laminate 100 includes a copper foil 12, a fluororesin film 132, a core layer 11, a fluororesin film 132 and a copper foil 12 which are stacked in sequence. When manufacturing the copper clad laminate 100, the copper foil 12, the fluororesin film 132 and the core layer 11 can be manufactured respectively, and the above components are stacked and placed, and pressed under high temperature and high pressure to form the copper clad laminate 100.
[0058] In one example, the core layer 11 may be a substrate. Since the fluororesin film 132 cannot flow at high temperatures, it cannot fill the pores inside the substrate, so the overall reliability of the copper clad laminate 100 is poor. Moreover, at 10 GHz, its dielectric constant Dk>3.0, and dielectric loss Df≥0.008, that is, the dielectric loss Df of the copper clad laminate 100 is high, and the dielectric performance of the copper clad laminate 100 is poor.
[0059] In another example, the core layer 11 may be a polyimide film. Since there is no substrate in the copper clad laminate 100, its mechanical strength is poor. In addition, at 10 GHz, its dielectric constant Dk ranges from ≥2.6, and its dielectric loss Df is ≥0.001, that is, the dielectric constant Dk of the copper clad laminate 100 is too low, the dielectric loss Df is too high, and the dielectric performance of the copper clad laminate 100 is poor.
[0060] In another related technique, Figure 2 As shown, the copper clad laminate 100 includes a copper foil 12, a fluororesin emulsion film 13, a core layer 11, a fluororesin emulsion film 13 and a copper foil 12 which are stacked in sequence.
[0061] The core layer 11 may be a polytetrafluoroethylene stretched film or a fluororesin film. In the related art, since there is no substrate in the copper clad laminate 100, its mechanical strength is poor. In addition, at 10 GHz, the dielectric constant Dk ranges from 2.0 to 2.6, and the dielectric loss Df is ≤ 0.0008. That is, the dielectric constant Dk of the copper clad laminate 100 is low, the dielectric loss Df is high, and the dielectric performance of the copper clad laminate 100 is poor.
[0062] Based on this, the present application embodiment provides a copper clad laminate 100. Figure 3As shown, the copper clad laminate 100 may include a first copper foil 11 , a second copper foil 12 and a body 13 .
[0063] The structure and size of the first copper foil 11 and the second copper foil 12 can be the same. That is, the length, width and thickness of the first copper foil 11 are the same as those of the second copper foil 12. The first copper foil 11 and the second copper foil 12 are stacked and spaced apart, that is, the first copper foil 11 and the second copper foil 12 are stacked and spaced apart, and there is a spacing between the first copper foil 11 and the second copper foil 12. The surface of the first copper foil 11 facing away from the second copper foil 12 can be used as the upper surface of the copper clad laminate 100, and the surface of the second copper foil 12 facing away from the first copper foil 11 can be used as the lower surface of the copper clad laminate 100. It can be understood that the first copper foil 11 and the second copper foil 12 can be used as conductive layers of a printed circuit board, and circuit structures can be set on the first copper foil 11 and the second copper foil 12, respectively.
[0064] like Figure 3 As shown, the body 13 may include: at least two wetted substrates 131 and a fluororesin film 132. The number of the wetted substrates 131 may be two, three, four or more. The body 13 is described below by taking the number of the wetted substrates 131 as two as an example.
[0065] like Figure 3 As shown, two wetted substrates 131 are stacked between the first copper foil 11 and the second copper foil 12. It can be said that the two wetted substrates 131 are stacked, and both of the two wetted substrates 131 are arranged between the first copper foil 11 and the second copper foil 12.
[0066] like Figure 3 As shown, each impregnated substrate 131 may include a substrate 1311 and a first fluororesin emulsion film 1312. The material of the substrate 1311 may include glass fiber cloth or quartz fiber cloth. Glass fiber cloth is mainly composed of glass fiber and short-line needle-punched non-woven fabric, and is an inorganic non-metallic material. Both glass fiber cloth and quartz fiber cloth have good toughness and are not easy to deform, so the processability of the two is good. When the substrate 1311 includes glass fiber cloth or quartz fiber cloth, the processability of the substrate 1311 is also good. It can be understood that the glass fiber cloth and the quartz fiber cloth have multiple pores inside.
[0067] The first fluororesin emulsion film 1312 may include fluororesin emulsion, filler and first additive. The filler may include ceramic filler. The first additive may include small molecule additive and coupling agent.
[0068] It is understood that fluororesin can refer to a class of thermoplastic resins containing fluorine atoms in the molecular structure. The main varieties of fluororesin include polytetrafluoroethylene, polychlorotrifluoroethylene, polyvinylidene fluoride, ethylene-tetrafluoroethylene copolymer, ethylene-chlorotrifluoroethylene copolymer, polyvinyl fluoride, etc. Fluororesin emulsion can refer to an emulsion liquid including fluororesin.
[0069] Part of the first fluororesin emulsion film 1312 is located inside the substrate 1311, and part of the first fluororesin emulsion film 1312 is arranged on the surface of the substrate 1311 facing the first copper foil 11 and the surface facing the second copper foil 12, and part of the first fluororesin emulsion film 1312 is also arranged on the side of the substrate 1311. When making the soaked substrate 131, the fluororesin emulsion, filler and additive can be prepared according to a preset mass ratio, and added to a high-speed mixer and stirred evenly to obtain a standby slurry. The standby slurry and the substrate 1311 are placed in the dipping tank of the glue machine, and part of the slurry will be immersed in the pores inside the substrate 1311, and part of the standby slurry is attached to and wrapped on the outer surface of the substrate 1311 to form the first fluororesin emulsion film 1312.
[0070] like Figure 3 As shown, the fluororesin film 132 is stacked between the first copper foil 11 and the second copper foil 12. That is, at least two wetting substrates 131 and the fluororesin film 132 are both arranged between the first copper foil 11 and the second copper foil 12. Moreover, the wetting substrates 131 are respectively arranged between the fluororesin film 132 and the first copper foil 11, and between the fluororesin film 132 and the second copper foil 12. That is, one of the wetting substrates 131 is arranged between the fluororesin film 132 and the first copper foil 11, and the other wetting substrate 131 is arranged between the fluororesin film 132 and the second copper foil 12, that is, the fluororesin film 132 is located between the two wetting substrates 131. In this way, in the copper clad laminate 100, the fluororesin film 132 is located in the middle of the copper clad laminate 100, and a wetting substrate 131 and the first copper foil 11 are arranged on its upper surface, and a wetting substrate 131 and the second copper foil 12 are arranged on its lower surface. That is to say, the copper clad laminate 100 has a symmetrical structure about the center of the fluororesin film 132 . Thus, when the copper clad laminate 100 is subjected to external force, the symmetrical structure can avoid uneven force on the upper and lower parts of the copper clad laminate 100 .
[0071] The fluororesin film 132 may include fluororesin and filler. The mass proportion of the fluororesin may be 20%-50%, that is, the ratio between the mass of the fluororesin and the mass of the fluororesin film 132 is greater than or equal to 20% and less than or equal to 50%. For example, the mass proportion of the fluororesin may be 20%, 30%, 40% or 50%, etc.
[0072] The mass proportion of the filler may be 50%-80%, that is, the ratio between the mass of the filler and the mass of the fluororesin film 132 is greater than or equal to 50% and less than or equal to 80%. For example, the mass proportion of the filler may be 50%, 60%, 70% or 80%.
[0073] If the mass proportion of the fluororesin is less than 20% and the mass proportion of the filler is greater than 80%, the mass proportion of the fluororesin is too small and the mass proportion of the filler is too large, which will result in large pores inside the fluororesin film 132. If the mass proportion of the fluororesin is greater than 50% and the mass proportion of the filler is less than 50%, the mass proportion of the fluororesin is too large and the mass proportion of the filler is too small, which results in poor dimensional stability of the fluororesin film 132. Therefore, when the mass proportion of the fluororesin is 20%-50% and the mass proportion of the filler is 50%-80%, the mass proportion of the fluororesin and the mass proportion of the filler are both moderate, which can reduce the situation of large pores in the fluororesin film 132 and improve the dimensional stability of the fluororesin film 132.
[0074] The fluororesin film 132 may be a dry fluororesin film, which is made by mixing dry powder fluororesin and filler uniformly, and has good dimensional stability.
[0075] The dielectric properties of the copper clad laminate 100 of the embodiment of the present application are tested and calculated, and the dielectric properties tables of Table 1 and Table 2 can be obtained. Table 1 is a dielectric property table of the copper clad laminate 100 when the material of the substrate 1311 includes glass fiber cloth. Table 2 is a dielectric property table of the copper clad laminate 100 when the material of the substrate 1311 includes quartz fiber cloth.
[0076] Table 1
[0077]
[0078] In Table 1, the material of the substrate 1311 in the wet substrate 131 includes glass fiber cloth. The dielectric constant Df and dielectric loss Dk of the wet substrate 131 are test values, the dielectric constant Df and dielectric loss Dk of the fluororesin film 132 are also test values, and the dielectric constant Df and dielectric loss Dk of the copper clad laminate 100 are calculated values. Mil can be referred to as milliinches, 1mil=25.4um. It can be understood that the length dimension of the wet substrate 131 is the same as the length dimension of the fluororesin film 132, and the width dimension of the wet substrate 131 is the same as the width dimension of the fluororesin film 132. Therefore, the volume ratio of the wet substrate 131 to the fluororesin film 132 and the thickness ratio of the wet substrate 131 to the fluororesin film 132 can be the same.
[0079] Table 2
[0080]
[0081]
[0082] In Table 2, the material of the substrate 1311 in the wet substrate 131 includes quartz fiber cloth. The dielectric constant Df and dielectric loss Dk of the wet substrate 131 are test values, the dielectric constant Df and dielectric loss Dk of the fluororesin film 132 are also test values, and the dielectric constant Df and dielectric loss Dk of the copper clad laminate 100 are calculated values.
[0083] In the embodiments of the present application, Figure 3 As shown, the impregnated substrate 131 includes a substrate 1311 and a first fluororesin emulsion film 1312 immersed in the substrate 1311 and attached to the upper and lower surfaces of the substrate 1311, and the substrate 1311 has good dimensional stability and good processability, so the impregnated substrate 131 has good dimensional stability and good processability. The copper clad laminate 100 includes at least two impregnated substrates 131, thereby improving the mechanical strength of the copper clad laminate 100. When the copper clad laminate 100 is processed, the copper clad laminate 100 is not prone to large deformation, so the copper clad laminate 100 has good overall processability.
[0084] In addition, the fluororesin film 132 has the characteristic of adjustable dielectric properties, that is, the dielectric properties of the fluororesin film 132 can be adjusted by adjusting the mass proportion of each component in the fluororesin film 132, thereby achieving better dielectric properties. For example, the fluororesin film 132 includes a fluororesin and a filler, and the dielectric properties of the fluororesin film 132 can be adjusted by adjusting the mass proportion of the fluororesin. The dielectric constant Df of the fluororesin film 132 in Table 1 and Table 2 is less than 0.0005, and the dielectric loss Dk is greater than 3.0, that is, the dielectric properties of the fluororesin film 132 are good. It can be understood that the dielectric loss Dk of the fluororesin film 132 in Table 1 and Table 2 is different because the mass proportion of the fluororesin in the fluororesin film 132 is different.
[0085] It can be seen from Table 1 that when the material of the substrate 1311 includes glass fiber cloth, the dielectric constant Df of the copper clad laminate 100 is 0.0005; it can be seen from Table 2 that when the material of the substrate 1311 includes quartz fiber cloth, the dielectric constant Df of the copper clad laminate 100 is 0.00042. Moreover, the dielectric loss Dk of the copper clad laminate 100 is 3.1. It can be seen that the dielectric constant Df of the copper clad laminate 100 is ≤ 0.0005, and the dielectric loss Dk of the copper clad laminate 100 is greater than 3.0, that is, the dielectric properties of the copper clad laminate 100 meet the dielectric property requirements.
[0086] like Figure 3As shown, the thickness of the wetted substrate 131 is less than the thickness of the fluororesin film 132. Exemplarily, the ratio between the thickness of the wetted substrate 131 and the thickness of the fluororesin film 132 can be 2:3. As shown in Tables 1 and 2, the dielectric loss of the wetted substrate 131 is higher than the dielectric loss of the fluororesin film 132. Therefore, when the thickness of the wetted substrate 131 is less than the thickness of the fluororesin film 132, the mass proportion of the wetted substrate 131 with higher dielectric loss in the copper clad laminate 100 can be smaller, while the mass proportion of the fluororesin film 132 with lower dielectric loss in the copper clad laminate 100 can be larger, thereby achieving lower dielectric loss of the copper clad laminate 100. In addition, by calculation, the thermal expansion coefficient DS of the copper clad laminate 100 is ≤500ppm.
[0087] In other embodiments of the present application, Figure 4 As shown, Figure 3 The difference between the embodiments shown is the structure of the body 13. The body 13 of this embodiment is Figure 3 On the basis of the embodiment shown, a second fluororesin emulsion film 133 is added. That is, in this embodiment, the body 13 includes at least two wetted substrates 131 and the fluororesin film 132 , and also includes the second fluororesin emulsion film 133 .
[0088] Part of the second fluororesin emulsion film 133 is located inside the fluororesin film 132, and part of the second fluororesin emulsion film 133 is arranged on the surface of the fluororesin film 132 facing the first copper foil 11 and in contact with one of the wetted substrates 131; part of the second fluororesin emulsion film 133 is arranged on the surface facing the second copper foil 12 and in contact with the other wetted substrate 131. Since the fluororesin film 132 may generally include fillers, when there are more fillers, part of the fillers will be exposed, that is, part of the fillers will be exposed on the surface of the fluororesin film 132. When part of the second fluororesin emulsion film 133 is arranged on the surface of the fluororesin film 132, during the process of manufacturing the copper clad laminate 100, during high temperature pressing, the second fluororesin emulsion film 133 can flow at high temperature, thereby covering the fluororesin film 132 exposed on the second fluororesin emulsion film 133, thereby increasing the surface flatness of the fluororesin film 132 with the second fluororesin emulsion film 133 attached to the surface, and further increasing the bonding force between the fluororesin film 132 and the wetted substrate 131.
[0089] Regarding the composition of the second fluororesin emulsion film 133, in a possible embodiment, the second fluororesin emulsion film 133 may only include fluororesin emulsion and a second additive, but no filler. The second additive may include a small molecule auxiliary agent and a coupling agent.
[0090] In another possible implementation, the second fluororesin emulsion film 133 may include fluororesin emulsion, a second additive and a filler. The filler may include a ceramic filler.
[0091] In this embodiment, the mass proportion of the second additive in the second fluororesin emulsion film 133 is lower than the mass proportion of the first additive in the first fluororesin emulsion film 1312. The mass proportion of the second additive may refer to the ratio between the mass of the second additive and the mass of the second fluororesin emulsion film 133. The mass proportion of the first additive may refer to the ratio between the mass of the first additive and the mass of the first fluororesin emulsion film 1312. Since part of the first fluororesin emulsion film 1312 needs to be immersed in the interior of the substrate 1311 and attached to the surface of the substrate 1311, and the material of the substrate 1311 is different from that of the first fluororesin emulsion film 1312, more first additives are needed to enable the first fluororesin emulsion film 1312 to be better immersed in the interior of the substrate 1311. The second fluororesin emulsion film 133 needs to be immersed in the interior of the fluororesin film 132 and attached to the surface of the fluororesin film 132. The material of the second fluororesin emulsion film 133 and the material of the fluororesin film 132 both include fluororesin, so less second additive is needed to enable the second fluororesin emulsion film 133 to be immersed in the interior of the fluororesin film 132. When the mass proportion of the second additive in the second fluororesin emulsion film 133 is lower than the mass proportion of the first additive in the first fluororesin emulsion film 1312, the second fluororesin emulsion film 133 can be immersed in the interior of the fluororesin film 132 while reducing the amount of the second additive, thereby reducing costs.
[0092] In other embodiments, the mass proportion of the second additive is the same as the mass proportion of the first additive, or the mass proportion of the second additive is higher than the mass proportion of the first additive.
[0093] The dielectric properties of the copper clad laminate 100 of this embodiment are tested and calculated, and the dielectric properties table of Table 3 can be obtained.
[0094] Table 3
[0095]
[0096] In Table 3, the material of the substrate 1311 in the wet substrate 131 includes glass fiber cloth. The dielectric constant Df and dielectric loss Dk of the wet substrate 131 are test values, the dielectric constant Df and dielectric loss Dk of the fluororesin film 132 are also test values, and the dielectric constant Df and dielectric loss Dk of the copper clad laminate 100 are calculated values.
[0097] It can be seen from Table 3 that the dielectric constant Df of the fluororesin film 132 is 0.0003, and the dielectric loss Dk is 3.6. It can be seen that the dielectric constant Df of the fluororesin film 132 is less than 0.0005, and the dielectric loss Dk is greater than 3.0, that is, the dielectric performance of the fluororesin film 132 is good.
[0098] It can be seen from Table 3 that when the material of the substrate 1311 includes glass fiber cloth, the dielectric constant Df of the copper clad laminate 100 is 0.0005, and the dielectric loss Dk of the copper clad laminate 100 is 3.1. It can be seen that the dielectric constant Df of the copper clad laminate 100 is ≤ 0.0005, and the dielectric loss Dk of the copper clad laminate 100 is greater than 3.0, that is, the dielectric properties of the copper clad laminate 100 meet the dielectric property requirements.
[0099] In other embodiments of the present application, Figure 5 As shown, Figure 3 The difference between the embodiments shown is the structure of the body 13. The body 13 of this embodiment is Figure 3 On the basis of the embodiment shown, at least two first adhesive films 134 are added. That is, in this embodiment, the body 13 includes at least two first adhesive films 134 in addition to the at least two wetted substrates 131 and the fluororesin film 132 .
[0100] When the number of the first adhesive films 134 is two, one of the first adhesive films 134 is located between the wetted substrate 131 and the first copper foil 11, and the other first adhesive film 134 is located between the wetted substrate 131 and the second copper foil 12. That is, when the number of the wetted substrates 131 is two, one of the first adhesive films 134 is disposed between the wetted substrate 131 and the first copper foil 11; and one of the first adhesive films 134 is disposed between the other wetted substrate 131 and the second copper foil 12. Since the first fluororesin emulsion film 1312 disposed on the surface of the substrate 1311 is usually thin, a portion of the substrate 1311 is exposed on the surface of the first fluororesin emulsion film 1312 facing the first copper foil 11, that is, the surface flatness of the wetted substrate 131 facing the first copper foil 11 is poor. When the first adhesive film 134 is set between the wet substrate 131 and the first copper foil 11, in the process of making the fluororesin film 132, the second copper foil 12, the first adhesive film 134, the wet substrate 131, the fluororesin film 132, the wet substrate 131, the first adhesive film 134 and the first copper foil 11 can be stacked in sequence and pressed under high pressure and high temperature. In this process, the first adhesive film 134 flows at high temperature, thereby covering the substrate 1311 exposed to the first fluororesin emulsion film 1312. The first adhesive film 134 is in contact with the first copper foil 11 on the side away from the wet substrate 131, thereby improving the surface flatness in contact with the first copper foil 11. When the circuit structure is formed on the first copper foil 11, the dimensional deformation of the circuit structure can be reduced. Moreover, when the surface flatness in contact with the first copper foil 11 is good, the bonding force between the wet substrate 131 and the first copper foil 11 can also be increased. Similarly, the first adhesive film 134 between the wetted substrate 131 and the second copper foil 12 can also reduce the dimensional deformation of the circuit structure formed on the second copper foil 12 and increase the bonding force between the wetted substrate 131 and the second copper foil 12 .
[0101] Moreover, the thickness of the first adhesive film 134 is less than 10 μm. If the thickness of the first adhesive film 134 is greater than 10 μm, the thickness of the first adhesive film 134 is too thick. On the one hand, under high-temperature pressing, it is easy to produce a large deformation, thereby affecting the circuit structure set on the first copper foil 11. On the other hand, when the first adhesive film 134 is too thick, the mass proportion of the wetted substrate 131 will be reduced, thereby affecting the dimensional stability of the copper clad laminate 100. Therefore, when the thickness of the first adhesive film 134 is less than 10 μm, the impact on the circuit structure set on the first copper foil 11 can be reduced, and the impact on the dimensional stability of the copper clad laminate 100 can also be reduced.
[0102] The material of the first adhesive film 134 may include fluororesin, and exemplarily, the material of the first adhesive film 134 may include PFA, PTFE or PEP. Moreover, the first adhesive film 134 may be a pure fluororesin film 132, that is, the first adhesive film 134 only includes fluororesin but no filler.
[0103] The dielectric properties of the copper clad laminate 100 of this embodiment are tested and calculated, and the dielectric properties table of Table 4 can be obtained.
[0104] Table 4
[0105]
[0106] In Table 4, the material of the substrate 1311 in the wet substrate 131 includes glass fiber cloth. The dielectric constant Df and dielectric loss Dk of the wet substrate 131 are test values, the dielectric constant Df and dielectric loss Dk of the fluororesin film 132 are also test values, and the dielectric constant Df and dielectric loss Dk of the copper clad laminate 100 are calculated values.
[0107] It can be seen from Table 4 that when the material of the substrate 1311 includes glass fiber cloth, the dielectric constant Df of the copper clad laminate 100 is 0.00049, and the dielectric loss Dk of the copper clad laminate 100 is 3.08. It can be seen that the dielectric constant Df of the copper clad laminate 100 is ≤ 0.0005, and the dielectric loss Dk of the copper clad laminate 100 is greater than 3.0, that is, the dielectric properties of the copper clad laminate 100 meet the dielectric property requirements.
[0108] In other embodiments of the present application, Figure 6 As shown, Figure 4 The difference between the embodiments shown is the structure of the body 13. The body 13 of this embodiment is Figure 4 On the basis of the embodiment shown, at least two first adhesive films 134 are added. That is, in this embodiment, the body 13 includes at least two first adhesive films 134 in addition to the at least two wetted substrates 131 , the fluororesin film 132 and the second fluororesin emulsion film 133 .
[0109] The material of the first adhesive film 134 may include fluororesin, and for example, the material of the first adhesive film 134 may include PFA or thermosetting hydrocarbon resin. Moreover, the first adhesive film 134 may be a pure fluororesin film 132, that is, the first adhesive film 134 only includes fluororesin but no filler.
[0110] The dielectric properties of the copper clad laminate 100 of this embodiment are tested and calculated, and the dielectric properties table of Table 5 can be obtained.
[0111] Table 5
[0112]
[0113] In Table 5, the material of the substrate 1311 in the wet substrate 131 includes glass fiber cloth. The dielectric constant Df and dielectric loss Dk of the wet substrate 131 are test values, the dielectric constant Df and dielectric loss Dk of the fluororesin film 132 are also test values, and the dielectric constant Df and dielectric loss Dk of the copper clad laminate 100 are calculated values.
[0114] It can be seen from Table 5 that when the material of the substrate 1311 includes glass fiber cloth, the dielectric constant Df of the copper clad laminate 100 is 0.00049, and the dielectric loss Dk of the copper clad laminate 100 is 3.08. It can be seen that the dielectric constant Df of the copper clad laminate 100 is ≤ 0.0005, and the dielectric loss Dk of the copper clad laminate 100 is greater than 3.0, that is, the dielectric properties of the copper clad laminate 100 meet the dielectric property requirements.
[0115] In other embodiments of the present application, Figure 7a and Figure 7b As shown, Figure 3 The difference between the embodiments shown is the structure of the body 13. Figure 7a As shown, at least two wetted substrates 131 are in contact with each other and are located between the fluororesin film 132 and the first copper foil 11. Figure 7b As shown, at least two wetted substrates 131 are in contact with each other and are located between the fluororesin film 132 and the second copper foil 12 .
[0116] like Figure 8 As shown, the embodiment of the present application further provides a printed circuit board 1, the printed circuit board 1 may include a first core board 10, the first core board 10 may include a copper clad board 100 and a circuit structure ( Figure 8 not shown).
[0117] In other embodiments of the present application, Fig. 9 As shown, Figure 8 The difference between the illustrated embodiments lies in the number of layers of the printed circuit board 1 . Figure 8The printed circuit board 1 shown is a single-layer board. In this embodiment, Fig. 9 As shown, the printed circuit board 1 can be a multi-layer board.
[0118] like Fig. 9 As shown, the printed circuit board 1 may include a first core board 10, a second core board 20, and an adhesive layer 30 located between the first core board 10 and the second core board 20. In this embodiment, the first core board 10 and the second core board 20 each have one layer, and the adhesive layer 30 also has one layer. In other embodiments, the first core board 10 may have two or three layers, the second core board 20 may also have two or three layers, and the adhesive layer 30 may also have multiple layers. In this way, a layer of adhesive layer 30 is provided between every two adjacent first core boards 10, a layer of adhesive layer 30 is provided between every two adjacent second core boards 20, and a layer of adhesive layer 30 is provided between the first core board 10 and the second core board 20.
[0119] Regarding the structure of the second core plate 20, in a possible implementation manner, as Fig. 9 As shown, the structure of the second core board 20 is the same as that of the first core board 10. Exemplarily, the second core board 20 also includes a first copper foil 11, a second copper foil 12 and a body 13, and the body 13 includes at least two wetted substrates 131 and a fluororesin film 132. In this way, when manufacturing the copper clad laminate 100, the first core board 10 and the second core board 20 can be manufactured by the same process, thereby simplifying the manufacturing process of the copper clad laminate 100.
[0120] In another possible implementation, the structure of the second core board 20 is different from that of the first core board 10. Exemplarily, the second core board 20 includes a first copper foil 11, a second copper foil 12 and a body 13, and the body 13 includes a wetted substrate 131 and two fluororesin films 132, etc.
[0121] like Fig.10 As shown, the adhesive layer 30 may include a body 13 and a second adhesive film 31 stacked on two opposite surfaces of the body 13. The material of the second adhesive film 31 may be a fluororesin, and illustratively, the material of the second adhesive film 31 may include soluble polytetrafluoroethylene (polyfluoroalkoxy, PFA) or a thermosetting hydrocarbon resin. Moreover, in one example, the second adhesive film 31 may include only a fluororesin film; in another example, the second adhesive film 31 may include a fluororesin film and a filler to obtain a lower thermal expansion coefficient.
[0122] Since the body 13 includes at least two wetted substrates 131 and a fluororesin film 132, the body 13 has high mechanical strength, good dimensional stability, good processability, and can achieve good dielectric properties. When the adhesive layer 30 includes the body 13, the adhesive layer 30 has high mechanical strength, good dimensional stability, good processability, and can achieve good dielectric properties. Moreover, when the adhesive layer 30 also includes a second adhesive film 31, the adhesive force between the adhesive layer 30 and the first core plate 10 can be improved, and the adhesive force between the adhesive layer 30 and the second core plate 20 can be improved.
[0123] In other embodiments of the present application, Fig.11 As shown, Fig. 9 The difference between the illustrated embodiments lies in the structure of the first core plate 10, the second core plate 20 and the body 13 in the adhesive layer 30. Fig.11 As shown, in this embodiment, the first core plate 10, the second core plate 20 and the body 13 in the adhesive layer 30 can be made of Figure 4 The structure of the body 13 in the embodiment shown is as follows. That is, in this embodiment, the body 13 includes at least two wetted substrates 131 , a fluororesin film 132 and a second fluororesin emulsion film 133 .
[0124] In other embodiments of the present application, Fig.12 As shown, Fig. 9 The difference between the illustrated embodiments lies in the structure of the first core plate 10, the second core plate 20 and the body 13 in the adhesive layer 30. Fig.12 As shown, in this embodiment, the first core plate 10, the second core plate 20 and the body 13 in the adhesive layer 30 can be made of Figure 5 The structure of the body 13 in the embodiment shown is as follows. That is, in this embodiment, the body 13 may include at least two wet substrates 131 , a fluororesin film 132 and at least two first adhesive films 134 .
[0125] In other embodiments of the present application, Fig.13 As shown, Fig. 9 The difference between the illustrated embodiments lies in the structure of the first core plate 10, the second core plate 20 and the body 13 in the adhesive layer 30. Fig.13 As shown, in this embodiment, the first core plate 10, the second core plate 20 and the body 13 in the adhesive layer 30 can be made of Figure 6 The structure of the body 13 in the embodiment shown is as follows. That is, in this embodiment, the body 13 includes at least two wetted substrates 131 , a fluororesin film 132 , a second fluororesin emulsion film 133 and at least two first adhesive films 134 .
[0126] It is understandable that in Fig. 9 , Figure 11-Figure 14In the embodiment shown, the structures of the body 13 in the first core board 10, the body 13 in the second core board 20, and the body 13 in the adhesive layer 30 are the same. In other embodiments, the structures of the body 13 in the first core board 10 and the body 13 in the second core board 20 are the same, and the structures of the body 13 in the first core board 10 and the body 13 in the adhesive layer 30 are different. Alternatively, the structures of the body 13 in the first core board 10, the body 13 in the second core board 20, and the body 13 in the adhesive layer 30 are different from each other. Exemplarily, when the structure of the copper clad laminate 100 in the first core board 10 is Figure 3 The structure of the copper clad laminate 100 shown in FIG. 1 may be as follows: Figure 4 , Figure 5 , Figure 6 , Figure 7a or Figure 7b The structure of the main body 13 in the adhesive layer 30 can also be Figure 4 , Figure 5 , Figure 6 , Figure 7a or Figure 7b The structure in .
[0127] In other embodiments of the present application, Fig.14 As shown, Fig. 9 The difference between the embodiments shown is the structure of the adhesive layer 30. In this embodiment, Fig.14 As shown, the adhesive layer 30 includes two layers of thermosetting resin impregnated substrates 32 stacked and in contact with each other and a second adhesive film 31 located on the upper and lower surfaces of the two layers of thermosetting resin impregnated substrates 32 .
[0128] In other embodiments, when the structure of the adhesive layer 30 is Fig.14 When the two layers of thermosetting resin impregnated substrate 32 and the second adhesive film 31 are shown, the structure of the first core plate 10 and the second core plate 20 can be adopted. Figure 4-7a ,or Figure 7b The structure of the illustrated embodiment.
[0129] The present application also provides a method for manufacturing a copper clad laminate 100. The method can be applied to Figure 3 The embodiment shown. Fig.15 As shown, the production method may include:
[0130] S41, manufacturing at least two wetted substrates 131.
[0131] Each of the wetted substrates 131 includes a substrate 1311 and a first fluororesin emulsion film 1312 .
[0132] When preparing at least two wetted substrates 131 , the fluororesin emulsion, the first additive and the filler may be prepared according to a preset mass ratio, and the fluororesin emulsion, the first additive and the filler may be put into a mixer and stirred evenly to obtain a slurry to be used.
[0133] Provide at least two substrates 1311. Put at least two substrates 1311 and the slurry to be used into the dipping tank of the glue machine respectively, partially immerse the slurry to be used into the interior of the substrate 1311, and partially adhere to the surface of the substrate 1311, and form the first fluororesin emulsion film 1312 on the interior of the substrate 1311 and the surface of the substrate 1311 respectively, and obtain the semi-cured wet substrate 131 after drying the first additive in an oven. In this process, the thickness of the first fluororesin emulsion film 1312 formed on the surface of the substrate 1311 can be controlled by a glue scraper.
[0134] S42, preparing the fluororesin film 132.
[0135] The fluororesin and the filler are uniformly mixed according to a preset mass ratio to obtain a fluororesin film 132 .
[0136] S43, providing a first copper foil 11 and a second copper foil 12.
[0137] A first copper foil 11 and a second copper foil 12 are provided, and a coupling agent is disposed on a surface of the first copper foil 11 , and a coupling agent is disposed on a surface of the second copper foil 12 .
[0138] S44 , laminating at least two wetted substrates 131 , the fluororesin film 132 , the first copper foil 11 , and the second copper foil 12 to form the copper clad laminate 100 .
[0139] The second copper foil 12, the wetted substrate 131, the fluororesin film 132, the wetted substrate 131 and the first copper foil 11 are stacked in sequence and pressed together by an air compressor under vacuum, high pressure and high temperature to obtain the copper clad laminate 100. The copper clad laminate 100 has high mechanical strength. When the copper clad laminate 100 is processed, the copper clad laminate 100 is not prone to large deformation. Therefore, the copper clad laminate 100 has good processability as a whole.
[0140] In the embodiment of the present application, the impregnated substrate 131 includes a substrate 1311 and a first fluororesin emulsion film 1312 immersed in the interior of the substrate 1311 and attached to the upper and lower surfaces of the substrate 1311, and the substrate 1311 has good dimensional stability and good processability, therefore, the impregnated substrate 131 has good dimensional stability and good processability. The copper clad laminate 100 includes at least two impregnated substrates 131, thereby improving the mechanical strength of the copper clad laminate 100, and when the copper clad laminate 100 is processed, the copper clad laminate 100 is not prone to large deformation, therefore, the overall processability of the copper clad laminate 100 is good. In addition, the fluororesin film 132 has the characteristic of adjustable dielectric properties, therefore, the dielectric properties of the fluororesin film 132 can be adjusted by adjusting the proportion of each component in the fluororesin film 132, thereby achieving good dielectric properties. In other words, the copper clad laminate 100 has high mechanical strength, good dimensional stability, good processability and can achieve good dielectric properties.
[0141] In other embodiments of the present application, a method for manufacturing a copper clad laminate 100 is also provided. The method can be applied to Figure 4 The copper clad board 100 shown. Fig.16 As shown, the production method may include:
[0142] S51 , manufacturing at least two wetted substrates 131 .
[0143] Reference Fig.15 Step S41 is shown.
[0144] S52, preparing the wet fluororesin film 132.
[0145] The fluororesin and the filler are uniformly mixed according to a preset mass ratio to obtain a fluororesin film 132 .
[0146] The second fluororesin emulsion film 133 can be prepared by preparing the fluororesin emulsion and the second additive according to a preset mass ratio, and the fluororesin emulsion and the second additive are put into a stirrer and stirred evenly to obtain a slurry to be used.
[0147] The fluororesin film 132 and the slurry to be used are respectively placed in the dipping tank of the glue applicator, and part of the slurry to be used is immersed in the interior of the fluororesin film 132, and part of the slurry to be used is attached to the surface of the fluororesin film 132, and a second fluororesin emulsion film 133 is formed on the interior of the fluororesin film 132 and on the surface of the fluororesin film 132, respectively, and the semi-cured impregnated fluororesin film 132 is obtained after the second additive is dried in an oven. In this process, the thickness of the second fluororesin emulsion film 133 formed on the surface of the substrate 1311 can be controlled by a glue scraper.
[0148] S53, providing a first copper foil 11 and a second copper foil 12.
[0149] Reference Fig.15 Step S43 is shown.
[0150] S54 , laminating at least two wetted substrates 131 , the wetted fluororesin film 132 , the first copper foil 11 , and the second copper foil 12 to form the copper clad laminate 100 .
[0151] The second copper foil 12 , the impregnated substrate 131 , the impregnated fluororesin film 132 , the impregnated substrate 131 and the first copper foil 11 are stacked in sequence and pressed together by an air compressor under vacuum, high pressure and high temperature to obtain a copper clad laminate 100 .
[0152] In other embodiments of the present application, a method for manufacturing a copper clad laminate 100 is also provided. The method can be applied to Figure 5 In the embodiment shown. Fig.17 As shown, the production method may include:
[0153] S61 , manufacturing at least two wetted substrates 131 .
[0154] Reference Fig.15 Step S41 is shown.
[0155] S62, preparing the fluororesin film 132.
[0156] Reference Fig.15 Step S42 is shown.
[0157] S63 , providing at least two first adhesive films 134 .
[0158] The at least two first adhesive films 134 may be made of dry powder fluororesin.
[0159] S64, providing a first copper foil 11 and a second copper foil 12.
[0160] Reference Fig.15 Step S43 is shown.
[0161] S65 , laminating at least two wetted substrates 131 , the fluororesin films 132 , at least two first adhesive films 134 , the first copper foil 11 , and the second copper foil 12 to form the copper clad laminate 100 .
[0162] The second copper foil 12 , the wetted substrate 131 , the fluororesin film 132 , at least two first adhesive films 134 , the wetted substrate 131 and the first copper foil 11 are stacked in sequence and pressed together by an air compressor under vacuum, high pressure and high temperature to obtain the copper clad laminate 100 .
[0163] like Fig.18 As shown, the present application embodiment also provides a method for manufacturing a printed circuit board 1, which can be applied to Fig. 9 In the embodiment shown, the manufacturing method may include:
[0164] S71 , forming a first circuit structure on the copper clad laminate 100 to obtain a first core substrate 10 .
[0165] Copper clad laminate can be based on Fig.15 , Fig.16 or Fig.17 The copper clad laminate 100 is manufactured by the manufacturing method shown in the figure. A first circuit structure can be formed on the first copper foil 11 and the second copper foil 12 of the copper clad laminate 100 by an etching process to obtain a first core board 10.
[0166] S72 , forming a second circuit structure on the copper clad laminate 100 to obtain a second core substrate 20 .
[0167] Copper clad laminate can be based on Fig.15 , Fig.16 or Fig.17 The copper clad laminate 100 is manufactured by the manufacturing method shown in the figure. A second circuit structure can be formed on the first copper foil 11 and the second copper foil 12 of the copper clad laminate 100 by an etching process to obtain a second core board 20.
[0168] S73, preparing the adhesive layer 30.
[0169] You can refer to Fig.15 The step S41 shown in the figure is to make at least two wetted substrates 131. Fig.15 In step S42 shown, the fluororesin film 132 is produced.
[0170] Provide a first isolation layer and a second isolation layer. Press at least two wetted substrates 131, fluororesin film 132, first isolation layer and second isolation layer, at least two wetted substrates 131 and fluororesin film 132 are located between the first isolation layer and the second isolation layer. Remove the first isolation layer and the second isolation layer to obtain a pressed part.
[0171] At least two second adhesive films 31 are provided. Two of the second adhesive films 31 are disposed on two opposite surfaces of the pressing member to form an adhesive layer 30 .
[0172] S74 , pressing the first core board 10 , the adhesive layer 30 and the second core board 20 together to form a printed circuit board 1 .
[0173] The first core board 10 , the adhesive layer 30 and the second core board 20 are stacked in sequence and pressed together by an air compressor under vacuum, high pressure and high temperature to obtain a printed circuit board 1 .
[0174] The embodiments of the present application are described above in conjunction with the accompanying drawings, but the present application is not limited to the above-mentioned specific implementation methods. The above-mentioned specific implementation methods are merely illustrative and not restrictive. Under the guidance of the present application, ordinary technicians in this field can also make many forms without departing from the purpose of the present application and the scope of protection of the claims, all of which are within the protection of the present application.
Claims
1. A copper clad laminate, It is characterized in that It includes a first copper foil, a second copper foil and a body; The body comprises: At least two wetted substrates, the at least two wetted substrates are stacked between the first copper foil and the second copper foil, each of the wetted substrates comprises a substrate and a first fluororesin emulsion film, a portion of the first fluororesin emulsion film is located inside the substrate, and a portion of the first fluororesin emulsion film is provided on a surface of the substrate facing the first copper foil and a surface of the substrate facing the second copper foil; A fluororesin film is laminated between the first copper foil and the second copper foil.
2. The copper clad laminate according to claim 1, It is characterized in that The wet substrate is provided between the fluororesin film and the first copper foil, and between the fluororesin film and the second copper foil, respectively.
3. The copper clad laminate according to claim 1 or 2, It is characterized in that The body further includes at least two first adhesive films, one of which is located between the wetted substrate and the first copper foil, and one of which is located between the wetted substrate and the second copper foil.
4. The copper clad laminate according to claim 3, It is characterized in that The thickness of the first adhesive film is less than 10 μm.
5. The copper clad laminate according to any one of claims 1 to 4, It is characterized in that The thickness of the wet substrate is smaller than the thickness of the fluororesin film.
6. The copper clad laminate according to any one of claims 1 to 5, It is characterized in that The fluororesin film comprises a fluororesin and a filler; The mass proportion of the fluororesin is 20%-50%, and the mass proportion of the filler is 50%-80%.
7. The copper clad laminate according to any one of claims 1 to 6, It is characterized in that The body also includes a second fluororesin emulsion film, a portion of which is located inside the fluororesin film, a portion of which is arranged on the surface of the fluororesin film facing the first copper foil and in contact with one of the wetting substrates; a portion of the second fluororesin emulsion film is arranged on the surface facing the second copper foil and in contact with the other of the wetting substrates.
8. The copper clad laminate according to claim 7, It is characterized in that The first fluororesin emulsion film includes a first additive, and the second fluororesin emulsion film includes a second additive, wherein a mass proportion of the second additive is lower than a mass proportion of the first additive.
9. The copper clad laminate according to any one of claims 1 to 8, It is characterized in that The substrate includes glass fiber cloth or quartz fiber cloth.
10. A printed circuit board, It is characterized in that It comprises a first core board, wherein the first core board comprises a circuit structure and the copper clad board according to any one of claims 1 to 9, wherein the circuit structure is arranged on the copper clad board.
11. The printed circuit board according to claim 10, It is characterized in that The printed circuit board further includes a second core board and an adhesive layer, wherein the adhesive layer is stacked between the first core board and the second core board.
12. The printed circuit board according to claim 11, It is characterized in that The adhesive layer includes the main body and a second adhesive film stacked on two opposite surfaces of the main body.
13. The printed circuit board according to claim 11 or 12, It is characterized in that The structure of the second core plate is the same as that of the first core plate.
14. An electronic device, It is characterized in that It comprises a housing and a printed circuit board as claimed in any one of claims 10 to 13, wherein the printed circuit board is arranged in the housing.
15. A method for manufacturing a copper clad laminate, It is characterized in that The production method comprises: Prepare at least two wetted substrates, each of the wetted substrates comprises a substrate and a first fluororesin emulsion film, a portion of the first fluororesin emulsion film is immersed in the interior of the substrate, and a portion of the first fluororesin emulsion film is attached to two opposite surfaces of the substrate; Making fluororesin films; providing a first copper foil and a second copper foil; The at least two wetted substrates, the fluororesin film, the first copper foil and the second copper foil are pressed together to form the copper clad laminate, wherein the at least two wetted substrates are stacked between the first copper foil and the second copper foil, and the fluororesin film is stacked between the first copper foil and the second copper foil.
16. A method for manufacturing a printed circuit board, It is characterized in that The production method comprises: forming a first circuit structure on a copper-clad laminate to obtain a first core board, wherein the copper-clad laminate is manufactured according to the manufacturing method of claim 15; forming a second circuit structure on a copper-clad laminate to obtain a second core board, wherein the copper-clad laminate is manufactured according to the manufacturing method of claim 15; Making an adhesive layer; The first core board, the adhesive layer and the second core board are pressed together to form the printed circuit board.
17. The method according to claim 16, It is characterized in that The step of making the bonding layer comprises: preparing at least two wetted substrates and fluororesin films respectively; Laminating the at least two wetted substrates and the fluororesin film to form a laminated part; providing at least two second adhesive films; Two of the second adhesive films are respectively disposed on two opposite surfaces of the pressing member to form the adhesive layer.